A kind of residual oil catalytic cracking catalyst and preparation method thereof
High-pore volume silicon-aluminum materials are prepared by cheap silicon-aluminum sources, combined with matrix and molecular sieve, and constructed catalysts, which solves the problems of insufficient pore structure of the catalyst and insufficient resistance to heavy metal pollution, and improves heavy oil conversion performance and total liquid yield.
Patent Information
- Application Number
- CN202111502842.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-12-09
AI Technical Summary
The existing catalytic cracking catalysts have insufficient pore structure when treating heavy oil, resulting in insufficient cracking activity and resistance to heavy metal pollution, which cannot meet the needs of macromolecular cracking.
Silicon-aluminum materials with high pore volume, large specific surface area and double pore distribution were prepared by inexpensive silicon-aluminum sources, and catalysts were constructed using this as a support, combining matrix and molecular sieve to optimize the pore structure and acidic center distribution of the catalyst.
The pore structure distribution, resistance to heavy metal pollution and heavy oil conversion performance of the catalyst are significantly improved, and the total liquid yield is improved.
Smart Images

Figure CN116251616B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of oil refining catalysts, and in particular relates to a residual oil catalytic cracking catalyst and a preparation method thereof. Background Art
[0002] In order to maximize their benefits, oil refineries have begun to blend more and more residual oil in catalytic cracking units. Compared with distillate oil, residual oil has the characteristics of high density, high boiling point, low H / C atomic ratio, and high metal content. Due to the large molecular diameter of heavy oil molecules and the high heavy metal content, residual oil-based catalytic cracking catalysts need to have more medium and large pores to meet the cracking and diffusion requirements of large molecules. A large number of studies are devoted to introducing medium and large pores into catalytic cracking catalysts.
[0003] One of the main features of the GO-ULTRA catalyst (NPRA, 2010AM-10-175) newly launched by Albemarle in 2009 is the significant improvement in macropore structure. The macropores between 100-400nm have increased significantly, which greatly reduces over-cracking reaction, excessive hydrogen transfer activity and coke polymerization reaction. Compared with its catalyst RUBY, GO-ULTRA has high gasoline and diesel yields and good coke selectivity at the same catalyst-to-oil ratio, conversion rate and coke difference.
[0004] US 6776899 reported that sucrose was added during the catalyst synthesis process to introduce macropores into the matrix, thereby improving the activity and heavy metal resistance of the catalyst. CN1778676A disclosed a method for preparing an in-situ crystallization catalyst, which can effectively improve the pore structure of the catalyst by adding structural additives such as starch and carboxymethyl cellulose.
[0005] US4624773 reports a method for preparing a macroporous catalytic cracking catalyst using carbon black. The introduction of carbon black can produce at least 0.10 cm 3 g -1 Qi Yanping et al. (Energy Fuels, 24(5), 2010, 2825) synthesized a macroporous catalytic cracking catalyst by adding polystyrene beads of different particle sizes and different contents, and found that the addition of polystyrene beads not only introduced medium and macropores, but also improved the catalyst activity.
[0006] ENGHARD's DMS (Distributed Matrix Structures) technology has a card-like stacking morphology between particles and a highly dispersed matrix structure. At the same time, highly dispersed zeolite crystals cover the matrix surface to improve the catalyst selectivity. In addition, in order to improve the cracking ability of heavy oil, the DMS product contains a stable, mesoporous aluminum-rich carrier. The aluminum-rich carrier is obtained by alkali-modified high-temperature calcined kaolin (NPRA-AM-03-38).
[0007] CN201210062013.2 discloses a method for preparing a macroporous catalytic cracking catalyst, by introducing compounds with boiling points less than or equal to 150°C or compounds that decompose and completely convert into gases at 150°C into the spray slurry, and introducing mesopores and macropores during the catalyst spray drying process.
[0008] Zeolite molecular sieves in catalytic cracking catalysts mainly provide micropore channels, while medium and large pores are mainly provided by catalyst matrix materials. Synthesizing matrix materials rich in medium and large pore structures is an important way to prepare large-pore catalytic cracking catalysts and is also a hot topic in the current catalyst field.
[0009] Zheng Jinyu et al. (Petroleum Refining and Chemical Engineering, 2015, 46(9): 47-51) successfully prepared a disordered mesoporous silica-alumina material (JSA) with a pseudo-boehmite structure through gelation and aging processes. The material has a high specific surface area and pore volume, with a specific surface area of 300m 2 / g or more, pore volume greater than 0.7cm 3 / g, and the pore size is between 6 and 7 nm.
[0010] Maryam Khosravi Mardkhe (Applied Catalysis, A: General, 2014, 482: 16-23.) et al. introduced a silicon-doped alumina material. XRD showed that it still had the characteristic diffraction peaks of alumina. By adjusting the silicon content, large pore volume and large pore diameter silicon-doped alumina can be obtained, with a pore volume of 0.33 to 1.83 cm 3 / g range, the maximum pore size can reach 51.6nm.
[0011] CN03147975.8 introduces a mesoporous silicon-aluminum material with a pseudo-boehmite phase structure. The anhydrous chemical expression based on the weight of the oxide is: (0-0.3)Na2O·(40-90)Al2O3·(10-60)SiO2, and its specific surface area is 200-400m 2 / g, the pore volume is 0.5~2.0ml / g, the average pore diameter is 8~20nm, and the most probable pore diameter is 5~15nm.
[0012] CN201110251792.6 The invention provides an acidic silicon-aluminum catalytic material having a pseudo-boehmite crystal phase structure; its anhydrous chemical expression, measured by oxide weight, is: (0-0.2)Na2O·(44-46)SiO2·(54-56)Al2O3, the pore volume is 0.5-1.0 ml / g, and the average pore diameter is 8-15 nm.
[0013] The invention of CN201110251761.0 provides a mesoporous acidic silicon-aluminum catalytic material having a pseudo-boehmite crystal phase structure, and its anhydrous chemical expression is (0-0.2)Na2O·(16-20)SiO2·(80-84)Al2O3, based on the weight of the oxide, with a pore volume of 1.0-2.0 ml / g and an average pore diameter of 8-20 nm. The ratio of pyridine infrared B acid to L acid measured at 200°C of the material is 0.060-0.085.
[0014] CN201210409663.X provides a method for preparing silicon-containing alumina dry glue. The prepared silicon-containing alumina dry glue is calcined at 500°C to 950°C for 2 to 6 hours. The properties of the obtained silicon-containing alumina are as follows: the pore volume is 0.55 to 1.10 mL / g, and the pore volume of pores with a pore diameter of 10 nm to 50 nm accounts for 30% to 80% of the total pore volume.
[0015] Xubenjing et al. (Microporous and Mesoporous materials 238 (2017): 84-89) introduced water glass as a silicon source into the alumina synthesis system to synthesize silicon-containing alumina materials, and investigated the effects of 3%, 6%, 12% and 24% silicon oxide addition on the pore structure of the product. The pore volume of the synthesized material reached up to 1.46 cm 3 / g, with a specific surface area of 427m 2 / g.
[0016] CN201510861407.8 introduces an active mesoporous silicon-aluminum catalytic material having a pseudo-boehmite crystal phase structure and a specific surface area of 200 to 600 m 2 / g, the pore volume is 0.5-2.0 ml / g, the average pore diameter is 8-20 nm, and the ratio of the pyridine infrared B acid content to the L acid content measured at 200°C is 0.055-0.085.
[0017] CN201510864343.7 provides a method for preparing an active catalytic material, the material has a pseudo-boehmite crystal phase structure, and its anhydrous chemical expression is (0-0.2)Na2O·(10-60)SiO2·(40-90)Al2O3, based on the weight of the oxide, and its specific surface area is 200-600m2 / g, pore volume of 0.5-2.0ml / g, average pore size of 8-20nm, particle size distribution of the catalytic material is D(V,0.5)≤4μm, D(V,0.9)≤12μm, and the ratio of pyridine infrared B acid to L acid measured at 200°C is 0.055-0.085. The invention obtains better pore volume and smaller material particle size by online addition of silicon source. The preparation method of the material comprises the following steps: (1) neutralizing an aluminum source and an alkaline solution sodium metaaluminate at room temperature to 85°C to form a gel, and controlling the pH value of the gel process to be maintained at 7-11; (2) adding the required silicon source to the gel slurry in a parallel flow manner in the neutralization gel process according to the weight ratio of SiO2:Al2O3=1:(0.6-9) to achieve online addition of the silicon source, and then aging at room temperature to 90°C for 1-10 hours; (3) exchanging the obtained solid precipitate at room temperature to 100°C for 1-3 times according to the weight ratio of solid precipitate (dry basis): ammonium salt: H2O=1:(0.1-1):(10-30), each time for 0.5-1 hour, until the sodium content in the solid precipitate is less than 0.2%. The active catalytic material obtained by the method provided by the present invention has obvious mesopore characteristics, smaller particle size, contains B acid and L acid centers, and the ratio of B acid to L acid is high, and the material has higher cracking activity.
[0018] CN201710382520.7 discloses a porous catalytic material, the XRD spectrum of which shows a diffuse diffraction peak at a 2θ angle of 25° to 27°, and a FAU crystal phase structure, and its chemical composition contains 50 to 80% silicon and 20 to 50% aluminum by weight of oxides, with a total specific surface area of 250 m 2 / g, the ratio of micropore specific surface area to total specific surface area is ≯28%, the ratio of the number of B acid centers to the number of L acid centers measured by pyridine infrared at 200°C is ≥0.30; when the surface Al / Si atomic ratio measured by XPS method is a, and the bulk Al / Si atomic ratio measured by XRF method is b, a / b=1.1-1.6. The material is a mixture of amorphous silicon aluminum oxide and zeolite.
[0019] CN201710382478.9 discloses a highly active catalytic material, wherein the XRD spectrum of the catalytic material has characteristic diffraction peaks of pseudo-boehmite structure at 2θ angles of 14°, 28°, 38.5°, 49° and 65°, the ratio of the number of B acid centers to the number of L acid centers measured by pyridine infrared at 200°C is 0.10-0.23, the chemical composition calculated by weight of oxides contains 15-45% silicon and 55-85% aluminum, and the specific surface area is 300-500m 2 / g, the average pore size is 5-18nm, when c is the surface Al / Si atomic ratio measured by XPS method, d is the bulk Al / Si atomic ratio measured by XRF method, c / d=1.2-1.6. The preparation method of the material is: adding a silicon source and an alkaline aluminum source into a container in a parallel flow manner at room temperature to 60°C and stirring, controlling the pH value to be 13-14 to mix and form a gel, then adding an acidic aluminum source, and controlling the end point pH value of the slurry system to be 8.0-10.5, then treating at a constant temperature of 40-80°C, washing, filtering, and ion exchange of the obtained solid precipitate to remove impurity ions, wherein the weight ratio of the silicon source to the aluminum source is 1:(1.2-5.7), the silicon source is calculated as silicon oxide, the aluminum source is calculated as aluminum oxide, and is the sum of the alkaline aluminum source and the acidic aluminum source.
[0020] Alumina, silicon-containing alumina or its precursors and silicon-alumina materials are usually prepared by sol-gel method, which is closely related to the pH value, reaction temperature and condensation rate of aluminum and silicon ions. At present, although there are many reports on the preparation of silicon-containing alumina, silicon-containing alumina precursors or silicon-alumina materials, the pore volume of the materials is generally less than 2.0 ml / g and the specific surface area is generally 500 m 2 g -1 The pore size is smaller and mainly single pore distribution, while for macromolecular cracking, such as catalytic cracking, due to the wide distribution of heavy oil molecular size, the material is often required to have double pores or multi-level pore distribution. The present invention is based on the use of cheap silicon aluminum sources to prepare silicon aluminum materials with higher pore volume, large specific surface area, containing B acid centers and double pore distribution, and using them as carrier materials to construct catalytic cracking catalysts with high efficiency heavy oil conversion capabilities. Summary of the invention
[0021] Based on the above, the main purpose of the present invention is to prepare a silicon-aluminum material with higher pore volume, larger specific surface area, containing B acid centers and having a double pore distribution through a cheap silicon-aluminum source, and use this as a carrier material to construct a catalytic cracking catalyst with efficient heavy oil conversion capability.
[0022] To this end, the present invention provides a residual oil catalytic cracking catalyst, which comprises 50-85 parts of a matrix and 15-50 parts of a molecular sieve based on 100 parts of the catalyst mass composition, wherein the matrix comprises 1-20 parts of a silicon-aluminum material based on 100 parts of the catalyst mass composition, wherein the silicon-aluminum material has a pseudo-boehmite structure, and its anhydrous chemical expression is (0-0.2) Na2O: (4-30) SiO2: (70-96) Al2O3 based on the weight of the oxide, and has a double pore distribution of 2-40nm and 70-300nm, and a specific surface area greater than 500 and not greater than 650m 2 / g, the pore volume is 2.1-2.8ml / g, and the ratio of the pyridine infrared B acid content to the L acid content measured at 200°C is 0.10-0.38.
[0023] The residual oil catalytic cracking catalyst of the present invention preferably comprises 60-80 parts of matrix and 20-40 parts of molecular sieve based on 100 parts of catalyst mass, wherein the matrix comprises 4-15 parts of silicon-aluminum material.
[0024] The residual oil catalytic cracking catalyst of the present invention, wherein the silicon-aluminum material has a dual pore distribution of 2-40nm and 70-300nm.
[0025] The residual oil catalytic cracking catalyst of the present invention is preferably prepared by the following steps:
[0026] (1) preheating the acidic aluminum source and sodium aluminate solution to 45-70° C. respectively, adding them into the reaction kettle in parallel, maintaining the temperature at 45-70° C., stirring the reaction, and the pH value of the reaction is 6-8;
[0027] (2) adding a silicon source at a weight ratio of SiO2:Al2O3=0.05-0.43:1, and adding an alcohol solvent and stirring evenly for primary aging, maintaining the primary aging temperature at 45-70°C and the primary aging pH value at 6-8;
[0028] (3) heating to 80-100° C., adding an alkaline solution to adjust the pH value to 8.5-10.0, and performing secondary aging under stirring to obtain a solid precipitate;
[0029] (4) Filter, wash, exchange and dry the obtained solid precipitate.
[0030] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, the preheating first heats the acidic aluminum source and sodium aluminate reaction materials to a certain temperature, which can be achieved in various ways, such as water bath heating, steam heating, and oil bath heating.
[0031] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, the filtering, washing, exchanging and drying of the obtained solid precipitate are conventional technical means in the art, and the exchanging refers to the ammonium exchange and / or acid exchange at 60-100° C. after the product is washed. The following process conditions are recommended for the ammonium exchange: the solid precipitate is exchanged at 60-100° C. according to the weight ratio of precipitate (dry basis): ammonium salt: H2O=1:(0.1-1):(5-10); exchange 1-3 times, each exchange for 0.3-1 hour, until the sodium content in the solid precipitate is less than 0.2wt%. The ammonium salt used for the exchange is selected from one or more of ammonium chloride, ammonium nitrate, ammonium carbonate, ammonium sulfate and ammonium bicarbonate. The acid exchange is recommended to use the following process conditions: the solid precipitate is mixed in a weight ratio of precipitate (dry basis): H2O=1:(5-10), then the pH is adjusted to 2.5-3.5 with an acid solution, and the exchange is carried out at 60-100°C; the exchange is performed 1-3 times, each time for 0.3-1 hour, until the sodium content in the solid precipitate is less than 0.3wt%. The acid solution used for the exchange is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, oxalic acid, and citric acid solutions.
[0032] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, the drying is a general technology and can be carried out in an oven, or by spray drying or flash drying.
[0033] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, the acidic aluminum source is one or more of aluminum nitrate, aluminum sulfate and aluminum chloride.
[0034] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, the concentration of the acidic aluminum source is 50-150 g / L in terms of alumina, and the concentration of the sodium metaaluminate solution is 20-130 g / L in terms of alumina.
[0035] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, the silicon source is selected from one or more of water glass, sodium silicate and silicate compounds.
[0036] In the method for preparing the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, it is preferred that in step (2), the silicon source and the alcohol solvent are added simultaneously, or the silicon source is added first and then the alcohol solvent is added.
[0037] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, the acidic aluminum source is calculated by weight of aluminum oxide, and the added amount of the alcohol solvent is 1-10 times, more preferably 2-5 times, of the acidic aluminum source.
[0038] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, the alcohol solvent is a compound in which hydrogen atoms in saturated aliphatic hydrocarbons and / or alicyclic hydrocarbons are replaced by hydroxyl groups.
[0039] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, the alcohol solvent is a C1-C8 monohydric alcohol, dihydric alcohol or trihydric alcohol, and C2-C4 alcohol is further preferred. More preferably, the alcohol solvent is selected from one or more of ethanol, ethylene glycol, propanol, glycerol, butanol and butanediol.
[0040] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, the first aging time is 0.5-3h, and the second aging time is 0.5-3h.
[0041] In the preparation method of the silicon-aluminum material of the residual oil catalytic cracking catalyst of the present invention, it is preferred that the alkaline solution is selected from one or more of ammonia water, sodium metaaluminate solution, water glass, and sodium hydroxide solution.
[0042] The residual oil catalytic cracking catalyst of the present invention is preferably that the matrix also includes one or more of alumina, clay, silica gel, and silica-alumina colloid, and is further preferably alumina and clay. More preferably, the clay is selected from one or more of kaolin, halloysite, montmorillonite, and bentonite, and the alumina is selected from one or more of α-alumina, β-alumina, γ-alumina, δ-alumina, η-alumina, θ-alumina, alumina precursor pseudo-boehmite, aluminum sol, and aluminum hydroxide.
[0043] The residual oil catalytic cracking catalyst of the present invention is preferably a mixture of two aluminum oxide precursors, more preferably a mixture of pseudo-boehmite and aluminum sol, wherein the aluminum oxide from the pseudo-boehmite is 0 to 40 parts by mass of the catalyst, more preferably 10 to 35 parts; and the aluminum oxide from the aluminum sol is 4 to 15 parts by mass of the catalyst.
[0044] The residue catalytic cracking catalyst of the present invention is preferably that the molecular sieve is various molecular sieves with acidic centers, and is further preferably selected from one or more of Y-type, X-type, Beta, ZSM-5, MOR, MCM-22, HY, REY, USY, REHY, REUSY, and HZSM-5.
[0045] To this end, the present invention also provides a method for preparing a residual oil catalytic cracking catalyst, comprising the following steps: mixing and slurrying a matrix containing silicon-aluminum material and a molecular sieve, adding acid and heating for aging; and then molding, drying and calcining the slurry to obtain a catalyst.
[0046] The preparation method of the slurry described in the present invention is well known to those skilled in the art. The present invention does not impose any specific restrictions on the manner of adding the silicon-aluminum material, and the slurry can be added before or after acidification.
[0047] The method for preparing the residual oil catalytic cracking catalyst of the present invention is preferably that the acid is an inorganic acid, selected from one or more of hydrochloric acid, phosphoric acid, sulfuric acid and nitric acid; further preferably, the aging conditions are: temperature 40-90°C, time 0.5-3 hours.
[0048] The method for preparing the residual oil catalytic cracking catalyst of the present invention is preferably that the molding and drying is spray molding and drying, and the process conditions are that the furnace temperature of the spray tower is controlled at 450-550°C and the spray tail gas temperature is controlled at 200-300°C.
[0049] The method for preparing the residual oil catalytic cracking catalyst of the present invention preferably further comprises treating the obtained catalyst with ion exchange to further remove impurity ions, including Na + , SO4 2- , Cl - Etc., further preferably, the conditions for the ion exchange are: acid exchange or ammonium exchange, pH value 2.5-3.5, and exchange time 0.3-2 hours.
[0050] The beneficial effects of the present invention are as follows:
[0051] The residual oil catalytic cracking catalyst provided by the present invention contains a silicon-aluminum material, which has a higher pore volume, a larger specific surface area, a double pore distribution, a higher thermal stability, a higher acid content, and contains a B acid center. The residual oil catalytic cracking catalyst of the present invention prepared by using the material has a better pore structure distribution, a better resistance to heavy metal pollution, a stronger heavy oil conversion performance and a higher total liquid yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 XRD spectra of the silicon-aluminum material and the industrial pseudo-boehmite material prepared in Example 3. Figure 1 It is shown that the silicon-aluminum material prepared in Example 3 has a pseudo-boehmite crystal phase structure, but its crystallinity is lower than that of industrial pseudo-boehmite.
[0053] Figure 2 This is the SEM image of the silicon-aluminum material prepared in Example 3. Figure 2 It shows that the silicon-aluminum material is composed of stacked nano-short rods, and two types of pore distributions, medium pores and large pores, can be clearly observed.
[0054] Figure 3 This is the BJH pore distribution curve of the silicon-aluminum material AS-3 prepared in Example 3. Figure 3 It shows that the silicon-aluminum material prepared in Example 3 has a dual pore distribution of 2-40nm and 70-300nm, respectively, while the comparative industrial pseudo-boehmite material has only a single pore distribution between 2-4nm, and the pore diameter is 3.4nm; DB-1 and DB-2 are the BJH pore distribution curves of the materials prepared in Comparative Example 1 and Comparative Example 2, respectively. DETAILED DESCRIPTION
[0055] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0056] Analytical methods
[0057] In each embodiment, the content of Na2O, A12O3 and SiO2 in the product was determined by X-ray fluorescence method (see "Analysis Methods in Petrochemical Industry (RIPP Experimental Methods)", edited by Yang Cuiding et al., Science Press, published in 1990). The specific surface area and pore structure were measured by low-temperature nitrogen adsorption-desorption method, and the pore distribution curve was calculated by BJH method. Scanning electron microscopy (SEM) was characterized by ULTRA-Plus field emission scanning electron microscope of Zeiss, Germany.
[0058] Pyridine adsorption infrared spectroscopy (Py-FTIR) was used to characterize the acid type of the sample using a TENSOR-27 Fourier transform infrared spectrometer produced by Bruker Corporation of the United States. 10 mg of the sample was pressed into a tablet and placed in an in-situ detection cell. The surface was cleaned in a vacuum environment at 350°C for two hours, and then infrared analysis was performed.
[0059] The wear strength of the spray microspheres was determined by the gas generation method. The method standard is Q / SYLS 0518-2002, which is the standard of the China Petroleum and Petrochemical Research Institute. Before the measurement, the spray microspheres were not subjected to any calcination: the spray microspheres were placed in the MS-C wear index analyzer, a device for measuring the wear index, and were impacted by air flow for 5 hours. The amount of fine powder collected in the first hour was the amount of fine powder contained in the microsphere preparation itself, and the amount of fine powder collected in the last 4 hours was the amount of fine powder generated (less than 15 μm). The percentage of the mass of the fine powder collected in the last 4 hours to the total mass of the sample was the wear index.
[0060] Pore volume determination by water drop method: Take about 80g of catalyst sample and place it in an evaporating dish, burn it at 480℃ for 1 hour, take it out and cool it in a desiccator, take 20g of sample and add it to a conical flask, accurate to 0.1g. Add distilled water to the conical flask through a burette. With the addition of water, the fluidity of the catalyst deteriorates. Use a glass rod to stir and shake it continuously until the sample loses fluidity and all aggregates together. Note the water consumption and use Vp=V / m to calculate the sample pore volume. Vp-sample pore volume, ml / g; V-consumed titration water volume, ml; m-sample mass, g.
[0061] Source of raw materials
[0062] Aluminum chloride, sodium aluminate, aluminum sulfate, aluminum nitrate, propanol, ethanol, ethylene glycol, butanol, butanediol, ammonium nitrate, ammonium sulfate, ammonium chloride, methyl orthosilicate, ethyl orthosilicate, and sodium silicate are analytical reagents and are produced by Sinopharm Chemical Reagent Co., Ltd.
[0063] Sodium silicate, hydrochloric acid, ammonia water, and industrial pseudo-boehmite were provided by PetroChina Lanzhou Petrochemical Catalyst Plant.
[0064] NaY zeolite directing agent, produced by the catalyst plant of Lanzhou Petrochemical Company;
[0065] Kaolin, an industrial product of China Kaolin Corporation, reduced by 20.43%;
[0066] Pseudo-boehmite, produced by Shanxi Aluminum Plant, reduced by 31.5%;
[0067] Aluminum sol, containing 23.7wt% Al2O3, produced by the catalyst plant of Lanzhou Petrochemical Company;
[0068] REUSY molecular sieve, produced by the catalyst plant of Lanzhou Petrochemical Company, reduced by 7.9%, Na2O content 1.1 wt%, RE2O3 content 7.0 wt%;
[0069] Example 1
[0070] Silicon aluminum material preparation
[0071] Prepare 150g / L aluminum nitrate solution (calculated by weight of alumina, the same below) and 70g / L sodium aluminate solution, and heat them to 55°C and 60°C respectively. Then, add the aluminum nitrate and sodium aluminate solutions into the reactor in parallel with stirring. Keep the gelling temperature at 55°C during the addition process, and control the addition rate of the two solutions so that the gelling pH value = 6.0. Continue stirring for 35 minutes after the addition is completed, then add water glass according to SiO2:Al2O3=0.35:1. After the addition of water glass, add propylene glycol at 5 times the weight of alumina, then continue stirring and aging at 55°C for 2.0 hours, then raise the temperature to 90°C, add water glass to adjust the pH value to 9.5, and stir and age at 90°C for 1.0 hour. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to the ratio of ammonium chloride: solid precipitate (dry basis): water = 0.2:1:5, and ion exchange is performed at 70°C to remove sodium ions therein. The exchange is repeated once, each time for 0.5h. After each exchange, it is washed and filtered, and then dried at 110°C for 20h to obtain the silicon-aluminum material AS-1 provided by the present invention, and the elemental analysis chemical composition is 0.06Na2O:74.1Al2O3:25.9SiO2.
[0072] Catalyst preparation
[0073] 1.56 kg of kaolin (dry basis, industrial product of China Kaolin Corporation, the same below), 1.475 kg of aluminum sol (containing 23.7 wt% Al2O3, produced by the Catalyst Plant of Lanzhou Petrochemical Company, the same below) and 4.3 kg of deionized water are added into a slurrying tank for slurrying, and then 1.62 kg of pseudo-boehmite (solid content 64.18%, product of Shanxi Aluminum Plant, the same below) is added and stirred for 1 hour, and then 145 g of concentrated nitric acid is added and stirred for 1.5 hours, and then aged at 65°C for 2 hours, and then 468 g of medium- and macroporous silicon-aluminum material AS-1 (dry basis, the same below) is added and stirred for 1 hour.
[0074] 1.127 kg of REUSY molecular sieve (solid content 71%, Na2O content 1.1 wt%, RE2O3 content 7.1 wt%, silicon-aluminum ratio 5.1, produced by Lanzhou Petrochemical Company Catalyst Plant, the same below) and 2.5 kg of deionized water were mixed and slurried for 1 hour, then added to the first step slurrying tank, slurried and homogenized for 3 hours, and then spray-dried.
[0075] The catalyst obtained by spray drying was calcined at 550° C. for 1.5 h, then stirred in a hydrochloric acid aqueous solution with a pH of 3.0 for 60 minutes, filtered, and dried at 160° C. for 6 hours to obtain the cracking catalyst CAT-1 provided by the present invention.
[0076] The composition of the catalyst CAT-1 is: 39 wt% kaolin, 26 wt% alumina derived from pseudo-boehmite, 7.0 wt% alumina derived from alumina sol, 8 wt% silica-alumina material AS-1, and 20 wt% REUSY molecular sieve.
[0077] Example 2
[0078] Silicon aluminum material preparation
[0079] Prepare 60g / L aluminum chloride solution and 90g / L sodium aluminate solution, and heat them to 70°C and 45°C respectively. Then, add the aluminum chloride and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 60°C during the feeding process. Control the feeding rate of the two solutions so that the gelling pH value = 8.0. Continue stirring for 25 minutes after the feeding is completed. Then, add sodium silicate solution according to SiO2:Al2O3=0.42:1. After the sodium silicate is added, add butanediol at 3 times the weight of alumina. Then, continue stirring and aging at 60°C for 3.0 hours, then raise the temperature to 80°C, add ammonia water to adjust the pH value to 10.0, and stir and age at 80°C for 0.5 hour. After the obtained product is filtered and washed, the obtained solid precipitate is mixed with solid precipitate (dry basis): water = 1:7, hydrochloric acid is added to adjust the pH to 3.0, and ion exchange is carried out at 90°C to remove sodium ions, the exchange is carried out for 0.8h, and after the exchange, it is washed and filtered, and then dried at 130°C for 10h to obtain the silicon-aluminum material AS-2 provided by the present invention, and the elemental analysis chemical composition is 0.18Na2O:70.2Al2O3:29.6SiO2.
[0080] Catalyst preparation
[0081] 1.771 kg of kaolin, 3.161 kg of aluminum sol and 2.9 kg of deionized water were added to a slurrying tank for slurrying, and then 1.091 kg of pseudo-boehmite was added and stirred for 1.5 hours. Then 171 g of concentrated hydrochloric acid was added and stirred for 2.0 hours. After aging at 70°C for 1.5 hours, 292 g of silica-alumina material AS-2 was added and stirred for 2 hours.
[0082] 1.127 kg of REUSY molecular sieve and 4.3 kg of deionized water were mixed and slurried for 1.5 hours, then added to the first-step slurrying tank, slurried and homogenized for 2 hours, and then spray-dried.
[0083] The catalyst obtained by spray drying was calcined at 500° C. for 2.0 h, then stirred in a hydrochloric acid aqueous solution with a pH of 2.8 for 45 minutes, filtered, and dried at 130° C. for 10 hours to obtain the cracking catalyst CAT-2 provided by the present invention.
[0084] The composition of the catalyst CAT-2 is: 30 wt% kaolin, 14 wt% alumina from pseudo-boehmite, 12 wt% alumina from alumina sol, 4 wt% silica-alumina material AS-2, and 40 wt% REUSY molecular sieve.
[0085] Example 3
[0086] Silicon aluminum material preparation
[0087] Prepare 120g / L aluminum sulfate solution and 50g / L sodium aluminate solution, and heat them to 60°C and 65°C respectively. Then, add the aluminum sulfate and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 63°C during the feeding process. Control the feeding speed of the two solutions so that the gelling pH value is 7.5. Continue stirring for 15 minutes after the feeding is completed. Then, add methyl orthosilicate solution according to SiO2:Al2O3=0.15:1. After the addition of methyl orthosilicate is completed, add propanol at 3 times the weight of alumina. Then, continue stirring and aging at 63°C for 1.0 hour, then raise the temperature to 95°C, add sodium aluminate solution to adjust the pH value to 8.5, and stir and age at 95°C for 2.0 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to ammonium chloride: solid precipitate (dry basis): water = 1:0.4:7, and ion exchange is performed at 90°C to remove sodium ions therein. The exchange is repeated twice, each time for 1.0h. After each exchange, the product is washed and filtered, and then dried at 120°C for 15h to obtain the silicon-aluminum material AS-3 provided by the present invention, and the elemental analysis chemical composition is 0.03Na2O:86.6Al2O3:13.4SiO2.
[0088] Catalyst preparation
[0089] 0.765 kg of kaolin, 1.897 kg of aluminum sol and 3.1 kg of deionized water were added to a slurrying tank for slurrying, and then 2.103 kg of pseudo-boehmite was added and stirred for 1.0 hour. Then 247 g of concentrated hydrochloric acid was added and stirred for 1.0 hour. After aging at 60°C for 1.2 hours, 450 g of silica-alumina material AS-3 was added and stirred for 1.5 hours.
[0090] 2.218 kg of REUSY molecular sieve and 3.4 kg of deionized water were mixed and slurried for 0.5 hours, then added to the first-step slurrying tank, slurried and homogenized for 1.8 hours, and then spray-dried.
[0091] The catalyst obtained by spray drying was calcined at 450° C. for 1.5 h, then stirred in a hydrochloric acid aqueous solution with a pH of 3.3 for 80 minutes, filtered, and dried at 120° C. for 16 hours to obtain the cracking catalyst CAT-3 provided by the present invention.
[0092] The composition of the catalyst CAT-3 is: 17 wt% kaolin, 30 wt% alumina from pseudo-boehmite, 8 wt% alumina from alumina sol, 10 wt% silica-alumina material AS-2, and 35 wt% REUSY molecular sieve.
[0093] Example 4
[0094] Silicon aluminum material preparation
[0095] Prepare 105g / L aluminum chloride solution and 110g / L sodium aluminate solution, and heat them to 45°C and 50°C respectively. Then, add the aluminum chloride and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 47°C during the feeding process. Control the feeding rate of the two solutions so that the gelling pH value = 7.0. Continue stirring for 20 minutes after the feeding is completed. Then, add water glass according to SiO2:Al2O3=0.25:1. After the water glass is added, add butanol at 8 times the weight of alumina. Then, continue stirring and aging at 47°C for 1.5 hours, then raise the temperature to 100°C, add sodium silicate solution to adjust the pH value to 9.0, and stir and age at 100°C for 3.0 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to ammonium sulfate: solid precipitate (dry basis): water = 0.4:1:8, and ion exchange is performed at 80°C to remove sodium ions therein. The exchange is repeated once, each time for 0.75h. After each exchange, it is washed and filtered, and then dried at 150°C for 14h to obtain the silicon-aluminum material AS-4 provided by the present invention, and the elemental analysis chemical composition is 0.09Na2O:79.8Al2O3:20.1SiO2.
[0096] Catalyst preparation
[0097] 2.255 kg of kaolin, 2.898 kg of aluminum sol and 4.5 kg of deionized water were added to a slurrying tank for slurrying, and then 0.857 kg of pseudo-boehmite was added and stirred for 3.0 hours. Then 130 g of concentrated hydrochloric acid was added and stirred for 0.5 hour. After aging at 75°C for 2.0 hours, 770 g of silica-alumina material AS-4 was added and stirred for 3 hours.
[0098] 1.937 kg of REUSY molecular sieve and 2.6 kg of deionized water were mixed and slurried for 1.7 hours, then added to the first slurrying tank, slurried and homogenized for 1.2 hours, and then spray-dried.
[0099] The catalyst obtained by spray drying was calcined at 600° C. for 0.8 h, then stirred in a hydrochloric acid aqueous solution with a pH of 3.5 for 90 minutes, filtered, and dried at 160° C. for 7 hours to obtain the cracking catalyst CAT-4 provided by the present invention.
[0100] The composition of the catalyst CAT-4 is: 41 wt% kaolin, 10 wt% alumina from pseudo-boehmite, 10 wt% alumina from alumina sol, 14 wt% silica-alumina material AS-4, and 25 wt% REUSY molecular sieve.
[0101] Example 5
[0102] Silicon aluminum material preparation
[0103] Prepare 85g / L aluminum sulfate solution and 20g / L sodium aluminate solution, and heat them to 65°C and 70°C respectively. Then, add the aluminum sulfate and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 68°C during the feeding process. Control the feeding speed of the two solutions so that the gelling pH value is 6.5. Continue stirring for 30 minutes after the feeding is completed. Then, add tetraethyl orthosilicate solution according to SiO2:Al2O3=0.05:1. After the addition of tetraethyl orthosilicate is completed, add propanol at 6 times the weight of alumina. Then, continue stirring and aging at 68°C for 0.5 hour, then heat to 85°C, add sodium hydroxide solution to adjust the pH value to 9.8, and stir and age at 85°C for 2.5 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to ammonium nitrate: solid precipitate (dry basis): water = 0.9:1:6, and ion exchange is performed at 95°C to remove sodium ions therein. The exchange is repeated twice, each time for 0.4h. After each exchange, the product is washed and filtered, and then dried at 120°C for 16h to obtain the silicon-aluminum material AS-5 provided by the present invention, and the elemental analysis chemical composition is 0.10Na2O:95.1Al2O3:4.8SiO2.
[0104] Catalyst preparation
[0105] 0.99 kg of kaolin, 1.423 kg of aluminum sol and 2.6 kg of deionized water were added to a slurrying tank for slurrying, and then 0.841 kg of pseudo-boehmite was added and stirred for 1.6 hours. Then 109 g of concentrated hydrochloric acid was added and stirred for 1.4 hours. After aging at 67°C for 1.2 hours, 360 g of silica-alumina material AS-5 was added and stirred for 1.9 hours.
[0106] 1.183 kg of REUSY molecular sieve and 1.7 kg of deionized water were mixed and slurried for 1.3 hours, then added to the first-step slurrying tank, slurried and homogenized for 2.2 hours, and then spray-dried.
[0107] The catalyst obtained by spray drying was calcined at 560° C. for 1.1 h, then stirred in a hydrochloric acid aqueous solution with a pH of 3.2 for 70 minutes, filtered, and dried at 135° C. for 12 hours to obtain the cracking catalyst CAT-5 provided by the present invention.
[0108] The composition of the catalyst CAT-5 is: 33 wt% kaolin, 18 wt% alumina from pseudo-boehmite, 9 wt% alumina from aluminum sol, 12 wt% silica-alumina material AS-5, and 28 wt% REUSY molecular sieve.
[0109] Example 6
[0110] Silicon aluminum material preparation
[0111] Prepare 135g / L aluminum chloride solution and 80g / L sodium aluminate solution, and heat them to 50°C and 55°C respectively. Then, add the aluminum chloride and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 52°C during the feeding process. Control the feeding rate of the two solutions so that the gelling pH value is 7.8. Continue stirring for 10 minutes after the feeding is completed. Then, add water glass according to SiO2:Al2O3=0.30:1. After the water glass is added, add ethanol at twice the weight of alumina. Then, continue stirring and aging at 52°C for 2.5 hours, then raise the temperature to 82°C, add ammonia solution to adjust the pH value to 9.3, and stir and age at 82°C for 1.5 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to the ratio of ammonium chloride: solid precipitate (dry basis): water = 0.6:1:10, and ion exchange is performed at 85°C to remove sodium ions therein. The exchange is repeated once, each time for 0.6h. After each exchange, the product is washed and filtered, and then dried at 140°C for 12h to obtain the silicon-aluminum material AS-6 provided by the present invention, and the elemental analysis chemical composition is 0.13Na2O:76.8Al2O3:23.1SiO2.
[0112] Catalyst preparation
[0113] 1.86 kg of kaolin, 3.477 kg of aluminum sol and 3.7 kg of deionized water were added to a slurrying tank for slurrying, and then 2.057 kg of pseudo-boehmite was added and stirred for 2.3 hours. Then 254 g of concentrated hydrochloric acid was added and stirred for 1.7 hours. After aging at 73°C for 1.6 hours, 360 g of silica-alumina material AS-6 was added and stirred for 2.1 hours.
[0114] 2.535 kg of REUSY molecular sieve and 3.1 kg of deionized water were mixed and slurried for 0.9 hours, then added to the first slurrying tank, slurried and homogenized for 1.6 hours, and then spray-dried.
[0115] The catalyst obtained by spray drying was calcined at 590° C. for 1.3 h, then stirred in a hydrochloric acid aqueous solution with a pH of 2.7 for 85 minutes, filtered, and dried at 155° C. for 8 hours to obtain the cracking catalyst CAT-6 provided by the present invention.
[0116] The composition of the catalyst CAT-6 is: 31 wt% kaolin, 22 wt% alumina from pseudo-boehmite, 11 wt% alumina from aluminum sol, 6 wt% silica-alumina material AS-5, and 30 wt% REUSY molecular sieve.
[0117] Comparative Example 1
[0118] Silicon aluminum material preparation
[0119] Comparative Example 1 was prepared according to the preparation process of CN201510864343.7.
[0120] Aluminum sulfate and sodium aluminate are used as raw materials, and the gel is formed at 63°C in parallel, and the pH value of the gel is controlled to be 7.5. At the same time, methyl orthosilicate solution is added online according to SiO2:Al2O3=0.15:1, and mixed with the gel slurry in parallel. After the raw materials are added, the slurry is heated to 90°C and aged for 2.0 hours. After filtering and washing, the obtained product is mixed with ammonium chloride: solid precipitate (dry basis): water=1:0.4:10, and ion exchange is carried out at 90°C to remove sodium ions. The exchange is repeated twice, each time for 1.0h, and after each exchange, it is washed and filtered, and then dried at 120°C for 15h, and the comparative silicon aluminum material DB-1 is obtained, and the elemental analysis chemical composition is 0.04Na2O:86.8Al2O3:13.2SiO2.
[0121] Catalyst preparation
[0122] 0.765 kg of kaolin, 1.897 kg of aluminum sol and 3.1 kg of deionized water were added to a slurrying tank for slurrying. Then 2.103 kg of pseudo-boehmite was added and stirred for 1.0 hour. Then 247 g of concentrated hydrochloric acid was added and stirred for 1.0 hour. After aging at 60°C for 1.2 hours, 450 g of silica-alumina material DB-1 was added and stirred for 1.5 hours.
[0123] 2.218 kg of REUSY molecular sieve and 3.4 kg of deionized water were mixed and slurried for 0.5 hours, then added to the first-step slurrying tank, slurried and homogenized for 1.8 hours, and then spray-dried.
[0124] The catalyst obtained by spray drying was calcined at 450° C. for 1.5 h, then stirred in a hydrochloric acid aqueous solution with a pH of 3.3 for 80 minutes, filtered, and dried at 120° C. for 16 hours to obtain the cracking catalyst CAT-A provided by the present invention.
[0125] The composition of the catalyst CAT-A is: 17 wt% kaolin, 30 wt% alumina from pseudo-boehmite, 8 wt% alumina from alumina sol, 10 wt% silica-alumina material DB-1, and 35 wt% REUSY molecular sieve.
[0126] Comparative Example 2
[0127] Silicon aluminum material preparation
[0128] Comparative Example 2 was prepared according to the preparation process of CN201710382520.7.
[0129] A small amount of deionized water was added to the beaker, and then water glass (250 g / L, silicon oxide) and sodium aluminate solution (110 g / L, aluminum oxide) were added in parallel at 47°C by strong stirring, and the flow rate was controlled so that the water glass and sodium aluminate were added at the same time, and the pH value was 13.0; then 105 g / L of aluminum chloride solution was added, and the end point pH value of the slurry system was controlled to be 9.0, and then the product was treated at a constant temperature for 3.0 hours at 100°C. After filtering and washing, the obtained solid precipitate was mixed according to ammonium sulfate: solid precipitate (dry basis): water = 0.4:1:8, and ion exchange was performed at 80°C to remove the sodium ions therein, and the exchange was repeated once, each time for 0.75h, and after each exchange, it was washed and filtered, and then dried at 150°C for 14h, and the comparative silicon aluminum material DB-2 was obtained, and the elemental analysis chemical composition was 0.08Na2O:79.9Al2O3:20.0SiO2.
[0130] Catalyst preparation
[0131] 2.255 kg of kaolin, 2.898 kg of aluminum sol and 4.5 kg of deionized water were added to a pulping tank for pulping, and then 0.857 kg of pseudo-boehmite was added and stirred for 3.0 hours. Then 130 g of concentrated hydrochloric acid was added and stirred for 0.5 hour. After aging at 75°C for 2.0 hours, 770 g of silica-alumina material DB-2 was added and stirred for 3 hours.
[0132] 1.937 kg of REUSY molecular sieve and 2.6 kg of deionized water were mixed and slurried for 1.7 hours, then added to the first slurrying tank, slurried and homogenized for 1.2 hours, and then spray-dried.
[0133] The catalyst obtained by spray drying was calcined at 600°C for 0.8h, then stirred in a hydrochloric acid aqueous solution with pH=3.5 for 90 minutes, filtered, and dried at 160°C for 7 hours to obtain the cracking catalyst CAT-B provided by the present invention.
[0134] The composition of the catalyst CAT-B is: 41 wt% kaolin, 10 wt% alumina from pseudo-boehmite, 10 wt% alumina from alumina sol, 14 wt% silica-alumina material DB-2, and 25 wt% REUSY molecular sieve.
[0135] Table 1 provides the pore structure data and pyridine infrared acidity data of samples AS-1 to AS-6 prepared in Examples 1-5, as well as industrial pseudo-boehmite and comparative tests.
[0136] Table 1 Physicochemical properties of different samples
[0137]
[0138] Table 2 Catalyst composition
[0139]
[0140] Table 3 Physical and chemical properties of catalysts
[0141]
[0142] In Table 3, the pore volume* was measured using the water drop method.
[0143] As can be seen from Table 3, the analysis of the physical and chemical properties of the catalyst shows that the catalyst of the present invention, which introduces silicon-aluminum materials with specific physical and chemical properties, has a higher water droplet method pore volume than the comparative catalyst.
[0144] Test Example 1
[0145] Catalyst Evaluation:
[0146] The catalyst reaction performance was evaluated using a fixed fluidized bed device, and the raw oil used was Xinjiang vacuum wide fraction wax oil and Xinjiang vacuum residue oil, with a residue blending ratio of 30%. The raw oil properties are shown in Table 4. Table 5 shows the catalyst after aging at 800°C and 100% steam for 10 hours; and the catalytic cracking reaction conditions are: reaction temperature 500°C, catalyst-oil mass ratio of 4.0.
[0147] Table 4 Properties of feedstock oil used for catalyst selectivity evaluation
[0148]
[0149] Table 5 Catalyst reaction evaluation results
[0150]
[0151] As shown in Table 5, compared with Comparative Example 1, the oil slurry yield of Example 3 decreased by 1.06 percentage points, and the total liquid yield increased by 1.58 percentage points; compared with Comparative Example 2, the oil slurry yield of Example 4 decreased by 1.31 percentage points, and the total liquid yield increased by 1.44 percentage points. For the catalytic device, the total liquid yield increased by only 0.5 percentage points, which can bring huge economic benefits to the oil refining enterprise.
[0152] In summary, the evaluation results of the fixed fluidized bed show that after the catalyst of the present invention adds silicon-aluminum materials with specific physical and chemical properties, the catalyst reaction performance is improved. Compared with the control catalyst, it shows the advantages of high conversion rate, strong heavy oil conversion ability and increased total liquid yield.
[0153] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.
Claims
1. A residual oil catalytic cracking catalyst, comprising 50 to 85 parts of a matrix and 15 to 50 parts of a molecular sieve, based on 100 parts of the catalyst by mass, characterized in that: The matrix contains 1 to 20 parts of a silicon-aluminum material based on 100 parts of the catalyst mass. The silicon-aluminum material has a pseudo-boehmite structure, and its anhydrous chemical expression is (0-0.2)Na2O: (4-30)SiO2: (70-96)Al2O3 based on the weight of the oxide, and its specific surface area is greater than 500 m 2 / g, and not more than 650 m 2 / g, the pore volume is 2.1-2.8ml / g, and the ratio of the pyridine infrared B acid content to the L acid content measured at 200°C is 0.13-0.
38.
2. The residual oil catalytic cracking catalyst according to claim 1, characterized in that Based on 100 parts of catalyst mass composition, the residual oil catalytic cracking catalyst comprises 60-80 parts of matrix and 20-40 parts of molecular sieve, and the matrix comprises 4-15 parts of silicon-aluminum material.
3. The residual oil catalytic cracking catalyst according to claim 1, characterized in that: The silicon aluminum material has a dual pore distribution of 2-40 nm and 70-300 nm.
4. The residual oil catalytic cracking catalyst according to claim 1, characterized in that: The silicon-aluminum material is prepared by the following steps: (1) Preheat the acidic aluminum source and sodium aluminate solution to 45-70°C respectively, add them into the reactor in parallel, maintain the temperature at 45-70°C, stir and react, and the pH value of the reaction is 6-8; (2) Add silicon source at a weight ratio of SiO2: Al2O3 = 0.05-0.43:1, and add alcohol solvent and stir evenly for primary aging, maintaining the primary aging temperature at 45-70°C and the primary aging pH value at 6-8; (3) Raising the temperature to 80-100°C, adding an alkaline solution to adjust the pH value to 8.5-10.0, and performing secondary aging under stirring to obtain a solid precipitate; (4) Filter, wash, exchange and dry the obtained solid precipitate.
5. The residual oil catalytic cracking catalyst according to claim 4, characterized in that The acidic aluminum source is one or more of aluminum nitrate, aluminum sulfate and aluminum chloride.
6. The residual oil catalytic cracking catalyst according to claim 4, characterized in that: The concentration of the acidic aluminum source is 50-150 g / L in terms of aluminum oxide, and the concentration of the sodium metaaluminate solution is 20-130 g / L in terms of aluminum oxide.
7. The residual oil catalytic cracking catalyst according to claim 4, characterized in that: The silicon source is selected from one or more of sodium silicate and silicate compounds.
8. The residual oil catalytic cracking catalyst according to claim 4, characterized in that: The silicon source is selected from water glass.
9. The residual oil catalytic cracking catalyst according to claim 4, characterized in that: In step (2), the silicon source and the alcohol solvent are added simultaneously, or the silicon source is added first and then the alcohol solvent.
10. The residual oil catalytic cracking catalyst according to claim 4, characterized in that: The acidic aluminum source is based on the weight of aluminum oxide, and the added amount of the alcohol solvent is 1-10 times that of the acidic aluminum source.
11. The residual oil catalytic cracking catalyst according to claim 10, characterized in that: The acidic aluminum source is based on the weight of aluminum oxide, and the added amount of the alcohol solvent is 2-5 times that of the acidic aluminum source.
12. The residual oil catalytic cracking catalyst according to claim 4, characterized in that: The alcohol solvent is a compound in which hydrogen atoms in saturated aliphatic hydrocarbons and / or alicyclic hydrocarbons are replaced by hydroxyl groups.
13. The residual oil catalytic cracking catalyst according to claim 12, characterized in that: The alcohol solvent is a C1-C8 monohydric alcohol, dihydric alcohol or trihydric alcohol.
14. The residual oil catalytic cracking catalyst according to claim 13, characterized in that: The alcohol solvent is a C2-C4 alcohol.
15. The residual oil catalytic cracking catalyst according to claim 13, characterized in that: The alcohol solvent is selected from one or more of ethanol, ethylene glycol, propanol, glycerol, butanol and butanediol.
16. The residual oil catalytic cracking catalyst according to claim 4, characterized in that: The time of the first aging is 0.5-3 h, and the time of the second aging is 0.5-3 h.
17. The residual oil catalytic cracking catalyst according to claim 4, characterized in that: The alkaline solution is selected from one or more of ammonia water, sodium aluminate solution, water glass, and sodium hydroxide solution.
18. The residual oil catalytic cracking catalyst according to claim 1, characterized in that: The matrix also includes one or more of alumina, clay, silica gel, and silica-alumina gel.
19. The residual oil catalytic cracking catalyst according to claim 1, characterized in that: The matrix also includes alumina and clay.
20. The residual oil catalytic cracking catalyst according to claim 1, characterized in that: The molecular sieve is selected from one or more of Y-type, X-type, Beta, ZSM-5, MOR, MCM-22, HY, REY, USY, REHY, REUSY, and HZSM-5.
21. A method for preparing a residual oil catalytic cracking catalyst according to any one of claims 1 to 20, characterized in that: The following steps are involved: The matrix containing silicon-aluminum material is mixed with molecular sieve and slurried, and then acid is added and the temperature is raised for aging; then the slurry is molded, dried and calcined to obtain a catalyst.
22. The method for preparing a residual oil catalytic cracking catalyst according to claim 21, characterized in that: The method also includes subjecting the obtained catalyst to acid exchange or ammonium exchange treatment.