Preparation of Ru single atom-loaded MOF / C3N4 and its application in photocatalytic carbon dioxide reduction and nitrogen fixation
By growing Ru single atom-supported MOF/C3N4 catalyst in situ on C3N4 material, the problems of photocarrier recombination and hydrogen evolution reaction in photocatalytic carbon dioxide reduction and nitrogen fixation reaction are solved, and efficient catalytic activity and stability are achieved. CO, The yields of CH4 and NH3 are significantly improved, and Gibbs free energy is reduced.
Patent Information
- Application Number
- CN202310345357.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-04-03
AI Technical Summary
In photocatalytic carbon dioxide reduction and nitrogen fixation reaction, the recombination of photogenerated carriers and hydrogen evolution reaction limit the catalytic activity, resulting in low catalyst utilization and insufficient reaction activity.
By growing metal organic frames (MOFs) in situ on C3N4 materials and introducing Ru single atoms, forming Ru single atom-loaded MOF/C3N4 catalysts, fixing Ru single atoms using the unsaturated coordination sites of MOFs to inhibit photogenerated carrier recombination and improve catalytic activity.
The activity of photocatalytic carbon dioxide reduction and nitrogen fixation reaction was significantly improved. The CO yield was 3 times that of C3N4, the CH4 yield was 4 times that of MOF/C3N4, and the NH3 yield was 3 times that of MOF/C3N4 and C3N4, while reducing the reaction. The Gibbs free energy in the process improves the photocurrent and stability of the catalyst.
Smart Images

Figure CN116251625B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photocatalytic technology, and in particular to a method for preparing Ru single-atom-loaded MOF / C3N4 and its application in photocatalytic carbon dioxide reduction and nitrogen fixation. Background Art
[0002] As a new type of green energy, photocatalysis has attracted the attention of many researchers in the current energy crisis and environmental problems. In the process of photocatalytic research, great progress has been made in photocatalytic water splitting, photocatalytic degradation, photocatalytic carbon dioxide reduction and photocatalytic nitrogen fixation. In recent years, photocatalytic carbon dioxide reduction reaction (CO2RR) and photocatalytic nitrogen reduction reaction (NRR) have become research hotspots. CO2RR is the reduction of CO2 as a greenhouse gas to CO, CH4 and other valuable fuels. Compared with the traditional method of Haber Bosch, NRR, which converts nitrogen into ammonia products that people can use directly, can effectively reduce energy consumption and pollution. Both CO2RR and NRR can effectively reduce greenhouse gas emissions and are a promising way to solve the energy crisis. Current research mainly focuses on single photocatalytic reactions (CO2RR or NRR). If the catalyst can photocatalyze CO2 and N2, the utilization rate of the catalyst can be greatly improved. The main mechanism of CO2RR and NRR is that semiconductor materials generate photogenerated electrons and holes (photogenerated charge carriers) under light conditions, and the photogenerated charge carriers move to the catalyst surface and contact with the reactants to generate products. This also provides a theoretical possibility for achieving dual catalysis of CO2RR and NRR.
[0003] The main problem affecting the photocatalytic activity is the severe recombination of photogenerated carriers, in which photogenerated electrons recombine with photogenerated holes when moving from the bulk to the surface. At the same time, the hydrogen evolution reaction (HER) is also an important factor limiting CO2RR and NRR. Schrauzer et al. believed that HER competes with CO2RR and NRR. This is because the reaction process requires reactive hydrogen (H) produced by water decomposition. + ) and reactive oxygen (O 2- ), and the reactive hydrogen easily combines to produce H2, thereby reducing the concentration of reactive hydrogen. And the generated H2 is very easy to adhere to the catalyst surface, which hinders the contact between the reactants and the catalyst, thereby inhibiting the activity of CO2RR and NRR. In electrochemistry, the inhibition of hydrogen in the electrochemical reduction of CO2 and N2 has been studied. At the same time, the single atom inhibition of hydrogen has also been studied.
[0004] Since their discovery, single atom catalysts (SACs) have shown excellent catalytic activity in many fields such as electrocatalysis and photocatalysis. Compared with nanocluster catalysts, SACs have high selectivity and activity due to the presence of unsaturated sites. In addition, SACs can significantly improve the efficiency of atom utilization. SACs are not electrons with zero valence charge. SACs are usually stabilized by covalent coordination or ionic interactions with surface atoms or ligands on adjacent supports, thereby generating partial charges through the interaction of metal supports. However, the atoms themselves are unstable and easily agglomerated and deactivated, so the choice of template is crucial. Metal-organic framework (MOF) materials with high specific surface area, unsaturated coordination sites, high tunability and chemical stability. It is also a hot material studied by researchers. Therefore, MOF is one of the ideal supports for fixing single atoms, and its unique structure is more conducive to the dispersion and fixation of single atoms. Summary of the invention
[0005] Purpose of the invention: In view of the problems existing in the prior art, the present invention provides a method for preparing Ru single-atom-loaded MOF / C3N4 and its application in photocatalytic carbon dioxide reduction and nitrogen fixation. Ru single-atom-loaded MOF / C3N4 material is formed by in-situ growth of MOF and in-situ anchoring of Ru single atoms on C3N4 sheets. The catalyst prepared by the present invention has high photocurrent, low surface resistance and effective inhibition of photogenerated carrier recombination, and has excellent catalytic activity for both CO2RR and NRR.
[0006] Technical solution: The present invention provides a method for preparing Ru single atom-loaded MOF / C3N4, comprising the following steps:
[0007] Step 1, dissolving 2,5-dihydroxyterephthalic acid and Zn(NO3)2·6H2O in DMF solvent, slowly adding deionized water and stirring until completely mixed to obtain a mixed solution;
[0008] Step 2, adding C3N4 to the mixed solution and stirring, and adding RuCl3 dropwise during the stirring process;
[0009] Step 3, diluting triethylamine with DMF solvent, and adding the diluted solution dropwise to the product obtained in step 2, stirring, centrifuging, washing, and drying;
[0010] Step 4: calcine the dried product under a hydrogen atmosphere to obtain Ru single atom-loaded MOF / C3N4.
[0011] Further, the mass ratio of 2,5-dihydroxyterephthalic acid, Zn(NO3)2·6H2O and C3N4 is 1:4.5:20-50;
[0012] And / or, in step 2, the RuCl3 is specifically 1-5 mL of RuCl3 with a concentration of 10 mg / mL.
[0013] Furthermore, the specific preparation steps of the C3N4 are as follows:
[0014] S1. Add melamine and phosphite to deionized water, stir evenly, react at 170-180°C for 9-10h, wash and dry to obtain a precursor;
[0015] S2. Mix the precursor, glycerol and ethanol, reflux at 90-100° C. for 3-4 hours, wash and dry to obtain a solid product, and then calcine and sonicate the solid product to obtain C3N4.
[0016] Further, in S1, the mass ratio of melamine to phosphite is 1:1.2;
[0017] And / or, in S2, the mass volume ratio of the precursor, glycerol and ethanol is 0.6g:5mL:15mL.
[0018] Further, in S1, the stirring is specifically stirring in a water bath at 80-90° C. for 1-2 h;
[0019] and / or, in S2, the calcination is specifically calcined at 500° C. for 2 h at a heating rate of 2° C. / min;
[0020] And / or, in S2, the ultrasonic treatment is specifically ethanol ultrasonic treatment for 9-10 hours.
[0021] Furthermore, in step 1, the volume ratio of the DMF solvent to deionized water is 10:1;
[0022] And / or, in step 3, the volume ratio of the DMF solvent to triethylamine is 5:1.
[0023] Furthermore, in step 4, the specific conditions of the calcination are calcination at 200° C. for 2 h at a heating rate of 10° C. / min.
[0024] Preferably, in step 2, the stirring time is 11-13h;
[0025] And / or, in step 3, the stirring time is 1-2h;
[0026] And / or, in step three, the drying is specifically drying under vacuum at 50-60° C. for 11-13 h.
[0027] The present invention also provides an application of Ru single-atom-loaded MOF / C3N4 prepared by any of the methods described above in photocatalytic carbon dioxide reduction.
[0028] The present invention also provides an application of Ru single-atom loaded MOF / C3N4 prepared by any of the methods described above in photocatalytic nitrogen fixation.
[0029] The synthesis process of the Ru single atom-loaded MOF / C3N4 prepared by the present invention is as follows: Figure 1 As shown. We first added the sheet C3N4 to the Zn(NO3)2·6H2O solution (including ligands: 2,5-DOBDC; DMF and H2O) and stirred it for a long time. The purpose is to make the Zn ions adhere evenly to the surface of C3N4, which is more conducive to the relatively uniform dispersion of MOF during the in situ synthesis process. Then RuCl3 was added to the solution. After stirring for a certain period of time, triethylamine solution was slowly added. The triethylamine solution promotes the combination of zinc ions with ligands to form MOF-74. Since MOF has unsaturated coordination, Ru ions will coordinate with the unsaturated coordination sites on MOF and fix the dispersed Ru to form Ru single atoms.
[0030] Beneficial effects: The Ru single atom-loaded MOF / C3N4 material prepared by the present invention is formed by the in-situ growth of MOF and the in-situ anchoring of Ru single atoms on C3N4 sheets. It has excellent catalytic activity for both CO2RR and NRR, and the CO yield is 3 times that of C3N4, the CH4 yield is 4 times that of MOF / C3N4, and the NH3 yield is 3 times that of MOF / C3N4 and C3N4. The Ru single atom-loaded MOF / C3N4 catalyst prepared by the present invention has high photocurrent, low surface resistance and effective inhibition of photogenerated carrier recombination. Through theoretical calculations, it is found that the 4d orbital of Ru can form doping energy levels and promote electron transfer. At the same time, the introduction of Ru can significantly reduce the Gibbs free energy in the CO2RR and NRR reaction processes. The present invention has important guidance and significance for the synthesis of single-atom catalytic materials with high photocatalytic CO2RR and NRR activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Schematic diagram of the synthesis process of Ru single atom-loaded MOF / C3N4 prepared in the present invention;
[0032] Figure 2 This is a spherical aberration corrected HAADF-STEM image of the Ru / MOF / C3N4 material prepared in Embodiment 1 of the present invention;
[0033] Figure 3 Line scan intensity distribution diagram (a) and TEM image (b) of Ru / MOF / C3N4 material prepared in embodiment 1 of the present invention;
[0034] Figure 4This is a line scanning intensity curve diagram of the Ru / MOF / C3N4 material prepared in Embodiment 1 of the present invention;
[0035] Figure 5 This is a schematic diagram of EDS characterization of the Ru / MOF / C3N4 material prepared in Embodiment 1 of the present invention;
[0036] Figure 6 Schematic diagram of the structural model of the Ru / MOF / C3N4 material prepared in Embodiment 1 of the present invention;
[0037] Figure 7 XANES spectrum of the Ru / MOF / C3N4 material prepared in Embodiment 1 of the present invention;
[0038] Figure 8 FT-EXAFS spectrum of the Ru / MOF / C3N4 material prepared in Embodiment 1 of the present invention;
[0039] Fig. 9 Ru k-edge wavelet transform function of Ru / MOF / C3N4 material, Ru and RuO2 prepared in embodiment 1 of the present invention;
[0040] Fig.10 Schematic diagram of photocurrent response (a) and EIS graph (b) of Ru / MOF / C3N4, MOF-74, MOF / C3N4 and C3N4 materials;
[0041] Fig.11 Photoluminescence emission spectra (a) and transient fluorescence spectra (b) of Ru / MOF / C3N4, MOF-74 and MOF / C3N4 materials;
[0042] Fig.12 Schematic diagram of the CO (a), CH4 (b), NH3 (c), and H2 (d) yields of the photocatalytic reactions of Ru / MOF / C3N4, MOF-74, MOF / C3N4, and C3N4 materials;
[0043] Fig.13 Schematic diagram of CH4 production from the photocatalytic reaction of the catalyst under CO2 and Ar gas;
[0044] Fig.14 Schematic diagram of the apparent quantum yield of Ru / MOF / C3N4 materials at different wavelengths (a) and schematic diagram of their cyclic activity (b, c, d);
[0045] Fig.15 Schematic diagram of the geometric structure of MOF-74 and Ru / MOF-74 materials;
[0046] Fig.16Calculated free energy diagrams for the photocatalytic (a) CO2RR, (b) NRR (distal), and (c) NRR (alternating) pathways of MOF-74 and Ru / MOF-74 materials.
[0047] Fig.17 Schematic diagram of the energy band structure of type II heterojunction C3N4 and Ru / MOF-74 materials. DETAILED DESCRIPTION
[0048] The present invention is described in detail below in conjunction with the accompanying drawings.
[0049] Implementation 1:
[0050] The present invention provides a method for preparing a Ru single atom-loaded MOF / C3N4 material, and the specific steps are as follows:
[0051] Step 1: Preparation of C3N4:
[0052] 1 g of melamine and 1.2 g of phosphite were added to 100 ml of H2O and stirred at 80°C for 1 h in a water bath. The solution was then transferred to a Teflon reactor and heated at 180°C for 10 h. The resulting product was washed three times with water and dried at 60°C for 10 h to obtain the precursor. 0.6 g of the precursor was added to a flask containing 5 ml of glycerol and 15 ml of ethanol and refluxed at 90°C for 3 h. The solid product was then washed three times with ethanol and dried at 60°C for 10 h. Finally, the product was calcined at 500°C for 2 h in a muffle furnace at a heating rate of 2°C / min. The product was ultrasonically treated by ethanol for 10 h to obtain C3N4.
[0053] Step 2: Preparation of Ru single atom loaded MOF / C3N4:
[0054] 0.045 g Zn(NO3)2·6H2O and 0.01 g 2,5-dihydroxyterephthalic acid (2,5-DOBDC) were weighed and added to 50 mL N,N-dimethylformamide (DMF), and then 5 mL H2O was slowly added to the solution and stirred until completely dissolved. Then 0.5 g C3N4 was added and magnetically stirred for 12 h. During the stirring process, 1 mL of RuCl3 with a concentration of 10 mg / mL was slowly added to the solution and stirred for 1 h. 1 mL of triethylamine was diluted into 5 mL DMF and then added dropwise to the solution and stirred for 1 h. The catalyst was centrifuged, washed and dried under vacuum at 60 °C for 12 h. Finally, the product was calcined at 200 °C for 2 h under a hydrogen atmosphere at a heating rate of 10 °C / min to obtain Ru single atom-loaded MOF / C3N4 material, recorded as Ru / MOF / C3N4.
[0055] The Ru single atom-loaded MOF / C3N4 material prepared in this embodiment was characterized, and the results are as follows:
[0056] like Figure 2 As shown in Figure 2, the presence of a large number of Ru single atoms can be demonstrated by spherical aberration-corrected high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM). The widespread and uniform distribution of Ru single atoms without aggregation indicates that the MOF material plays a key role in the immobilization of Ru single atoms as a template. Figure 3 As shown in a, the size of a single Ru atom is about 0.2 nm. Figure 3 b shows the MOF particles formed on C3N4 during the in situ synthesis process. It can be seen that this in situ synthesis allows the formation of very small MOFs with a size of about 2-3 nm on the surface. The small size and dispersion of MOF are more conducive to suppressing the aggregation of Ru single atoms. We performed a line scan on the catalyst surface ( Figure 4 a), it was found that the peak position of Zn represents MOF, and the peak position of Ru is the same as that of Zn ( Figure 4 b), indicating that Ru atoms only exist in MOF, but not on the C3N4 surface of the material. In addition, the EDS characterization of Ru / MOF / C3N4 can also reveal the distribution of Zn and Ru elements. It can be seen that Ru is evenly distributed, which is consistent with the distribution range of Zn ( Figure 5 a, b, c, d).
[0057] Since electron microscopy usually only provides structural information of a specific local area, we performed XAFS analysis to further obtain more information about the overall structure of the atomic distribution. The Ru single atom forms a Ru-O bond with the unsaturated coordinated oxygen in the MOF, and the most stable position of Ru is obtained by calculation, from which we constructed the following Figure 6 The structural model is shown. X-ray absorption near-edge structure (XANES) analysis was performed to first observe the electronic structure of Ru. It can be seen that the white line intensity of Ru / MOF / C3N4 is higher than that of Ru foil and RuO2 ( Figure 7 ), indicating that the Ru species in Ru / MOF / C3N4 is in an oxidized form (Ru δ+ ). We further used X-ray absorption fine structure spectroscopy (XAFS) to resolve the local fine structure of Ru / MOF / C3N4. The Fourier transform extended X-ray absorption fine structure (EXAFS) spectrum of Ru / MOF / C3N4 showed a main peak at 1.5Å, which was attributed to Ru-O ( Figure 8). In contrast to the EXAFS spectra of Ru foil and RuO2, Ru / MOF / C3N4 shows no peak at 2.4Å for Ru-Ru coordination, indicating that Ru atoms are not aggregated and are distributed atomically in MOF. The corresponding wavelet transform (WT) map also shows the atomic dispersion of Ru, with an intensity maximum at 4.5Å -1 , from Ru scattering ( Fig. 9 ). Quantitative structural parameter analysis based on EXAFS spectrum fitting shows that a single Ru atom is coordinated with about three O atoms, which is consistent with the established structural model.
[0058] Implementation 2:
[0059] This embodiment is substantially the same as Embodiment 1, the main difference being that the amount of RuCl3 added is specifically 3 mL of RuCl3 with a concentration of 10 mg / mL, and other conditions remain unchanged.
[0060] Apart from this, this embodiment is completely the same as Embodiment 1 and will not be described in detail here.
[0061] Implementation 3:
[0062] This embodiment is substantially the same as Embodiment 1, the main difference being that the amount of RuCl3 added is specifically 5 mL of RuCl3 with a concentration of 10 mg / mL, and other conditions remain unchanged.
[0063] Apart from this, this embodiment is completely the same as Embodiment 1 and will not be described in detail here.
[0064] Comparative Example 1:
[0065] MOF-74: Weigh 0.952 g Zn(NO3)2·6H2O and 0.1 g 2,5-dihydroxyterephthalic acid (2,5-DOBDC), add them to 200 mL N,N dimethylformamide (DMF), and stir for 1 hour until the solid is completely dissolved. Then slowly add 10 ml H2O to the solution, and add 1 ml triethylamine dropwise to form a yellow precipitate. The resulting precipitate is centrifuged, washed, and dried in a vacuum oven at 60 °C for 24 hours to obtain the final catalyst.
[0066] Comparative Example 2:
[0067] MOF / C3N4: Weigh 0.045 g Zn(NO3)2·6H2O and 0.01 g 2,5-dihydroxyterephthalic acid (2,5-DOBDC), add them to 50 mL N,N-dimethylformamide (DMF), slowly add 5 mL H2O, and stir until completely dissolved. Then add 0.5 g C3N4 and stir magnetically for 12 h. Dilute 1 mL triethylamine into 5 mL DMF, then add dropwise to the solution and stir for 1 h. Centrifuge the catalyst, wash it, and finally dry it at 60 ° C under vacuum for 12 h to obtain the catalyst.
[0068] Comparative Example 3:
[0069] Ru / MOF-74: 0.045 g Zn(NO3)2·6H2O and 0.01 g 2,5-dihydroxyterephthalic acid (2,5-DOBDC) were weighed and added to 50 mL N,N-dimethylformamide (DMF), and then 5 mL H2O was slowly added to the solution and stirred until completely dissolved. During stirring, 1 mL of RuCl3 with a concentration of 10 mg / mL was slowly added to the solution and stirred for 1 hour. 1 mL of triethylamine was diluted into 5 mL DMF and then added dropwise to the solution and stirred for 1 h. The catalyst was centrifuged, washed and dried under vacuum at 60 °C for 12 h. Finally, the product was calcined at 200 °C for 2 h under a hydrogen atmosphere at a heating rate of 10 °C / min to obtain the final catalyst.
[0070] The performance of the catalysts prepared in Implementation Example 1 and Comparative Examples 1-3 was tested and discussed, and the results are as follows:
[0071] Test the optoelectronic properties of different materials. Fig.10 a shows the photocurrent response characteristics of the material, which well indicates the concentration of photogenerated carriers generated by the material under light irradiation and the transfer of photogenerated carriers on the surface of the material. In the test, the voltage was 0V and no bias voltage was applied. Compared with single MOF-74 and C3N4, the photocurrent of MOF / C3N4 formed after the composite is slightly improved. This is also because the transfer of electrons and holes on the band after the compound semiconductor material reduces the recombination of photogenerated carriers. When the Ru single atom material Ru / MOF / C3N4 was formed, its photocurrent intensity was observed to be about three times higher than that of MOF / C3N4, indicating that the introduction of Ru single core can effectively reduce the recombination of photogenerated carriers and increase carrier mobility. The addition of EIS also confirmed this result. As Fig.10 As shown in b, Ru / MOF / C3N4 has the smallest radius, which means it has the smallest surface resistance. Having a small surface resistance makes it easier for charges to transfer on the surface of the material. Steady-state PL spectrum ( Fig.11a) shows that Ru / MOF / C3N4 and MOF / C3N4 emit fluorescence at 470 nm. Compared with MOF / C3N4, Ru / MOF / C3N4 exhibits significant fluorescence quenching, which also indicates that Ru / MOF / C3N4 inhibits the recombination of electrons and holes, thus reducing the fluorescence intensity. However, the fluorescence intensity of MOF-74 is very weak because its photogenerated carrier capacity is weak, which is also obvious from the characterization of the lowest photocurrent. Fig.11 The transient fluorescence spectra in b show the average fluorescence lifetimes of different catalysts. The average PL lifetimes of Ru / MOF / C3N4, MOF / C3N4, and MOF are 35.8, 28.1, and 3.3 ns, respectively. The fluorescence lifetime is the time it takes for an electron to return from an excited state to the ground state after the excitation light is removed. The longer the fluorescence lifetime, the longer it takes for an electron to return from an excited state to the ground state, which means it takes longer to recombine with a hole. Therefore, a longer fluorescence lifetime also means that the recombination rate of photocarriers in the material is slower. This is also consistent with the photocurrent results.
[0072] The photocatalytic activities of different materials in CO2RR, NRR and hydrogen evolution reaction (HER) were studied. The products of photocatalytic reduction of CO2RR include CO and CH4. Fig.12 a It can be seen that the activity of Ru / MOF / C3N4 is significantly higher than that of other catalysts. In the absence of sacrificial agent, the activity of Ru / MOF / C3N4 reaches 11.8 μmol·g at 8 hours. -1 , which is about twice that of MOF / C3N4 and three times that of C3N4 and MOF-74. Especially in the first hour, the yield reached 5.7 μmol·g -1 , significantly higher than several other catalysts. CH4 is a more valuable reduction product than the product CO. CH4 has a higher calorific value and is non-toxic, but its catalytic production is also more difficult than CO. Eight electrons are required to complete the reaction, which requires strong reducing power and sufficient electrons from the photocatalyst. At 8 hours, the activity of MOF / C3N4 was 7.3 μmol·g -1 , about 4 times that of MOF / C3N4 ( Fig.12 b). The activity of single C3N4 or MOF-74 is negligibly low. In addition, in photocatalytic NRR, Ru / MOF / C3N4 still exhibits excellent catalytic activity, reaching 8.1 m mol·g in 1 h. -1 ,like Fig.12 As the detection of ammonia nitrogen is easily inaccurate due to other factors, we also measured the product by an ammonium ion composite electrode (ray magnetic ion meter PXSJ-270F) as another double check method and obtained 8 mmol·g in 1 hour. -1The yield of ammonia nitrogen also shows the accuracy of the ammonia nitrogen yield. Its activity is about 3 times that of MOF / C3N4 and about 6 times that of C3N4, while pure MOF-74 material has no nitrogen fixation activity.
[0073] The HER activity of different materials is studied. After H2O is decomposed into active hydrogen under photocatalysis, the active hydrogen is more likely to combine with each other to generate H2, thereby reducing the amount of active hydrogen. And the generated H2 tends to adhere to the catalyst surface, hindering the contact between the catalyst and the reactants and hindering the reaction. Fig.12 d, it can be seen that compared with MOF / C3N4, Ru / MOF / C3N4 can effectively reduce the generation of H2. At 4 hours, the hydrogen generation of Ru / MOF / C3N4 is only about 1 / 3 of that of MOF / C3N4, which is more conducive to increasing the concentration of active hydrogen and thus promoting the catalytic activity of the catalyst. Although many researchers have conducted extensive research on MOF and C3N4 materials for photocatalytic CO2RR, the carbon source of the product has been proven. We compared the catalysts under CO2 and Ar gases, such as Fig.13 As shown, no product was detected under Ar atmosphere, indicating that the product came from CO2, not the carbon in MOF or C3N4. Due to different test conditions, the yield cannot represent the catalytic level of catalysts in the same field. Therefore, we tested the apparent quantum yield (AQY) of the catalyst at different wavelengths ( Fig.14 a). At a wavelength of 365 nm, when the product is CO, the AQY is 7.8%, and when the product is CH4, the AQY is 2.1%. At 420 nm, when the product is CO, the AQY is 7.7%, and when the product is CH4, the AQY is 1.9%. The CH4 product of a single Au atom on an ultrathin ZnIn2S4 nanosheet catalyst published by Li Song, Hefeng Cheng et al. in 2022 had an AQY of 0.12% at 450 nm. It can be seen that the AQY of Ru / MOF / C3N4 in this work is significantly higher than that of other catalysts. We also tested the cyclic activity of the Ru / MOF / C3N4 catalyst and found that the activity of the catalyst was basically stable, which also shows that the catalyst has excellent stability ( Fig.14 b, c, d).
[0074] To further understand the role of Ru single atom loading, we investigated two models (MOF-74, Ru / MOF-74) in three pathways of CO2RR and NRR (alternating hydrogenation and remote hydrogenation) ( Fig.15) performed theoretical calculations of the Gibbs free energy. The reason for the two pathways of NRR is that there are two widely accepted mechanisms for the conversion of N2 to NH3. These are generally referred to as the distal mechanism and the alternating mechanism. We also calculated the Gibbs free energy of each intermediate for different models of the different reaction pathways. As can be seen from the figure, in both the CO2RR and NRR systems, Ru / MOF-74 greatly reduces the Gibbs free energy during the reaction ( Fig.16 a, b, c). This indicates that single-atom Ru plays a key role in lowering the free energy of the reaction and promoting the reaction.
[0075] To further analyze the electron transfer mechanism of Ru / MOF / C3N4 catalyst, we calculated the band gaps of C3N4 and MOF-74 by UV-Vis spectroscopy. Fig.17 As shown, when the two materials C3N4 and MOF-74 are excited by light, electrons jump from the valence band to their respective conduction bands. Since the conduction band of C3N4 is higher than that of MOF-74, electrons from the conduction band of C3N4 will be transferred to the conduction band of MOF-74. The valence band position of MOF-74 is lower than that of C3N4, so the holes on MOF-74 will be transferred to the valence band of C3N4, thereby forming a separation of electrons and holes in space and effectively reducing the recombination of photogenerated carriers. Due to the presence of Ru single atoms in MOF-74, a doping level is formed, so the electrons in the conduction band of MOF-74 will be transferred to the doping level, which further reduces the recombination of electrons and holes and increases the concentration of photogenerated carriers. As an active site, Ru receives electrons when it comes into contact with the reactants.
[0076] In summary, the present invention prepares a Ru single atom catalyst Ru / MOF / C3N4 anchored on MOF on C3N4. It has excellent catalytic activity for both CO2RR and NRR, with a CO yield that is three times that of C3N4, a CH4 yield that is four times that of MOF / C3N4, and a NH3 yield that is three times that of MOF / C3N4 and C3N4. The Ru / MOF / C3N4 catalyst has high photocurrent, low surface resistance, and effective suppression of photogenerated carrier recombination. Through theoretical calculations, it is found that the 4d orbital of Ru can form a doping energy level and promote electron transfer. At the same time, the introduction of Ru can significantly reduce the Gibbs free energy during the CO2RR and NRR reactions. Finally, we analyzed the electron transfer process of the Ru / MOF / C3N4 catalyst under light and the active sites involved in the reaction. These results have important guidance and significance for the synthesis of single-atom catalytic materials with high photocatalytic CO2RR and NRR activity.
[0077] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing Ru single atom-loaded MOF / C3N4, characterized in that: The following steps are involved: Step 1, dissolving 2,5-dihydroxyterephthalic acid and Zn(NO3)2·6H2O in DMF solvent, slowly adding deionized water and stirring until completely mixed to obtain a mixed solution; Step 2, adding C3N4 to the mixed solution and stirring, and adding RuCl3 dropwise during the stirring process; wherein the stirring time is 11-13h; Step 3, diluting triethylamine with DMF solvent, and adding the diluted solution dropwise to the product obtained in step 2, stirring, centrifuging, washing, and drying; Step 4: calcine the dried product under a hydrogen atmosphere to obtain Ru single atom-loaded MOF / C3N4.
2. The method for preparing Ru single atom-loaded MOF / C3N4 according to claim 1, characterized in that: The mass ratio of 2,5-dihydroxyterephthalic acid, Zn(NO3)2·6H2O and C3N4 is 1:4.5:20-50; And / or, in step 2, the RuCl3 is specifically 1-5 mL of RuCl3 with a concentration of 10 mg / mL.
3. The method for preparing Ru single atom-loaded MOF / C3N4 according to claim 2, characterized in that: The specific preparation steps of the C3N4 are as follows: S1. Add melamine and phosphite to deionized water, stir evenly, react at 170-180°C for 9-10h, wash and dry to obtain a precursor; S2. Mix the precursor, glycerol and ethanol, reflux at 90-100° C. for 3-4 hours, wash and dry to obtain a solid product, and then calcine and sonicate the solid product to obtain C3N4.
4. The method for preparing Ru single atom-loaded MOF / C3N4 according to claim 3, characterized in that: In S1, the mass ratio of melamine to phosphite is 1:1.2; And / or, in S2, the mass volume ratio of the precursor, glycerol and ethanol is 0.6g:5mL:15mL.
5. The method for preparing Ru single atom-loaded MOF / C3N4 according to claim 3, characterized in that: In S1, the stirring is specifically stirring in a water bath at 80-90° C. for 1-2 h; and / or, in S2, the calcination is specifically calcined at 500° C. for 2 h at a heating rate of 2° C. / min; And / or, in S2, the ultrasonic treatment is specifically ethanol ultrasonic treatment for 9-10 hours.
6. The method for preparing Ru single atom-loaded MOF / C3N4 according to claim 1, characterized in that: In step 1, the volume ratio of the DMF solvent to deionized water is 10:1; And / or, in step 3, the volume ratio of the DMF solvent to triethylamine is 5:
1.
7. The method for preparing Ru single atom-loaded MOF / C3N4 according to claim 1, characterized in that: In step 4, the specific conditions of the calcination are calcination at 200° C. for 2 h at a heating rate of 10° C. / min.
8. The method for preparing Ru single atom-loaded MOF / C3N4 according to any one of claims 1 to 7, characterized in that: In step 3, the stirring time is 1-2h; And / or, in step three, the drying is specifically drying under vacuum at 50-60° C. for 11-13 h.
9. Use of Ru single atom-loaded MOF / C3N4 prepared by the method according to any one of claims 1 to 8 in photocatalytic carbon dioxide reduction.
10. Use of Ru single atom-loaded MOF / C3N4 prepared by the method according to any one of claims 1 to 8 in photocatalytic nitrogen fixation.