A 1000MPa grade easy-to-weld extra-thick hydropower steel and a manufacturing method thereof

Through low-carbon, Ni+Mo+Nb+B component systems and specific production processes, the existing 1000MPa-grade hydropower steel plates are solved, and 1000MPa-grade easy-to-weld extra-thick hydropower steel with high strength and excellent welding performance is achieved. The manufacturing of the company meets the high performance needs of large hydropower stations.

CN116254471BActive Publication Date: 2024-12-06ANGANG STEEL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202310167172.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-12-06
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

The overall strength of the existing 1000MPa grade hydroelectric steel plate is low, the yield strength and tensile strength are insufficient, and the production process is complex, making it difficult to meet the needs of high performance and high thickness.

Method used

Using low-carbon, Ni+Mo+Nb+B component system, combined with converter smelting, outside furnace refining, mold casting, recrystallization zone + unrecrystallization zone rolling and offline tempering heat treatment technology, Ceq and Pcm are controlled, and a unique design is designed. Production process to improve the strength and welding performance of steel plates.

Benefits of technology

The room temperature tensile strength of the steel plate is achieved to reach 980MPa, the yield strength reaches 900MPa, the elongation after break is ≥20%, the impact absorption energy of -40℃ is ≥200J, and it has excellent low-temperature toughness and easy welding, which meets the 1000MPa of large hydropower stations. Use requirements for grade easy welding of extra-thick hydropower steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116254471B_ABST
    Figure CN116254471B_ABST
Patent Text Reader

Abstract

The present invention relates to a 1000MPa grade easy-to-weld extra-thick hydroelectric steel and a manufacturing method thereof. The chemical components of the steel are C: 0.08%-0.12%; Si: 0.05%-0.09%; Mn: 0.50%-0.80%; P≤0.008%; S≤0.001%; ​​Ni: 1.35%-1.75%; Mo: 0.71%-0.95%; Nb: 0.05%-0.08%; B: 0 .0035%~0.005%; Ca: 0.001%~0.004%; Al: 0.03%~0.07%; [H]≤1.5ppm; [O]≤8ppm; 1<Mo / Mn<2; the balance is Fe and impurities; The present invention adopts low carbon, Ni+Mo+Nb+B component system, controls Ceq and Pcm at the same time, and cooperates with a unique production process to ensure that the steel plate has high strength and toughness and good welding performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of 1000MPa grade steel plate manufacturing, and in particular to a 1000MPa grade easy-to-weld extra-thick hydropower steel and a manufacturing method thereof. Background Art

[0002] In recent years, the goals of carbon peak and carbon neutrality have been proposed, which has further developed the use of clean energy. As one of the clean energy sources, hydropower does not produce any carbon emissions or pollution and is renewable, so it has become a top priority in the development of clean energy. The large-scale construction of hydropower projects has led to the widespread use of 800MPa hydropower steel, and at the same time, there is a demand for 1000MPa steel plates.

[0003] Hydropower steel requires excellent toughness, weldability, cold formability and other properties. For 1000MPa hydropower steel, the requirements for various properties are more stringent. Due to the difficulty in producing 1000MPa high-strength hydropower steel, only a very small number of steel mills at home and abroad are able to produce it.

[0004] The Chinese invention patent with authorization announcement number CN102653846B discloses "a thick, easy-to-weld, tempered, high-strength steel plate for hydropower and its production method". The steel plate is composed of the following chemical components in weight percentage: C: 0.15% to 0.18%, Si: 0.15% to 0.35%, Mn: 0.90% to 1.00%, P≤0.012%, S≤0.005%, Ni: 1.52% to 1.60%, Cr: 0.30% to 0.40%, Nb: 0.020% to 0.030%, Al: 0.020% to 0.050%, Mo: 0.20% to 0.30%, V: 0.055% to 0.065%, B: 0.0007% to 0.0015%, Ti: 0.015% to 0.025%, and the balance is Fe and unavoidable impurities. The production method of the steel plate includes the following steps: electric furnace smelting → LF / VD refining → die casting → ingot heating → rolling → water cooling after rolling → hot stacking → heat treatment → finished product. The maximum thickness of the hydropower large-thickness easy-to-weld quenched and tempered high-strength steel plate can reach 230mm, and it has the characteristics of good welding performance, low yield strength ratio, excellent low-temperature impact toughness and good thickness direction performance, but its overall strength is low, the yield strength is only above 440MPa, and the tensile strength is only between 540MPa and 720MPa.

[0005] The Chinese patent application with publication number CN108504960A discloses "a 1000MPa grade low crack hydropower steel plate for large hydropower projects and its production method". The steel plate has a thickness of 10 to 50 mm and includes the following chemical components in mass percentage: C: 0.06 to 0.17%, Si: ≤0.15%, Mn: 0.8 to 2.0%, P: ≤0.010%, S: ≤0.003%, Ni: 1.0 to 2.0%, Cu: 0.10 to 0.25%, Cr: 0.3 to 1.5%, Mo: 0.4 to 0.7%, V+Nb+Ti: ≤0.1%, Als: 0.015 to 0.045%, Ce≤0.020%, CEV≤0.64%, Pcm≤0.28%, and the rest are Fe and residual elements. The steel plate composition is designed with low C, high Ni (1.0-2.0%) + Cr + Mo composition, and is produced using die casting + blanking + reheating controlled rolling and controlled cooling + offline tempering process. Ceq≤0.64%, Pcm≤0.28% are both relatively high, and the production process is complicated.

[0006] The Chinese patent application with publication number CN114058960A discloses "a 25-60 mm thick 1000 MPa grade high-strength, high-toughness and easy-to-weld nano steel and its preparation method". According to the mass percentage of alloy elements, C: 0.03-0.08, Si: 0.2-0.4, Mn: 0.7-1.1, P≤0.01, S≤0.0015, Cu: 1.5-2.5, Ni: 6.0-8.0, Cr: 0.5-0.8, Mo: 0.45-0.6, Nb: 0.02-0.1, Ti: 0.01-0.05, Al: 0.005-0.05, and the balance is Fe and inevitable impurities, including the following steps: smelting and refining - mold casting or continuous casting - rolling - heat treatment. The yield strength of the nano steel is ≥1000MPa, the Charpy V-notch impact energy at -84°C at 1 / 4 and 1 / 2 thickness of the steel plate is ≥200J, and the elongation is ≥15%. The steel plate contains high Cu (1.5-2.5%), high Ni (6-8%) components, a carbon equivalent of more than 0.65%, and a high alloy cost.

[0007] Publication No. CN104532157A discloses “a quenched and tempered high-strength steel with a yield strength of 900-1000 MPa and a production method thereof”, and its chemical composition by weight is: C 0.16-0.20%, Si 0.10-0.30%, Mn 0.80-1.60%, Cr 0.20-0.70%, Mo 0.10-0.45%, Ni 0.10-0.50%, Nb 0.010-0.030%, Ti 0.010-0.030%, V 0.010-0.050%, B 0.0005-0.0005% .0030%, Al0.02~0.06%, Ca0.001~0.004%, N0.002~0.005%, P≤0.020%, S≤0.010%, O≤0.008%, the rest are Fe and unavoidable impurities, and: Ceq0.51~0.60%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15; 3.7≤Ti / N≤7.0; 1.0≤Ca / S≤3.0; 0.8%≤Mo+0.8Ni+0.4Cr+6V≤1.3%. It adopts controlled rolling and controlled cooling and offline quenching + tempering process, and the steel plate produced has a yield strength of 900~1080MPa, a tensile strength of 950~1200MPa, an elongation>10%, and an impact energy>40J at -40℃. However, the steel plate adopts a relatively high C (0.16-0.2%), a Ni+Cr+Mo+B composition system, and adds trace elements Nb, V, Ti, and N. The elongation of the steel plate after fracture is less than 15%, and the impact absorption energy at -40°C is less than 120J.

[0008] It can be seen that the existing technologies generally have problems such as high carbon equivalent and insufficient performance. Summary of the invention

[0009] The present invention provides a 1000MPa grade easy-to-weld extra-thick hydropower steel and a manufacturing method thereof, which adopts a low-carbon, Ni+Mo+Nb+B component system, controls Ceq and Pcm at the same time, and cooperates with a unique production process to ensure that the steel plate has high strength and toughness while also having good welding performance.

[0010] In order to achieve the above object, the present invention adopts the following technical solutions:

[0011] A 1000MPa grade easy-to-weld extra-thick hydroelectric steel, the chemical composition of which is as follows by weight: C: 0.08%-0.12%; Si: 0.05%-0.09%; Mn: 0.50%-0.80%; P≤0.008%; S≤0.001%; ​​Ni: 1.35%-1.75%; Mo: 0.71%-0.95%; Nb: 0.05%-0.08%; B: 0.0035%-0.005%; Ca: 0.001%-0.004%; Al: 0. 03%~0.07%; [H]≤1.5ppm; [O]≤8ppm; 1<Mo / Mn<2; the balance is Fe and unavoidable impurities; in addition: carbon equivalent Ceq<0.50%, and Ceq=C+Mn / 6+Si / 24+Ni / 40+Cr / 5+Mo / 4+V / 14; welding crack sensitivity coefficient Pcm≤0.25%, and Pcm=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B.

[0012] Furthermore, the room temperature tensile strength of the finished steel plate is ≥980MPa, the yield strength is ≥900MPa, the elongation after fracture is ≥20%; the impact absorption energy at -40°C is ≥200J, the tensile section shrinkage in Z direction is >60%, the non-ductile transition temperature TNDT is ≤-50°C, and the impact absorption energy at -40°C of the welded joint under the welding heat input of 10 to 100kJ / cm is ≥150J.

[0013] A method for manufacturing 1000MPa grade easy-to-weld extra-thick hydropower steel comprises the following steps:

[0014] 1) Smelting: The converter smelting + refining outside the furnace is adopted. During the refining outside the furnace, the molten steel is treated with calcium to make the non-metallic inclusions in the steel ≤0.5 level;

[0015] 2) Casting; during the casting process, the tundish superheat is controlled at 15-25°C, and the billet pulling speed is 1.3-1.6 m / min; the secondary cooling water adopts the air-water spray method, and the cooling rate is 100-150°C / m; the electromagnetic stirring method is adopted at the end of solidification, and the electromagnetic stirring current is 300-350A and the frequency is 4-6Hz;

[0016] 3) Stacking and slow cooling: After the continuous casting billet is off the line, the stacking and slow cooling are more than 40 hours, and the center segregation rating of the billet is ≤0.5;

[0017] 4) Heating: The continuous casting billet is heated in a heating furnace, the soaking section temperature is 1170-1210°C, and the soaking time is 2.5-3.5h;

[0018] 5) Rolling; two-stage controlled rolling is adopted; the first stage is rolling in the recrystallization zone, the starting rolling temperature is 1120-1150°C, the pass reduction rate is 10%-25%; the final rolling temperature is 990-1020°C; the intermediate billet is water-cooled to 860-880°C, the second stage is rolling in the non-recrystallization zone, the total reduction rate is greater than 60%, and the final rolling temperature is controlled at 710-740°C;

[0019] 6) Heat treatment after rolling: adopt offline quenching and tempering heat treatment method, the quenching and holding temperature is 850-890℃, the holding time is 2-5min / mm, the tempering and holding temperature is 570-620℃, and the holding time is 2-6min / mm.

[0020] Furthermore, the thickness of the continuous casting billet is 300-450 mm, the thickness of the intermediate billet is 2-3 times the thickness of the finished steel plate, and the thickness of the finished steel plate is 70-110 mm.

[0021] Furthermore, the continuous casting ingot is descaled by high pressure water after it leaves the furnace.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1) Adopt low carbon, Ni+Mo+Nb+B composition system design, and control 1<Mo / Mn<2, Ceq<0.5%, Pcm≤0.25% at the same time, to provide alloy composition guarantee for steel plate with high strength and toughness and good welding performance;

[0024] 2) The converter + refining outside the furnace is used to control P≤0.008%, S≤0.001%, [H]≤1.5ppm, [O]≤8ppm in the steel, and appropriate calcium treatment process is used to improve the purity of the steel and reduce the non-metallic inclusions in the steel. The non-metallic inclusion rating coarseness is ≤0.5 level;

[0025] 3) According to the design characteristics of the alloy composition in the steel, the recrystallization zone + non-recrystallization zone controlled rolling method is adopted. Through multi-pass high-penetration deformation and micro-alloy strengthening mechanism, the core structure and performance of the extra-thick plate are effectively improved, and the lamellar tearing resistance of the steel plate is improved;

[0026] 4) Through the design of low-carbon, Ni+Mo+Nb+B composition system, combined with controlled rolling + offline quenching and tempering heat treatment process, the production of hydropower steel with a thickness of 70-110mm, a tensile strength of 1000MPa and easy welding is achieved. The steel plate has excellent strength, toughness and welding performance;

[0027] 5) The room temperature tensile strength of the steel plate is ≥980MPa, the yield strength is ≥900MPa, and the elongation after fracture is ≥20%; the impact absorption energy at -40℃ is ≥200J, the tensile section shrinkage in Z direction is >60%, the non-ductile transition temperature TNDT is ≤-50℃, and the impact absorption energy of the welded joint at -40℃ under the welding heat input of 10-100kJ / cm is ≥150J. It has excellent low-temperature toughness and easy weldability, and can fully meet the use requirements of large hydropower stations for 1000MPa grade easy-to-weld extra-thick hydropower steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a typical metallographic structure photograph of the 1000MPa grade easy-to-weld extra-thick hydropower steel described in the present invention. DETAILED DESCRIPTION

[0029] The 1000MPa grade easy-to-weld extra-thick hydropower steel disclosed by the present invention has the following chemical components by weight: C: 0.08%-0.12%; Si: 0.05%-0.09%; Mn: 0.50%-0.80%; P≤0.008%; S≤0.001%; ​​Ni: 1.35%-1.75%; Mo: 0.71%-0.95%; Nb: 0.05%-0.08%; B: 0.0035%-0.005%; Ca: 0.001%-0.004%; Al: 0.03%~0.07%; [H]≤1.5ppm; [O]≤8ppm; 1<Mo / Mn<2; the balance is Fe and unavoidable impurities; in addition: carbon equivalent Ceq<0.50%, and Ceq=C+Mn / 6+Si / 24+Ni / 40+Cr / 5+Mo / 4+V / 14; welding crack sensitivity coefficient Pcm≤0.25%, and Pcm=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B.

[0030] Furthermore, the room temperature tensile strength of the finished steel plate is ≥980MPa, the yield strength is ≥900MPa, the elongation after fracture is ≥20%; the impact absorption energy at -40°C is ≥200J, the tensile section shrinkage in Z direction is >60%, the non-ductile transition temperature TNDT is ≤-50°C, and the impact absorption energy at -40°C of the welded joint under the welding heat input of 10 to 100kJ / cm is ≥150J.

[0031] The method for manufacturing a 1000MPa grade easy-to-weld extra-thick hydropower steel of the present invention comprises the following steps:

[0032] 1) Smelting: The converter smelting + refining outside the furnace is adopted. During the refining outside the furnace, the molten steel is treated with calcium to make the non-metallic inclusions in the steel ≤0.5 level;

[0033] 2) Casting; during the casting process, the tundish superheat is controlled at 15-25°C, and the billet pulling speed is 1.3-1.6 m / min; the secondary cooling water adopts the air-water spray method, and the cooling rate is 100-150°C / m; the electromagnetic stirring method is adopted at the end of solidification, and the electromagnetic stirring current is 300-350A and the frequency is 4-6Hz;

[0034] 3) Stacking and slow cooling: After the continuous casting billet is off the line, the stacking and slow cooling are more than 40 hours, and the center segregation rating of the billet is ≤0.5;

[0035] 4) Heating: The continuous casting billet is heated in a heating furnace, the soaking section temperature is 1170-1210°C, and the soaking time is 2.5-3.5h;

[0036] 5) Rolling; two-stage controlled rolling is adopted; the first stage is rolling in the recrystallization zone, the starting rolling temperature is 1120-1150°C, the pass reduction rate is 10%-25%; the final rolling temperature is 990-1020°C; the intermediate billet is water-cooled to 860-880°C, the second stage is rolling in the non-recrystallization zone, the total reduction rate is greater than 60%, and the final rolling temperature is controlled at 710-740°C;

[0037] 6) Heat treatment after rolling: adopt offline quenching and tempering heat treatment method, the quenching and holding temperature is 850-890℃, the holding time is 2-5min / mm, the tempering and holding temperature is 570-620℃, and the holding time is 2-6min / mm.

[0038] Furthermore, the thickness of the continuous casting billet is 300-450 mm, the thickness of the intermediate billet is 2-3 times the thickness of the finished steel plate, and the thickness of the finished steel plate is 70-110 mm.

[0039] Furthermore, the continuous casting ingot is descaled by high pressure water after it leaves the furnace.

[0040] The reasons for designing the chemical composition of the 1000MPa grade easy-to-weld extra-thick hydropower steel described in the present invention are as follows:

[0041] (1) C: It has a solid solution strengthening effect and can form fine carbides with Nb and Mo, thereby playing an effective precipitation strengthening role during heating, rolling deformation and heat treatment. However, the increase in carbon content is not conducive to the welding performance of steel, so the C content in the present invention is controlled to 0.08% to 0.12%.

[0042] (2) Si: It plays a role in solid solution strengthening and can improve the hardenability and tempering resistance of steel. However, too high Si content will reduce the welding performance of steel, so the Si content in the steel of the present invention is controlled to 0.05% to 0.09%.

[0043] (3) Mn: It can improve the hardenability of steel and has the effect of solid solution strengthening. More importantly, the present invention uses Mn in combination with Mo and controls 1<Mo / Mn<2 to inhibit the formation of alloy infiltration during long-term tempering, improve the toughness of the steel plate after heat treatment, and improve the welding performance of the steel plate. However, an increase in manganese content will reduce the welding performance of steel. Therefore, the present invention controls the Mn content in the steel to be 0.50% to 0.80%.

[0044] (4) P and S: Both are harmful elements. P damages the low-temperature toughness of the steel plate, and S easily forms sulfide inclusions in the steel, which reduces the impact toughness of the steel and impairs the welding performance. Therefore, the lower the content of both, the better. The present invention controls P≤0.008% and S≤0.001% in the steel.

[0045] (5) Ni: used to expand the austenite zone, facilitate the effective implementation of the controlled rolling process of the present invention; reduce the near-transformation temperature and improve the low-temperature toughness of the steel plate; strengthen the ferrite, refine the controlled cooling structure; and improve the hardenability of the steel plate. However, an increase in the nickel content is not conducive to improving the welding performance, so the present invention controls the Ni content to 1.35% to 1.75%.

[0046] (6) Mo: The main functions of the present invention are: 1) to play a certain role in solid solution strengthening; 2) to improve the hardenability of steel; 3) to improve the stability of carbides, thereby improving the strength of steel; 4) by using it in combination with Mn and controlling 1<Mo / Mn<2, it can inhibit the formation of alloy infiltration during long-term tempering, improve the toughness of the steel plate after heat treatment, and improve the welding performance of the steel plate. Considering the influence of molybdenum on welding performance, the present invention controls the Mo content to 0.71% to 0.95%.

[0047] (7) Nb: The main functions of Nb in the steel of the present invention are as follows: 1) when the steel billet is heated, it prevents the austenite grains from growing and increases the grain coarsening temperature; 2) when rolling in the recrystallization zone, the niobium dissolved in the austenite can interact with the dislocations to prevent the migration of the grain boundaries and the coarsening of the recrystallized grains; 3) when rolling in the non-recrystallization zone, the fine niobium carbonitride precipitated by deformation can pin the austenite subgrains and promote the nucleation of ferrite, which plays a role in refining the grains; 4) it expands the range of the austenite non-recrystallization zone, which is beneficial to the implementation of the controlled rolling process; 5) it improves the hardenability of the steel; 6) it inhibits the formation of Fe(C, B)6, and ensures that the boron in the steel exists basically in the form of solid solution boron. For this reason, the present invention controls the Nb content in the steel to be 0.05% to 0.08%.

[0048] (8) B: used to improve the hardenability of steel and improve the strength of steel after controlled cooling and tempering. Too high a boron content will cause segregation and reduce the toughness of the steel. Therefore, the B content in the steel of the present invention is controlled to be 0.0035% to 0.005%.

[0049] (9) Ca: used to denature oxides and sulfides in the molten steel, improve the cleanliness of the molten steel, refine the grains, improve the toughness of the steel plate, and improve the lamellar tear resistance of the extra-thick plate of the present invention. However, too much Ca can easily form large-sized compounds and damage the toughness of the steel plate. Therefore, the present invention controls the Ca content in the steel to 0.001% to 0.004%.

[0050] (10) Al: It has a certain deoxidation effect and can form AlN, refine the grains, and improve the toughness of the steel plate. The Al content is controlled to be 0.03% to 0.07% in the present invention.

[0051] (11) H and O: H and O have adverse effects on the properties of the steel plate. The present invention controls [H]≤1.5ppm and [O]≤8ppm.

[0052] The present invention discloses a method for manufacturing 1000MPa grade easy-to-weld extra-thick hydropower steel. The design principle is as follows:

[0053] 1. The steel billet is smelted by converter + refining outside the furnace, and the P in the steel is controlled to be ≤0.008%, S ≤0.001%, [H] ≤1.5ppm, [O] ≤8ppm. The molten steel is treated with calcium in the refining process outside the furnace to denature the inclusions in the molten steel, improve the cleanliness of the steel, and make the non-metallic inclusions in the molten steel spherical, with a coarseness and fineness grade of no more than 0.5. At the same time, the fluidity of the molten steel is improved and the as-cast structure is improved.

[0054] 2. During the casting process, the superheat of the tundish is controlled at 15-25°C, the billet pulling speed is 1.3-1.6m / min, the secondary cooling water is air-water spray, and the cooling rate is 100-150°C / m to ensure that the temperature drop inside and outside the billet is balanced and there are no cracks. Electromagnetic stirring is used at the end of solidification, with an electromagnetic stirring current of 300-350A and a frequency of 4-6Hz to expand and refine the equiaxed crystal band, improve the distribution of inclusions, eliminate the billet shrinkage, and reduce center porosity and center segregation.

[0055] 3. After the continuous casting billet is off the production line, it is stacked and slowly cooled for more than 40 hours to further homogenize the as-cast structure, reduce the internal stress of the billet, reduce the segregation of the billet, and ensure that the segregation of the billet is ≤0.5. The thickness of the continuous casting billet is preferably 300-450mm.

[0056] 4. The continuous casting billet is heated in a heating furnace (preferably a step heating furnace) with a soaking section temperature of 1170-1210°C and a soaking time of 2.5-3.5 hours. Under this heating process, the billet is heated evenly, austenitized sufficiently, and has no coarsening tendency.

[0057] 5. After the ingot is taken out of the furnace, it is descaled by high-pressure water, and then two-stage controlled rolling is adopted. In the first stage, the recrystallization zone rolling, the start rolling temperature is 1120-1150℃, the pass reduction rate is 10-25%, and the interval time between rolling passes is minimized to prevent the growth of austenite grains. The thickness of the intermediate billet is 2-3 times the thickness of the finished steel plate, and the final rolling temperature is 990-1020℃. The intermediate billet is cooled to 860-880℃ by water, and the second stage of non-recrystallization zone rolling is carried out. The total reduction rate is greater than 60%, and the final rolling temperature is controlled at 710-740℃.

[0058] 6. After rolling, the steel plate is subjected to offline quenching and tempering heat treatment, wherein the quenching and holding temperature is 850-890℃, the holding time is 2-5min / mm, the tempering and holding temperature is 570-620℃, the holding time is 2-6min / mm. Reasonable quenching and tempering process ensures that the steel plate has excellent strength and toughness.

[0059] Typical metallographic structure photos of the 1000MPa grade easy-to-weld extra-thick hydroelectric steel described in the present invention are as follows: Figure 1 As shown, the structure of the steel is tempered troostite.

[0060] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0061] [Example]

[0062] The chemical composition of the steel in each embodiment is shown in Table 1, the continuous casting and heating process parameters of the steel in each embodiment are shown in Table 2, the rolling and heat treatment process parameters of the steel in each embodiment are shown in Table 3, and the mechanical properties of the finished steel plate in each embodiment are shown in Table 4.

[0063] Table 1 Chemical composition of steel (wt%)

[0064]

[0065]

[0066] Table 2 Continuous casting and heating process parameters of steel

[0067]

[0068] Table 3 Rolling and heat treatment process parameters of steel

[0069]

[0070]

[0071] Table 4 Mechanical properties of steel plates in quenched and tempered state

[0072]

[0073] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for manufacturing 1000MPa grade easy-to-weld extra-thick hydropower steel, characterized in that: The chemical composition of the steel is calculated by weight as follows: C: 0.08% ~ 0.12%; Si: 0.05% ~ 0.09%; Mn: 0.50% ~ 0.80%; P ≤ 0.008%; S ≤ 0.001%; ​​Ni: 1.35% ~ 1.75%; Mo: 0.71% ~ 0.95%; Nb: 0.05% ~ 0.08%; B: 0.0035% ~ 0.005%; Ca: 0.001% ~ 0.004%; Al: 0.03% ~ 0.07%; [H] ≤ 1.5ppm; [O] ≤ 8ppm; 1 < Mo / Mn < 2; the balance is Fe and unavoidable impurities; in addition, the carbon equivalent Ceq < 0.50%, and Ceq = C + Mn / 6 + Si / 24 + Ni / 40 + Cr / 5 + Mo / 4+ V / 14; welding crack sensitivity coefficient Pcm≤0.25%, and Pcm= C+ Si / 30+ Mn / 20+ Cu / 20+ Ni / 60+ Cr / 20+Mo / 15+ V / 10+ 5B; The method for manufacturing the 1000MPa grade easy-to-weld extra-thick hydropower steel comprises the following steps: 1) Smelting: The converter smelting + refining outside the furnace is adopted. During the refining outside the furnace, the molten steel is treated with calcium to make the non-metallic inclusions in the steel ≤0.5 level; 2) Casting; During the casting process, the tundish superheat is controlled at 15-25°C, and the billet pulling speed is 1.3-1.6 m / min; the secondary cooling water adopts the air-water spray method, and the cooling rate is 100-150°C / m; the electromagnetic stirring method is adopted at the end of solidification, and the electromagnetic stirring current is 300-350A, and the frequency is 4-6Hz; 3) Stacking and slow cooling: After the continuous casting billet is off the line, the stacking and slow cooling are more than 40 hours, and the center segregation rating of the billet is ≤0.5; 4) Heating: The continuous casting billet is heated in a heating furnace, the soaking section temperature is 1170-1210°C, and the soaking time is 2.5-3.5h; 5) Rolling; two-stage controlled rolling is adopted; the first stage is rolling in the recrystallization zone, the starting rolling temperature is 1120-1150℃, and the pass reduction rate is 10%-25%; the final rolling temperature is 990-1020℃; the intermediate billet is water-cooled to 860-880℃, and the second stage is rolling in the non-recrystallization zone, the total reduction rate is greater than 60%, and the final rolling temperature is controlled at 710-740℃; 6) Heat treatment after rolling: adopt offline quenching and tempering heat treatment method, the quenching and holding temperature is 850-890℃, the holding time is 2-5min / mm, the tempering and holding temperature is 570-620℃, and the holding time is 2-6min / mm.

2. The method for manufacturing a 1000MPa grade easy-to-weld extra-thick hydropower steel according to claim 1, characterized in that: The room temperature tensile strength of the finished steel plate is ≥980MPa, the yield strength is ≥900MPa, and the elongation after fracture is ≥20%; the impact absorption energy at -40℃ is ≥200J, the tensile section shrinkage in Z direction is >60%, the non-ductile transition temperature TNDT is ≤-50℃, and the impact absorption energy at -40℃ of the welded joint under the welding heat input of 10~100kJ / cm is ≥150J.

3. The method for manufacturing a 1000MPa grade easy-to-weld extra-thick hydropower steel according to claim 1, characterized in that: The thickness of the continuous casting billet is 300-450 mm, the thickness of the intermediate billet is 2-3 times the thickness of the finished steel plate, and the thickness of the finished steel plate is 70-110 mm.

4. The method for manufacturing a 1000MPa grade easy-to-weld extra-thick hydropower steel according to claim 1, characterized in that: After the continuous casting billet comes out of the furnace, high-pressure water is used to descale it.

Citation Information

Patent Citations

  • Large-thickness easy-to-weld quenched and tempered high-strength steel plate for hydroelectricity and manufacturing method thereof

    CN102653846B

  • 900MPa-1000MPa grade (yield strength) quenched-tempered high-strength steel and production method thereof

    CN104532157A

  • 1000MPa grade low-crack hydroelectric steel plate for large-scale hydropower engineering and production method thereof

    CN108504960A

  • 1000 MPa-grade high-strength high-toughness easy-to-weld nano steel with thickness of 25-60 mm and preparation method thereof

    CN114058960A

  • Large-thickness easy-to-weld quenched and tempered high-strength steel plate for hydroelectricity and manufacturing method thereof

    CN102653846A