Internal electrode alloy layer and preparation method thereof
The palladium-amalgam layer is formed on the surface of the ceramic dielectric sheet through the liquid phase reduction method, which solves the problems of high cost and high-temperature sintering of traditional MLCC internal electrode materials, and achieves excellent performance and improved safety of MLCC.
Patent Information
- Application Number
- CN202310158680.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-20
AI Technical Summary
The cost of traditional MLCC internal electrode materials is high, and problems such as voids and sintering cracks in the ceramic dielectric are prone to occur during the high-temperature sintering process, leading to accidents such as capacitor leakage or explosion.
Palladium salt and mercury iodide are used to react in a solvent, and an internal electrode alloy layer is formed on the surface of the ceramic dielectric sheet through a liquid phase reduction method. The process temperature is 100 to 500°C, and the attached substances are removed by baking to form a dense palladium- Amalgam layer.
It achieves low-cost, mild-environment preparation of the internal electrode alloy layer, avoids high-temperature sintering steps, improves the performance and safety of MLCC, and reduces the amount of precious metal palladium.
Smart Images

Figure CN116254525B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of preparation of internal electrode materials of MLCC, and specifically relates to an internal electrode alloy layer and a preparation method thereof. Background Art
[0002] MLCC (Multi-layer Ceramic Capacitor) refers to multilayer ceramic capacitors, which are one of the most widely used basic electronic components. It has wide application value in new energy vehicles and electric energy storage. The rapid development of new energy vehicles and energy storage power stations has also driven the growing demand for MLCC.
[0003] The internal structure of MLCC can be divided into three parts: ceramic dielectric body, inner electrode and outer electrode. Specifically, MLCC is made of ceramic dielectric sheets with printed electrodes (inner electrodes) stacked in a staggered manner, sintered at high temperature once to form a ceramic chip, and then sealed with a metal layer (outer electrode) at both ends of the chip to form a monolithic structure, also known as a "monolithic capacitor".
[0004] The traditional MLCC internal electrode material is palladium / silver alloy or pure metal palladium. The cost of this electrode material is very high. Using base metals to replace precious metals has become a trend in the industry. At present, most of the products in precious metal MLCC have been replaced by cheaper base metal products, but there are still some products that use base metal materials and cannot meet certain performance requirements. However, there is still a demand to reduce the material cost of such precious metal products.
[0005] The internal electrode materials, organic carriers and inorganic additives of precious metal MLCC are printed, solidified and sintered at high temperature to form an internal electrode layer on the surface of the ceramic dielectric layer. The temperature of this process is very high (generally in the range of 900-1300°C), and it is easy for voids and sintering cracks to appear in the ceramic dielectric, causing the capacitor to leak and fail, and even cause accidents such as cracking and explosion. Summary of the invention
[0006] In view of the deficiencies in the prior art, an object of the present invention is to provide an inner electrode alloy layer and a preparation method thereof. The preparation process of the inner electrode alloy layer provided by the present invention is simple and low in cost.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] The first object of the present invention is to provide a method for preparing an inner electrode alloy layer, comprising the following steps:
[0009] Palladium salt and mercuric iodide are dispersed in a solvent to obtain a mixed solution, a ceramic dielectric sheet is placed in the mixed solution, the mixed solution is heated to 100-180°C and a reducing agent is added, and an inner electrode alloy layer is formed on the surface of the ceramic dielectric sheet as the reaction proceeds, and after the mixed solution turns black and then yellow, the ceramic dielectric sheet loaded with the inner electrode alloy layer is taken out, and the inner electrode alloy layer is obtained after washing and baking in a protective atmosphere. Preferably, the washing method is to use acid solution and ethanol to wash alternately for multiple times; the acid solution is dilute nitric acid with a mass fraction of 5% to 30% or hydrochloric acid with a volume fraction of 20% to 30%; the baking temperature is 400-500°C, and the time is 3-6 hours. The organic matter attached to the reaction product can be removed by baking, thereby improving the purity of the alloy product.
[0010] In a preferred embodiment, the palladium salt is bistriphenylphosphine palladium dichloride or palladium chloride; and the molar ratio of the palladium salt to mercuric iodide is (1:1) to (1:9).
[0011] In a preferred embodiment, the solvent is a mixed solvent composed of an alcohol reagent, pyridine and N,N-dimethylformamide. Further preferably, the alcohol reagent is ethanol, and the volume ratio of ethanol, pyridine and N,N-dimethylformamide is (15-25):(8-12):1; in the mixed solvent, the alcohol reagent serves to provide a liquid phase environment with a certain viscosity, pyridine serves to stack and polymerize the alloy product, and N,N-dimethylformamide serves as a stabilizer.
[0012] In a preferred embodiment, the reducing agent is 2,3,5,6-tetrahydroxy-2-hexene-4-lactone, and each 1L of the mixed solution corresponds to 100g of the reducing agent.
[0013] The second object of the present invention is to provide an inner electrode alloy layer, which is prepared by the preparation method as described in the first object above; the inner electrode alloy layer includes palladium and mercury, the mass fraction of palladium is 10% to 40%, and the mass fraction of mercury is 60% to 90%. Preferably, the inner electrode alloy layer is formed by stacking cubic particles with a particle size of 50 to 100 nm and fine protrusions on the surface; the thickness of the inner electrode alloy layer is 50 to 500 nm, the appearance is silver-gray, and the surface has a metallic luster.
[0014] The present invention has the following beneficial effects:
[0015] The present invention prepares an inner electrode alloy layer by a liquid phase reduction method, wherein the alloy layer includes palladium and mercury elements, and palladium-mercury alloys with a sheet morphology can be formed between the palladium and mercury elements, and the sheet palladium-mercury alloys can be further stacked and polymerized to obtain a dense layered structure. The environmental temperature required for the process of the present invention is between 100 and 500°C, and the environmental conditions are relatively mild. At the same time, the resource utilization of the mercury element is realized, the amount of precious metal palladium is reduced, and the production cost is reduced. During the formation process, the alloy layer can be directly grown in situ on the surface of the ceramic dielectric sheet to obtain a dense structure, avoiding the steps of printing curing and high-temperature sintering in the prior art to combine the ceramic dielectric layer and the inner electrode together. The process of the present invention is simple, and the MLCC containing the inner electrode alloy layer has excellent performance, which has positive value for the commercial application of precious metal MLCC. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a scanning electron microscope photograph of the inner electrode alloy layer prepared in Example 1 of the present invention.
[0017] Figure 2 This is an EDS spectrum of the inner electrode alloy layer prepared in Example 1 of the present invention.
[0018] Figure 3 This is an EDS spectrum of the inner electrode alloy layer prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0019] The present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are only used to illustrate the present invention and are not intended to limit the present invention. Unless otherwise specified, the preparation processes in the following examples are all conventional means in the prior art of the art, and therefore, no further description is given; the raw materials used are all commercially available products and are commercially available.
[0020] Example 1
[0021] The mixed solution used in this embodiment is composed of ethanol, pyridine and N,N-dimethylformamide, with a volume ratio of 20:10:1, and 200mL is configured; bistriphenylphosphine palladium dichloride (0.1mol) and mercuric iodide (0.1mol) are weighed and added to the mixed solvent, and the mixed solution is ultrasonicated with ultrasound for 10 minutes; the ceramic dielectric sheet is placed in the mixed solution, and then the mixed solution is heated to 120°C. After the solution turns into light gray, 2,3,5,6-tetrahydroxy-2-hexene-4-lactone (20g) is slowly added; after the mixed solution changes from a turbid black solution to a yellow clear solution, the ceramic dielectric sheet is taken out; the ceramic dielectric sheet is first washed with dilute nitric acid with a mass fraction of 15%, and then washed with an ethanol solvent, and this is repeated several times; the ceramic dielectric sheet carrying the alloy layer is placed in a nitrogen atmosphere for baking, and the baking temperature is 450°C, and it is kept for 5 hours to obtain an inner electrode alloy layer.
[0022] The inner electrode alloy layer was peeled off from the ceramic dielectric sheet and tested by scanning electron microscope. The results are as follows Figure 1 As shown, from Figure 1 From the scanning electron microscope image in FIG, it can be seen that the inner electrode alloy layer is formed by non-directional stacking of particles with a particle size of 50 to 100 nm and fine protrusions on the surface, and the thickness is uneven.
[0023] Figure 2 This is a picture of the local EDS spectrum of the inner electrode alloy layer. From the data characterized by the EDS spectrum, it can be seen that the mass ratio of palladium element to mercury element is close to 1:2.8, and the molar ratio is close to 1:1.5.
[0024] Example 2
[0025] The mixed solution used in this embodiment is composed of ethanol, pyridine and N,N-dimethylformamide, with a volume ratio of 20:10:1, and 200mL is configured; bistriphenylphosphine palladium dichloride (0.1mol) and mercuric iodide (0.5mol) are weighed respectively and added to the mixed solvent, and the mixed solution is ultrasonicated with ultrasound for 10 minutes; the ceramic dielectric sheet is placed in the mixed solution, and then the mixed solution is heated to 120°C. After the solution turns into light gray, 2,3,5,6-tetrahydroxy-2-hexene-4-lactone (20g) is slowly added; after the mixed solution changes from a turbid black solution to a yellow clear solution, the ceramic dielectric sheet is taken out; the ceramic dielectric sheet is first washed with concentrated hydrochloric acid with a volume fraction of 25%, and then washed with ethanol solvent, and this is repeated many times; the ceramic dielectric sheet carrying the alloy layer is placed in a nitrogen atmosphere for baking, and the baking temperature is 450°C, and it is kept for 5 hours to obtain an inner electrode alloy layer.
[0026] Figure 3This is a picture of the local EDS energy spectrum of the alloy layer. From the data characterized by the EDS energy spectrum, it can be seen that the mass ratio of palladium element to mercury element is close to 1:6, and the molar ratio is close to 1:3.
[0027] It should be noted that, in other embodiments, when the experimental process meets the following conditions, the purpose of the present invention can be achieved:
[0028] The temperature for heating the mixed solution is preferably 100 to 180°C, and specifically can be 100°C, 130°C, 150°C, 180°C, etc.;
[0029] The baking temperature is preferably 400-500° C., and can be specifically 400° C., 430° C., 480° C., 500° C., etc. The baking time is preferably 3-6 h, and can be specifically 3 h, 4 h, 6 h, etc.
[0030] Those skilled in the art can make appropriate selections of the above process parameters according to actual needs, and all of them can achieve the purpose of the present invention.
[0031] Obviously, the described embodiments are only some embodiments of the present invention, but not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing an inner electrode alloy layer, characterized in that: The following steps are involved: A mixed solution is obtained by dispersing palladium salt and mercuric iodide in a solvent, a ceramic dielectric sheet is placed in the mixed solution, the mixed solution is heated to 100-180°C and a reducing agent is added, and as the reaction proceeds, an inner electrode alloy layer is grown on the surface of the ceramic dielectric sheet. After the mixed solution turns black and then yellow, the ceramic dielectric sheet loaded with the inner electrode alloy layer is taken out, and the inner electrode alloy layer is obtained after washing and baking in a protective atmosphere. The molar ratio of the palladium salt to mercuric iodide is (1:1) to (1:9); and the reducing agent is 2,3,5,6-tetrahydroxy-2-hexene-4-lactone.
2. The method for preparing the inner electrode alloy layer according to claim 1, characterized in that: The palladium salt is bistriphenylphosphine palladium dichloride or palladium chloride.
3. The method for preparing the inner electrode alloy layer according to claim 1, characterized in that: The solvent is a mixed solvent consisting of an alcohol reagent, pyridine and N,N-dimethylformamide.
4. The method for preparing the inner electrode alloy layer according to claim 3, characterized in that: The alcohol reagent is ethanol; the volume ratio of the ethanol, pyridine and N,N-dimethylformamide is (15-25):(8-12):
1.
5. The method for preparing the inner electrode alloy layer according to claim 1, characterized in that: The washing method comprises washing with acid solution and ethanol alternately for multiple times.
6. The method for preparing the inner electrode alloy layer according to claim 1, characterized in that: The baking temperature is 400-500° C. and the baking time is 3-6 hours.
7. An inner electrode alloy layer, characterized in that: The inner electrode alloy layer is prepared by the preparation method as described in any one of claims 1 to 6; the inner electrode alloy layer includes palladium element and mercury element, the mass fraction of the palladium element is 10%~40%, and the mass fraction of the mercury element is 60%~90%.
8. The inner electrode alloy layer according to claim 7, characterized in that: The thickness of the alloy layer is 50-500 nm.