A catalytic material using MXene as a carrier to load cobalt and a preparation method thereof

By grafting the metal active site Co on the MXene support and wrapping the porous silicon oxide, the Co-Ti3C2@pSiO2 catalytic material is formed, and the problems of insufficient metal ion dissolution and catalytic activity are solved, and efficient degradation and reduction of organic pollutants are achieved. Second pollution.

CN116265098BActive Publication Date: 2024-11-22JIANGSU UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310147537.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-11-22
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

In the prior art, when removing organic pollutants in wastewater, metal ions are prone to dissolution, resulting in secondary pollution, and the catalyst lacks catalytic activity, making it difficult to effectively treat difficult-to-degrade organic wastewater.

Method used

Using MXene as a support, the metal active site Co is grafted on a single layer of Ti3C2 nanomaterial and wrapped with porous silica to form a Co-Ti3C2@pSiO2 catalytic material, ensuring that the metal active site is highly dispersed on the support and avoid dissolution. and improve catalytic activity.

Benefits of technology

It significantly improves the catalytic activity of the catalyst, can effectively degrade organic pollutants such as p-nitrophenol, and avoids the dissolution of metal ions during the reaction, reducing secondary pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116265098B_ABST
    Figure CN116265098B_ABST
Patent Text Reader

Abstract

The present invention discloses a catalytic material with MXene as a carrier and loaded with cobalt, wherein the catalytic material uses a monolayer Ti3C2 nanomaterial as a carrier, a metal active site Co is grafted on the carrier, and a porous silicon oxide is wrapped on the carrier, and the metal active site Co contacts an external reactant through a through hole on the porous silicon oxide. The present invention also discloses a preparation method of the above-mentioned catalytic material with MXene as a carrier and loaded with cobalt, specifically: uniformly dropping a Ti3C2 dispersion into a mixed solution of CTAC and TEA, fully mixing at room temperature, then sequentially adding a divalent cobalt salt and TEOS to the mixed material, placing the reaction material in a high-temperature oil bath for reaction, centrifuging, washing, and drying after the reaction; placing the dried solid matter in an inert atmosphere for heat treatment to obtain a Co‑Ti3C2@pSiO2 catalytic material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a catalytic material using MXene as a carrier to load cobalt, and also relates to a method for preparing the catalytic material. Background Art

[0002] Urban industrialization has caused a large amount of difficult-to-degrade organic wastewater to flow into the natural environment. These difficult-to-degrade organic substances include dyes, antibiotics, phenols, aldehydes, drugs and hormones. A large part of these organic substances are difficult to degrade. The characteristics of wastewater organic substances are: high concentration, complex composition, strong acidity and alkalinity, toxicity, and inability to biodegrade on their own. If they cannot be effectively treated, they will cause harm to human health. At present, the more widely used methods for removing organic pollutants from wastewater include: activated sludge method, adsorption method, microbial degradation method, chemical oxidation method and membrane separation method. However, these methods still have limitations. Advanced oxidation technology (AOPs) can mineralize organic pollutants into CO2 and H2O. This advantage is expected to achieve efficient removal of organic pollutants in wastewater.

[0003] MXene is a new type of two-dimensional (2D) nanomaterial, which is composed of several atomic layers of transition metal carbides, nitrides or carbonitrides. This material is similar to graphene layered materials. It was first reported in 2011 and has a molecular formula of M n+1 X n T x (n=1-3), M is a transition metal, X is carbon and / or nitrogen, and T is a surface functional group. MXene nanomaterials are widely used in energy storage and conversion, sensors, electromagnetic shielding, and biomedicine. As a family of 2D materials, MXene has attracted increasing attention in the field of wastewater treatment due to its unique layered structure, strong hydrophilicity, and high catalytic activity. 2+ In the process of activating AOPs of PMS, it shows excellent performance, but the metal ions in homogeneous catalysts are prone to cause secondary pollution, and heterogeneous catalysts can effectively improve this problem. Therefore, the development and preparation of efficient heterogeneous catalysts is of great significance to solving the urgent problem of environmental pollution. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a catalytic material with cobalt loaded on a MXene carrier, and also to provide a method for preparing the above-mentioned catalytic material. On the one hand, the catalytic material can effectively avoid the dissolution of metal ions during the liquid phase reaction process, and on the other hand, it can achieve a highly dispersed state of metal active sites on the carrier, thereby greatly improving the catalytic activity of the catalyst.

[0005] Technical solution: The catalytic material of the present invention using MXene as a carrier to load cobalt, the catalytic material using a single layer of Ti3C2 nanomaterial as a carrier, the metal active site Co is grafted on the carrier, porous silicon oxide is wrapped on the carrier, and the metal active site Co contacts the external reactant through the through holes on the porous silicon oxide.

[0006] The loading amount of Co is 1.9-5.9% of the mass of the catalytic material.

[0007] The method for preparing the catalytic material using MXene as a carrier to load cobalt comprises the following steps:

[0008] (1) The Ti3C2 dispersion is uniformly added dropwise to a mixed solution of CTAC (hexadecyltrimethylammonium chloride) and TEA (triethanolamine), and the mixture is fully mixed at room temperature. Then, divalent cobalt salt and TEOS (tetraethoxysilane) are added to the mixture in sequence, and the reaction material is placed in a high-temperature oil bath for reaction. After the reaction, the mixture is centrifuged, washed, and dried;

[0009] (2) The dried solid product is placed in an inert atmosphere for heat treatment to obtain a Co-Ti3C2@pSiO2 catalytic material.

[0010] In the reaction system, CTAC is a template for forming porous silica. At high temperature (80°C), the silica generated by the hydrolysis of TEOS grows on CTAC. During the heat treatment, the CTAC template is removed to form porous silica. TEA provides a weakly alkaline environment to promote the hydrolysis of TEOS, so that the pH value of the reaction material is 8 to 9. At the same time, during the heat treatment, the divalent cobalt salt decomposes, and the metal active site Co is connected to the carrier at high temperature.

[0011] Wherein, in step (1), in the mixed solution, the volume ratio of CTAC aqueous solution to TEA is 45-50:1; in the CTAC aqueous solution, the mass concentration of CTAC is 10-12%; the volume ratio of Ti3C2 dispersion to the mixed solution is 1:0.92-1.02; in the Ti3C2 dispersion, the mass concentration of Ti3C2 is 0.5 mg·L -1 .

[0012] Wherein, in step (1), the added molar ratio of Ti3C2, divalent cobalt salt and TEOS is 6.2:13.2~52.8:1.

[0013] Wherein, in step (1), the divalent cobalt salt is cobalt nitrate hexahydrate.

[0014] Wherein, in step (1), the oil bath temperature is 80-85° C., and the oil bath time is 1-2 h.

[0015] Wherein, in step (1), the drying is freeze drying, the freeze drying temperature is -40 to -80°C, and the drying time is 12 to 48 hours. Freeze drying can prevent the dispersed metal particles from agglomerating again.

[0016] Wherein, in step (2), the heat treatment temperature is 350-360° C., and the heat treatment time is 2-6 hours.

[0017] The surface of Ti3C2 material contains a large number of hydroxyl and carboxyl hydrophilic functional groups. Ti3C2 material is connected to the metal active site Co through active groups. The porous silicon oxide confines the metal cobalt connected to Ti3C2 between Ti3C2 and the porous silicon oxide, preventing the metal active site Co from dissolving during the reaction. Since silicon oxide is porous, it provides a smooth channel for the reactant to contact the metal active site. The present invention adopts an in-situ method to dope cobalt on the carrier and wrap porous silicon dioxide outside the carrier, so that the metal cobalt can be highly dispersed on the Ti3C2 carrier, and the metal cobalt is confined between the Ti3C2 carrier and the porous silicon dioxide.

[0018] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the catalytic material of the present invention can effectively improve the dispersion of the metal active site Co on Ti3C2@pSiO2, that is, the metal active site Co has good dispersion on Ti3C2@pSiO2, thereby obtaining a catalytic material with more accessible metal active sites, thereby improving the catalytic activity of the catalytic material, and exhibiting excellent degradation performance when activating PMS to degrade p-nitrophenol, and at the same time can effectively prevent the metal from dissolving during the reaction and causing secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The N2 adsorption-desorption isotherm of the catalytic material (Co-Ti3C2@pSiO2) of the present invention prepared in Example 4;

[0020] Figure 2 1 and 2 are XRD diagrams of the catalytic materials prepared in Example 1, Example 4 and Comparative Example 1. DETAILED DESCRIPTION

[0021] Example 1

[0022] The preparation method of porous silicon oxide wrapped single-layer Ti3C2 catalytic material is specifically as follows:

[0023] 10 mL of CTAC aqueous solution (the mass concentration of CTAC in the CTAC aqueous solution is 10%) and 200 μL of TEA were added to a beaker and stirred in a water bath at room temperature for 10 min. Then, 10 mL of Ti3C2 aqueous solution (the mass concentration of Ti3C2 in the Ti3C2 aqueous solution is 0.5 mg·L-1 ), the solution turned from white to dark green, and the same conditions were maintained and stirred for another 90 min; the reaction solution was poured into a 50 mL round-bottom flask, the oil bath was set to 80 ° C, 150 μL TEOS was added after the temperature stabilized, and the reaction was timed for 1 h; the product was collected by centrifugation, washed twice with ethanol to remove impurities, freeze-dried at -80 ° C for 48 h, and ground into powder, and the freeze-dried sample was placed in a tubular furnace and calcined under a nitrogen atmosphere at 2.0 ° C min -1 The sample was heat treated at 350°C for 360 min at a heating rate of , and a catalytic material of a single layer of Ti3C2 wrapped in porous silicon oxide was obtained.

[0024] The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. High-purity liquid chromatography was used to measure the catalytic material activated PMS to evaluate the degradation of p-nitrophenol. The reaction conditions for the degradation were room temperature, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05 g of catalytic material was added, stirred for 30 minutes, and then 0.5 g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 10.1% within 90 minutes.

[0025] Example 2

[0026] The present invention provides a method for preparing a catalytic material using MXene as a carrier to load cobalt, specifically comprising:

[0027] 10 mL of CTAC aqueous solution (the mass concentration of CTAC in the CTAC aqueous solution is 10%) and 200 μL of TEA were added to a beaker and stirred in a water bath at room temperature for 10 min. Then, 10 mL of Ti3C2 aqueous solution (the mass concentration of Ti3C2 in the Ti3C2 aqueous solution is 0.5 mg·L -1 ), the solution turned from white to dark green, and the same conditions were maintained and stirred for another 90 min; the reaction solution was poured into a 50 mL round-bottom flask, the oil bath was set to 80 ° C, and after the temperature stabilized, 0.02 g of cobalt nitrate hexahydrate was added, and after the cobalt nitrate hexahydrate was completely dissolved, 150 μL of TEOS was immediately added thereto, and the reaction was timed for 1 h; the product was collected by centrifugation, washed twice with ethanol to remove impurities, freeze-dried at -80 ° C for 48 h, and ground into powder, and the freeze-dried sample was placed in a tube furnace and calcined under a nitrogen atmosphere at 2.0 ° C min -1 The sample was heat treated at 350℃ for 360min at a heating rate of 1.5℃ and was Co-Ti3C2@pSiO2 catalytic material.

[0028] The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. High-purity liquid chromatography was used to measure the catalytic material activated PMS to evaluate the degradation of p-nitrophenol. The reaction conditions for the degradation were room temperature, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05 g of catalytic material was added, stirred for 30 minutes, and then 0.5 g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 45 minutes.

[0029] Example 3

[0030] The present invention provides a method for preparing a catalytic material using MXene as a carrier to load cobalt, specifically comprising:

[0031] 10 mL of CTAC aqueous solution (the mass concentration of CTAC in the CTAC aqueous solution is 10%) and 200 μL of TEA were added to a beaker and stirred in a water bath at room temperature for 10 min. Then, 10 mL of Ti3C2 aqueous solution (the mass concentration of Ti3C2 in the Ti3C2 aqueous solution is 0.5 mg·L -1 ), the solution turned from white to dark green, and the same conditions were maintained and stirred for another 90 min; the reaction solution was poured into a 50 mL round-bottom flask, the oil bath was set to 80 ° C, and after the temperature stabilized, 0.04 g of cobalt nitrate hexahydrate was added, and after the cobalt nitrate hexahydrate was completely dissolved, 150 μL of TEOS was immediately added thereto, and the reaction was timed for 1 h; the product was collected by centrifugation, washed twice with ethanol to remove impurities, freeze-dried at -80 ° C for 48 h, and ground into powder, and the freeze-dried sample was placed in a tubular furnace and calcined under a nitrogen atmosphere at 2.0 ° C min -1 The sample was heat treated at 350℃ for 360min at a heating rate of 1.5℃ and was Co-Ti3C2@pSiO2 catalytic material.

[0032] The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. High-purity liquid chromatography was used to measure the catalytic material activated PMS to evaluate the degradation of p-nitrophenol. The reaction conditions for the degradation were room temperature, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05 g of catalytic material was added, stirred for 30 minutes, and then 0.5 g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 30 minutes.

[0033] Example 4

[0034] The present invention provides a method for preparing a catalytic material using MXene as a carrier to load cobalt, specifically comprising:

[0035] 10 mL of CTAC aqueous solution (the mass concentration of CTAC in the CTAC aqueous solution is 10%) and 200 μL of TEA were added to a beaker and stirred in a water bath at room temperature for 10 min. Then, 10 mL of Ti3C2 aqueous solution (the mass concentration of Ti3C2 in the Ti3C2 aqueous solution is 0.5 mg·L -1 ), the solution turned from white to dark green, and the same conditions were maintained and stirred for another 90 min; the reaction solution was poured into a 50 mL round-bottom flask, the oil bath was set to 80 ° C, and after the temperature stabilized, 0.06 g of cobalt nitrate hexahydrate was added, and after the cobalt nitrate hexahydrate was completely dissolved, 150 μL of TEOS was immediately added thereto, and the reaction was timed for 1 h; the product was collected by centrifugation, washed twice with ethanol to remove impurities, freeze-dried at -80 ° C for 48 h, and ground into powder, and the freeze-dried sample was placed in a tubular furnace and calcined under a nitrogen atmosphere at 2.0 ° C min -1 The sample was heat treated at 350℃ for 360min at a heating rate of 1.5℃ and was Co-Ti3C2@pSiO2 catalytic material.

[0036] The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. High-purity liquid chromatography was used to measure the catalytic material activated PMS to evaluate the degradation of p-nitrophenol. The reaction conditions for the degradation were room temperature (25 ° C), an initial concentration of p-nitrophenol of 20 mg·L -1 First, 0.05g of catalytic material was added, stirred for 30 minutes, and then 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 20 minutes, and the reaction rate was 0.254min -1 .

[0037] Example 5

[0038] The present invention provides a method for preparing a catalytic material using MXene as a carrier to load cobalt, specifically comprising:

[0039] 10 mL of CTAC aqueous solution (the mass concentration of CTAC in the CTAC aqueous solution is 10%) and 200 μL of TEA were added to a beaker and stirred in a water bath at room temperature for 10 min. Then, 10 mL of Ti3C2 aqueous solution (the mass concentration of Ti3C2 in the Ti3C2 aqueous solution is 0.5 mg·L -1), the solution turned from white to dark green, and the same conditions were maintained and stirred for another 90 min; the reaction solution was poured into a 50 mL round-bottom flask, the oil bath was set to 80 ° C, and after the temperature stabilized, 0.08 g of cobalt nitrate hexahydrate was added, and after the cobalt nitrate hexahydrate was completely dissolved, 150 μL of TEOS was immediately added thereto, and the reaction was timed for 1 h; the product was collected by centrifugation, washed twice with ethanol to remove impurities, freeze-dried at -80 ° C for 48 h, and ground into powder, and the freeze-dried sample was placed in a tubular furnace and calcined under a nitrogen atmosphere at 2.0 ° C min -1 The sample was heat treated at 350℃ for 360min at a heating rate of 1.5℃ and was Co-Ti3C2@pSiO2 catalytic material.

[0040] The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. High-purity liquid chromatography was used to measure the catalytic material activated PMS to evaluate the degradation of p-nitrophenol. The reaction conditions for the degradation were room temperature, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05g of catalytic material was added, stirred for 30 minutes, and then 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 20 minutes, and the reaction rate was 0.11min -1 .

[0041] By comparing Examples 1 to 5, it can be seen that different amounts of cobalt nitrate hexahydrate introduced have a great influence on the catalytic material activation of PMS to degrade p-nitrophenol. The experimental results show that when 0.06 g of cobalt nitrate hexahydrate is added, the effect of activating PMS to degrade p-nitrophenol is best.

[0042] Example 6

[0043] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 15 °C and an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05g of catalytic material was added, stirred for 30 minutes, and then 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 45 minutes, and the reaction rate was 0.167min -1 .

[0044] Example 7

[0045] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 35 °C and an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05g of catalytic material was added, stirred for 30 minutes, and then 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 10 minutes, and the reaction rate was 0.283min -1 .

[0046] It can be seen from Examples 4, 6 and 7 that the experiments were conducted at different temperatures of 15, 25 and 35° C., and the results showed that the removal efficiency of p-nitrophenol was higher as the temperature increased.

[0047] Example 8

[0048] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 25 °C, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.2M H2SO4 was added to the solution to make the pH value of the solution 3, and then 0.05g of the catalytic material was added thereto. After stirring for 30 minutes, 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 20 minutes.

[0049] Example 9

[0050] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 25 °C, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.2M H2SO4 was added to the solution to make the pH value of the solution 5, and then 0.05g of catalytic material was added thereto. After stirring for 30 minutes, 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 20 minutes.

[0051] Example 10

[0052] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 25 °C, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.2M KOH was added to the solution to make the pH value 7, and then 0.05g of the catalytic material was added thereto. After stirring for 30 minutes, 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 20 minutes.

[0053] Embodiment 11

[0054] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 25 °C, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.2M KOH was added to the solution to make the pH value 9, and then 0.05g of the catalytic material was added thereto. After stirring for 30 minutes, 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 20 minutes.

[0055] It can be seen from Examples 8 to 11 that the initial pH value of the reaction solution has no significant effect on the catalytic activity.

[0056] Example 12

[0057] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 25 °C, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.0125 g of catalytic material was added, stirred for 30 minutes, and then 0.5 g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 60 minutes.

[0058] Embodiment 13

[0059] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 25 °C, an initial p-nitrophenol concentration of 20 mg·L -1First, 0.025 g of catalytic material was added, stirred for 30 minutes, and then 0.5 g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 45 minutes.

[0060] Embodiment 14

[0061] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 25 °C, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.075g of catalytic material was added, stirred for 30 minutes, and then 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 10 minutes.

[0062] It can be seen from Examples 4, 12, 13 and 14 that different initial catalyst concentrations have a significant effect on the degradation of p-nitrophenol, and the time for completely degrading p-nitrophenol is shortened from 45 min to 10 min.

[0063] Embodiment 15

[0064] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 25 °C, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05 g of catalytic material was added, stirred for 30 minutes, and then 0.125 g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 45 minutes.

[0065] Example 16

[0066] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 25 °C, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05 g of catalytic material was added, stirred for 30 minutes, and then 0.25 g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 20 minutes.

[0067] Embodiment 17

[0068] The performance of the catalyst material in Example 4 for activating PMS to remove p-nitrophenol was tested by HPLC: The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The degradation reaction conditions were 25 °C, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05 g of catalytic material was added, stirred for 30 minutes, and then 0.75 g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 100% within 10 minutes.

[0069] It can be seen from Examples 4, 15, 16 and 17 that different PMS concentrations have a significant effect on the degradation of p-nitrophenol.

[0070] Embodiment 18

[0071] Investigate the effect of anions and cations on the degradation of p-nitrophenol: The adsorption degradation process was carried out in a 500mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. High-purity liquid chromatography was used to measure the catalytic material activation of PMS to evaluate the degradation of p-nitrophenol. In the process of activating PMS to degrade organic pollutants, anions and cations and soluble organic pollutants are widely present in actual water bodies. The reaction conditions for the degradation are 25°C, an initial concentration of p-nitrophenol of 20 mg·L -1 First, add 0.05g of catalytic material, then add 5mmol L -1 Anion (HCO3 - , Cl - 、SO4 2- 、NO3 - ) and cations (Mg 2 + , Ca 2+ , K + 、Na + ) There are eight control experiments in total. All control experiments were carried out under the same conditions. After stirring for 30 minutes, 0.5g of PMS was added. The test results showed that HCO3 - It has a significant promoting effect on p-nitrophenol, Cl - There is a slight inhibitory effect, and other effects can be ignored. All of them can completely remove p-nitrophenol.

[0072] Embodiment 19

[0073] To investigate the stability of the catalytic material of Example 4: after the reaction, the catalytic material of Example 4 was collected by filtration, washed with deionized water, and freeze-dried at -80°C for 48 hours. The freeze-dried sample was placed in a tubular furnace and calcined at 350°C for 180 minutes under a nitrogen atmosphere to obtain the first regenerated catalyst.

[0074] The performance of the first regenerated catalytic material in activating PMS to remove p-nitrophenol was tested by HPLC: the adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The reaction conditions for the degradation were 25 °C and an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05g of the first regenerated catalyst was added, and after stirring for 30 minutes, 0.5g of PMS was added and catalytic degradation was carried out again. The reaction was run for 90 minutes. The test results showed that 99.1% of p-nitrophenol could be removed.

[0075] Embodiment 20

[0076] The stability of the catalytic material of Example 19 was investigated: after the reaction, the catalytic material of Example 19 was collected by filtration, washed with deionized water, and freeze-dried at -80°C for 48 hours. The freeze-dried sample was placed in a tubular furnace and calcined at 350°C for 180 minutes under a nitrogen atmosphere to obtain a second regenerated catalyst.

[0077] The performance of the second regenerated catalytic material in activating PMS to remove p-nitrophenol was tested by HPLC: the adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The reaction conditions for the degradation were 25 °C and an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05g of the first regenerated catalyst was added, and after stirring for 30 minutes, 0.5g of PMS was added and catalytic degradation was carried out again. The reaction was run for 90 minutes. The test results showed that 99.2% of p-nitrophenol could be removed.

[0078] Embodiment 21

[0079] To investigate the stability of the catalytic material of Example 20: After the reaction, the catalytic material of Example 20 was collected by filtration, washed with deionized water, and freeze-dried at -80°C for 48 hours. The freeze-dried sample was placed in a tubular furnace and calcined at 350°C for 180 minutes under a nitrogen atmosphere to obtain a third regenerated catalyst.

[0080] The performance of the third regenerated catalytic material activated PMS to remove p-nitrophenol was tested by HPLC: the adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. The reaction conditions for the degradation were 25 °C and an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05g of the third regenerated catalyst was added, and after stirring for 30 minutes, 0.5g of PMS was added and catalytic degradation was carried out again. The reaction was run for 90 minutes. The test results showed that 98.2% of p-nitrophenol could be removed.

[0081] It can be seen from Examples 19 to 21 that after three consecutive 90-min runs, the results show that the removal efficiency of the third regenerated catalyst for p-nitrophenol can still reach more than 98%, indicating that the catalytic material has good stability and repeatability.

[0082] Embodiment 22

[0083] The performance of catalytic material activation of PMS in Example 4 for removing 2,4,6-trichlorophenol was tested by high performance liquid chromatography: the adsorption degradation process was carried out in a 500 mL beaker, with 2,4,6-trichlorophenol as the target pollutant and PMS as the oxidant. The reaction conditions for the degradation were 25 °C, an initial concentration of 2,4,6-trichlorophenol of 20 mg·L -1 First, 0.05g of catalytic material was added, stirred for 30 minutes, and then 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on 2,4,6-trichlorophenol was 98% within 10 minutes.

[0084] Embodiment 23

[0085] The performance of catalytic material activating PMS to remove atrazine in Example 4 was tested by high performance liquid chromatography: the adsorption degradation process was carried out in a 500 mL beaker, with atrazine as the target pollutant and PMS as the oxidant. The reaction conditions for the degradation were 25 ° C and an initial atrazine concentration of 20 mg·L -1 First, 0.05g of catalytic material was added, stirred for 30 minutes, and then 0.5g of PMS was added. The test results showed that the degradation activity of the catalytic material on atrazine was 96.5% within 30 minutes.

[0086] Embodiment 24

[0087] The performance of catalytic material activating PMS to remove acetaminophen in Example 4 was tested by high performance liquid chromatography: the adsorption degradation process was carried out in a 500 mL beaker, with acetaminophen as the target pollutant and PMS as the oxidant. The reaction conditions for the degradation were 25°C and an initial concentration of acetaminophen of 20 mg·L -1 First, 0.05g of catalytic material was added, stirred for 30 minutes, and then 0.5g of PMS was added. The test results showed that the degradation activity of acetaminophen by the catalytic material was 100% within 5 minutes.

[0088] Comparative Example 1

[0089] A method for preparing a catalytic material using MXene as a carrier to load cobalt, specifically comprising:

[0090] 10 mL of CTAC aqueous solution (the mass concentration of CTAC in the CTAC aqueous solution is 10%) and 200 μL of TEA were added to a beaker and stirred in a water bath at room temperature for 10 min. Then, 10 mL of Ti3C2 aqueous solution (the mass concentration of Ti3C2 in the Ti3C2 aqueous solution is 0.5 mg·L -1 ), the solution turned from white to dark green, and the same conditions were maintained and stirred for another 90 min; the reaction solution was poured into a 50 mL round-bottom flask, the oil bath was set to 80 ° C, and after the temperature stabilized, 0.06 g of cobalt nitrate hexahydrate was added, and after the cobalt nitrate hexahydrate was completely dissolved, 150 μL of TEOS was immediately added thereto, and the reaction was timed for 1 h; after the reaction was completed, the obtained sample solution was evaporated to dryness in a 60 ° C water bath (the water bath evaporation drying method will cause the active site Co on the carrier to agglomerate), and the obtained solid sample was placed in a tubular furnace and calcined in a nitrogen atmosphere, and the heating rate was 2.0 ° C min -1 After heat treatment at 350℃ for 360min, the obtained sample is Co-Ti3C2@pSiO2-evap catalytic material.

[0091] The adsorption degradation process was carried out in a 500 mL beaker, with p-nitrophenol as the target pollutant and PMS as the oxidant. High-purity liquid chromatography was used to measure the catalytic material activated PMS to evaluate the degradation of p-nitrophenol. The reaction conditions for the degradation were room temperature, an initial p-nitrophenol concentration of 20 mg·L -1 First, 0.05 g of catalytic material was added, stirred for 30 minutes, and then 0.5 g of PMS was added. The test results showed that the degradation activity of the catalytic material on p-nitrophenol was 49.3% within 90 minutes.

[0092] like Figure 1 As shown in Figure 2, the porous structure of the sample was studied by N2 adsorption-desorption, proving that porous silica was successfully wrapped on the Ti3C2 carrier. Figure 2 As shown, Example 4 is a catalytic material prepared by the in-situ method, and its spectrum does not show the characteristic peak of Co, indicating that Co has good dispersibility on the Ti3C2 carrier; while the catalytic material prepared in Comparative Example 1 with the same Co loading as Example 4 (a different drying method is used in Comparative Example 1) shows obvious Co diffraction peaks on the spectrum, indicating that Co is agglomerated on the Ti3C2 carrier. This shows that Co is highly dispersed on the catalytic material carrier prepared by the in-situ method. It can be seen from the catalytic results of Comparative Example 1 that its catalytic degradation effect is significantly reduced, indicating that the active metal site Co shows good dispersibility on Ti3C2@pSiO2, which is more conducive to the degradation of the pollutant p-nitrophenol.

Claims

1. A catalytic material with cobalt supported by MXene, Features: The catalytic material is a single layer Ti 3 C 2 The nanomaterial is used as a carrier, the metal active site Co is grafted on the carrier, the porous silicon oxide is wrapped on the carrier, and the metal active site Co contacts the external reactant through the through holes on the porous silicon oxide; the loading amount of Co is 1.9-5.9% of the mass of the catalytic material; The above catalytic material is prepared by the following method, and the specific steps are as follows: (1) Ti 3 C 2 The dispersion is uniformly added dropwise to a mixed solution of CTAC aqueous solution and TEA, and the mixture is fully mixed at room temperature. Then, divalent cobalt salt and TEOS are sequentially added to the mixed material, and the reaction material is placed in a high-temperature oil bath for reaction. After the reaction, the mixture is centrifuged, washed, and freeze-dried. (2) The dried solid is placed in an inert atmosphere for heat treatment to obtain Co-Ti 3 C 2 @ p SiO 2 Catalytic materials; The catalytic material is used for catalyzing peroxymonosulfate to degrade the organic pollutant p-nitrophenol in water.

2. The catalytic material of claim 1 wherein the MXene is used as a carrier to support cobalt. Features: In step (1), the volume ratio of CTAC aqueous solution to TEA in the mixed solution is 45-50:1; the mass concentration of CTAC in the CTAC aqueous solution is 10-12%; Ti 3 C 2 The volume ratio of the dispersion to the mixed solution is 1:0.92~1.02; Ti 3 C 2 In the dispersion, Ti 3 C 2 The mass concentration is 0.5 mg·L −1 .

3. The catalytic material of claim 1 wherein the MXene is used as a carrier to support cobalt. Features: In step (1), Ti 3 C 2 The molar ratio of added divalent cobalt salt and TEOS is 6.2:13.2~52.8:

1.

4. The catalytic material of claim 1 wherein the MXene is used as a carrier to support cobalt. Features: In step (1), the divalent cobalt salt is cobalt nitrate hexahydrate.

5. The catalytic material of claim 1 wherein the MXene is used as a carrier to support cobalt. Features: In step (1), the oil bath temperature is 80-85°C, and the oil bath time is 1-2h.

6. The catalytic material of claim 1 wherein the MXene is used as a carrier to support cobalt. Features: In step (1), the freeze-drying temperature is -40 to -80°C, and the drying time is 12 to 48 hours.

7. The catalytic material of claim 1 wherein the MXene is used as a carrier to support cobalt. Features: In step (2), the heat treatment temperature is 350-360°C and the heat treatment time is 2-6 hours.