A graphene-based hydrogel spherical catalytic material and its preparation method and application

Through the design of graphene-based hydrogel sphere catalytic material, the problem of photocatalysts not responding to visible light in degrading organic pollutants is solved, and the efficient degradation of various organic pollutants is achieved, providing a safe and simple , green and inexpensive solutions.

CN116272941BActive Publication Date: 2024-11-08SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310288890.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-11-08
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

Existing photocatalysts have problems such as non-responsiveness of visible light and difficulty in recovering catalysts in degrading organic pollutants, which limits their wide application.

Method used

Using graphene-based hydrogel sphere catalytic material, the catalyst stability is achieved by combining graphene oxide with graphene-titanium oxide composite catalyst with materials such as sodium alginate and polyvinyl alcohol. Disperse and recycle and reuse.

Benefits of technology

It achieves efficient degradation of a variety of organic pollutants (≥90%), and provides a safe, simple, green and low-cost process with wide practical application value and industrial prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116272941B_ABST
    Figure CN116272941B_ABST
Patent Text Reader

Abstract

The present invention relates to a graphene-based hydrogel ball catalytic material and a preparation method and application thereof, wherein a graphene oxide / graphene-catalyst solution is added to a sodium alginate PVA solution to obtain a precursor solution; the precursor solution is added dropwise to a calcium chloride boric acid solution, and after being formed, it is moved to a sodium sulfate solution to obtain a catalyst-containing hydrogel ball. The present invention is applied to photocatalytic degradation of organic matter, solves the problems of low degradation efficiency of existing catalysts, difficulty in recovery, and poor anti-interference ability of the system, and has the characteristics of increasing the anti-interference ability of the system, improving the absorption capacity of the catalyst to visible light, and increasing the recycling of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water treatment, and in particular to a graphene-based hydrogel spherical catalytic material and a preparation method and application thereof. Background Art

[0002] In recent years, environmental pollution has attracted widespread attention from all over the world. Photocatalysts have potential application prospects in the degradation of organic pollutants. Titanium dioxide has been widely studied as a catalyst that is recognized to have high catalytic activity, strong stability, and no secondary pollution to the environment. Especially in recent years, with the advent of the research boom on visible light response, there has been an increasing number of studies on the doping and modification of titanium dioxide to reduce the bandgap width of catalyst materials and achieve visible light response, and the effect has gradually become obvious. However, in addition to the characteristics of the catalytic materials themselves, the recovery of the catalyst is also an urgent problem to be solved in daily use. Therefore, it is necessary to physically fix the catalyst material without significantly reducing its catalytic performance, so as to achieve the purpose of recycling and reusing the catalytic material. Summary of the invention

[0003] In order to overcome the shortcomings of the prior art, the present invention provides a graphene-based hydrogel spherical catalytic material and a preparation method and application thereof. The present invention uses conventional hydrogel as a substrate and obtains a catalyst-containing hydrogel through a simple mixing, molding and curing method.

[0004] The present invention is conceived for the common photocatalytic material TiO2. In the actual use process, there are problems such as no visible light response and difficult recovery of the catalytic material. It is necessary to compound and fix titanium dioxide to form a large-particle catalytic material with visible light response. Graphene has the characteristics of high specific surface area and surface modifiability. Graphene oxide (GO) has abundant oxygen-containing functional groups (hydroxyl, epoxy and carboxyl) so that it can be stably dispersed in water, and its large number of large π bonds can combine with partially reduced graphene to form a stable dispersion. Therefore, in the designed hydrogel material containing catalyst, graphene oxide and graphene-titanium oxide composite catalyst are first stably dispersed, and then compounded with hydrogel materials-PVA and sodium alginate to form a hydrogel catalyst with visible light response, uniform dispersion and stability. In addition, the preparation method is safe and simple, the process is green and environmentally friendly, and the cost is low.

[0005] The purpose of the present invention can be achieved by the following technical scheme: a graphene-based hydrogel spherical catalytic material is prepared by adding a graphene oxide / graphene-catalyst solution to a sodium alginate polyvinyl alcohol (PVA) solution to obtain a precursor solution; the precursor solution is added dropwise to a calcium chloride boric acid solution, and after a spherical gel is formed, the solution is transferred to a sodium sulfate solution to obtain a catalyst-containing hydrogel sphere.

[0006] The preparation method of the graphene-based hydrogel spherical catalytic material comprises the following specific steps:

[0007] (1) preparing a precursor solution: mixing a polyvinyl alcohol sodium alginate solution with a mixed solution containing graphene oxide and a graphene-titanium oxide composite catalyst to obtain a precursor solution;

[0008] (2) Preparation of spherical gel: adding the precursor solution dropwise into a calcium chloride boric acid solution to react and obtain a spherical gel;

[0009] (3) Preparation of graphene-based hydrogel spherical catalytic material: adding the spherical gel into a sodium sulfate solution and reacting sufficiently, taking out and washing to obtain the graphene-based hydrogel spherical catalytic material.

[0010] In the polyvinyl alcohol sodium alginate solution, the concentration of polyvinyl alcohol is 3-15% (w / v), and the mass ratio of sodium alginate to polyvinyl alcohol is 1:4-15.

[0011] The mass ratio of graphene oxide, graphene-titanium oxide composite catalyst and polyvinyl alcohol is 1:5-40:40-80.

[0012] The concentration of calcium chloride in the calcium chloride boric acid solution is 20 g / L, and the concentration of boric acid is 30 g / L.

[0013] The concentration of the sodium sulfate solution is 1M.

[0014] The application of the graphene-based hydrogel spherical catalytic material in the degradation and treatment of organic pollutants in water.

[0015] The graphene-based hydrogel catalytic material is placed in a photodegradation device and directly poured into wastewater containing organic pollutants for treatment.

[0016] The organic pollutants are one or more of dyes, animal and plant oils, and antibiotics, and the mass concentration is 0-100 mg / L and is not equal to 0.

[0017] Beneficial effects:

[0018] (1) In the present invention, PVA and sodium alginate are used as gel substrates, which are widely available and low in cost;

[0019] (2) The mixing, molding and curing method of the present invention is simple to operate, can save operation steps and time, and is a green and environmentally friendly synthesis method;

[0020] (3) The catalyst-containing hydrogel material of the present invention has a good decomposition efficiency (≥90%) for wastewater containing various organic pollutants. The catalyst-containing hydrogel material is expected to be applied in the field of sewage treatment and has a wide range of practical application value and industrial production prospects.

[0021] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic diagram of the preparation process of the graphene-based hydrogel spherical catalytic material in Example 1;

[0023] Figure 2 These are optical photographs and scanning electron microscope photographs of the graphene-based hydrogel sphere catalytic material in Example 1.

[0024] Figure 3 The graphene-based hydrogel spherical catalytic material in Example 1 shows the degradation effect of wastewater under visible light. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. The following specific embodiments are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0026] A method for preparing hydrogel spheres containing a catalyst comprises the following steps:

[0027] (1) Weigh a certain amount of polyvinyl alcohol (PVA) and add it to 1 L of water, heat and stir at 94° C. until it is completely dissolved, and cool to room temperature to obtain a PVA solution;

[0028] (2) Weigh a certain amount of sodium alginate, add it to the above PVA solution, and stir at room temperature until the solution is completely dissolved to obtain a mixed solution A;

[0029] (3) Weighing a certain amount of graphene oxide and graphene-titanium oxide composite catalyst, dispersing them by ultrasonication (2 h), adding them to the mixed solution A, and stirring them to form a mixed solution B;

[0030] (4) Weigh a certain amount of anhydrous calcium chloride and boric acid and add them to 1 L of water, stirring at room temperature until the solution is completely dissolved to obtain a mixed solution C;

[0031] (5) Weigh a certain amount of sodium sulfite and add it to 1 L of water. Stir at room temperature until the solution is completely dissolved to obtain solution D.

[0032] (6) Add the mixed solution A dropwise to the mixed solution C using a pump, and stir gently for 20 min (stirring speed not higher than 600 rpm), then take out;

[0033] (7) The obtained spherical gel was placed in solution D, and after gentle stirring for 2 h, it was taken out and washed with clean water for about 3 times to obtain hydrogel spheres containing the catalyst.

[0034] Preferably, the method for preparing catalyst-containing hydrogel spheres is characterized in that the mass ratio of the PVA and deionized water in step (1) is 7:100.

[0035] Preferably, the method for preparing catalyst-containing hydrogel spheres is characterized in that the mass ratio of sodium alginate to deionized water in step (2) is 1:100.

[0036] Preferably, the method for preparing catalyst-containing hydrogel balls is characterized in that the mass ratio of graphene oxide, graphene-titanium oxide composite catalyst and PVA in step (3) is 1:20:40.

[0037] Preferably, the method for preparing catalyst-containing hydrogel spheres is characterized in that the mass ratio of anhydrous calcium chloride, boric acid and deionized water in step (4) is 2:3:100.

[0038] Preferably, the method for preparing catalyst-containing hydrogel spheres is characterized in that the mass ratio of sodium sulfate to deionized water in step (5) is 3:20.

[0039] The second object of the present invention is a hydrogel containing a catalyst prepared by the method as described above.

[0040] The third object of the present invention is to use the above-mentioned hydrogel containing a catalyst for degrading organic pollutants in water, comprising the following steps:

[0041] Select wastewater containing organic pollutants, wherein the organic pollutants are one or more of dyes, antibiotics, animal and plant oils, small molecular organic matter, etc., with a mass concentration of 0-100 mg / L. Place the catalyst-containing hydrogel balls in a photodegradation device and directly pour the water containing organic pollutants. Measure the organic content and degradation efficiency of the filtrate by UV-visible spectrophotometer.

[0042] Embodiment 1:

[0043] Reference Figure 1 , a method for preparing a graphene-based hydrogel spherical catalytic material, comprising the following steps:

[0044] 1. Dissolve PVA in deionized water at 94°C with stirring to form a 10% (w / v) PVA aqueous solution;

[0045] 2. Weigh a certain amount of sodium alginate and dissolve it in the above PVA aqueous solution to form a mixed solution A, where the mass ratio of sodium alginate to PVA is 1:10.

[0046] 3. Weigh a certain amount of graphene oxide and graphene-titanium oxide (Long Mei, Cong Ye, Li Xuanke, et al. Hydrothermal synthesis of partially reduced graphene oxide / titanium dioxide composites and their photocatalytic activity [J]. Acta Physico-Chimica Sinica, 2013, 29(06): 1344-1350.) composite catalyst and ultrasonically disperse them in deionized water to form a mixed solution B. The mass ratio of graphene oxide to catalyst is 1:20.

[0047] 4. Mix the mixed solutions A and B, add a certain amount of deionized water, and stir evenly to form a precursor dispersion. At this time, the mass ratio of graphene oxide, composite catalyst, sodium alginate, and PVA is 1:20:5:50, and the concentration of PVA is 7% (w / v).

[0048] 5. Weigh a certain amount of anhydrous calcium chloride and boric acid to prepare a mixed solution C of 20g / L and 30g / L; weigh a certain amount of sodium sulfate to prepare a 1M solution D.

[0049] 6. Add the precursor solution dropwise into the mixed solution C, gently stir for 20 minutes, take it out and place it in solution D and continue stirring for 2 hours. Take it out and wash it to form hydrogel balls containing the catalyst.

[0050] 7. Figure 2 These are optical photographs and scanning electron microscope images of the hydrogel balls containing the catalyst in this example. It can be seen that the catalyst is evenly dispersed inside the three-dimensional gel balls and forms a special macroporous structure, which provides a large-aperture channel for water purification and improves the adsorption characteristics.

[0051] 8. Figure 3 This is a comparison of the hydrogel balls containing catalysts before and after photocatalytic degradation of wastewater in this example. As can be seen from the figure, it is explained that the composite of graphene and titanium oxide greatly improves the utilization efficiency of visible light, and can degrade organic pollutants in the original wastewater under visible light conditions.

[0052] Embodiment 2:

[0053] Reference Figure 1 , a method for preparing a graphene-based hydrogel spherical catalytic material, comprising the following steps:

[0054] 1. Dissolve PVA in deionized water at 94°C with stirring to form an 8% (w / v) PVA aqueous solution;

[0055] 2. Weigh a certain amount of sodium alginate and dissolve it in the above PVA aqueous solution to form a mixed solution A, where the mass ratio of sodium alginate to PVA is 1:5.

[0056] 3. Weigh a certain amount of graphene oxide and graphene-titanium oxide composite catalyst and ultrasonically disperse them in deionized water to form a mixed solution B, where the mass ratio of graphene oxide to catalyst is 1:10.

[0057] 4. Mix the mixed solutions A and B, add a certain amount of deionized water, and stir evenly to form a precursor dispersion. At this time, the mass ratio of graphene oxide, composite catalyst, sodium alginate, and PVA is 1:10:10:50, and the concentration of PVA is 8% (w / v).

[0058] 5. Weigh a certain amount of anhydrous calcium chloride and boric acid to prepare a mixed solution C of 20g / L and 30g / L; weigh a certain amount of sodium sulfate to prepare a 1M solution D.

[0059] 6. Add the precursor solution dropwise into the mixed solution C, gently stir for 20 minutes, take it out and place it in solution D and continue stirring for 2 hours. Take it out and wash it to form hydrogel balls containing the catalyst.

[0060] 7. Figure 2 These are optical photographs and scanning electron microscope images of the hydrogel balls containing the catalyst in this example. It can be seen that the catalyst is evenly dispersed inside the three-dimensional gel balls and forms a special macroporous structure, which provides a large-aperture channel for water purification and improves the adsorption characteristics.

[0061] 8. Figure 3 This is a comparison of the hydrogel balls containing catalysts before and after photocatalytic degradation of wastewater in this example. As can be seen from the figure, it is explained that the composite of graphene and titanium oxide greatly improves the utilization efficiency of visible light, and can degrade organic pollutants in the original wastewater under visible light conditions.

[0062] Embodiment three:

[0063] Reference Figure 1 , a method for preparing a graphene-based hydrogel spherical catalytic material, comprising the following steps:

[0064] 1. Dissolve PVA in deionized water at 94°C with stirring to form an 8% (w / v) PVA aqueous solution;

[0065] 2. Weigh a certain amount of sodium alginate and dissolve it in the above PVA aqueous solution to form a mixed solution A, where the mass ratio of sodium alginate to PVA is 1:5.

[0066] 3. Weigh a certain amount of TiO2 (Aladdin Reagent (Shanghai) Co., Ltd.) and ultrasonically disperse it in deionized water to form a mixed solution B.

[0067] 4. Mix the mixed solutions A and B, add a certain amount of deionized water, and stir evenly to form a precursor dispersion. At this time, the mass ratio of TiO2, sodium alginate, and PVA is 10:10:50, and the concentration of PVA is 8% (w / v).

[0068] 5. Weigh a certain amount of anhydrous calcium chloride and boric acid to prepare a mixed solution C of 20g / L and 30g / L; weigh a certain amount of sodium sulfate to prepare a 1M solution D.

[0069] 6. Add the precursor solution dropwise into the mixed solution C, gently stir for 20 minutes, take it out and place it in solution D and continue stirring for 2 hours. Take it out and wash it to form hydrogel balls containing the catalyst.

[0070] 7. Figure 3 This is a comparison of the hydrogel balls containing catalysts before and after the photocatalytic degradation of wastewater in this example. As can be seen from the figure, the composite of graphene and titanium oxide greatly improves the utilization efficiency of visible light, and can produce degradation of organic pollutants in the original wastewater under visible light conditions.

[0071] Embodiment 4:

[0072] Reference Figure 1 , a method for preparing a graphene-based hydrogel spherical catalytic material, comprising the following steps:

[0073] 1. Dissolve PVA in deionized water at 94°C with stirring to form a 10% (w / v) PVA aqueous solution;

[0074] 2. Weigh a certain amount of sodium alginate and dissolve it in the above PVA aqueous solution to form a mixed solution A, where the mass ratio of sodium alginate to PVA is 1:10.

[0075] 3. Weigh a certain amount of graphene oxide and graphene-titanium oxide composite catalyst and ultrasonically disperse them in deionized water to form a mixed solution B, where the mass ratio of graphene oxide to catalyst is 1:5.

[0076] 4. Mix the mixed solutions A and B, add a certain amount of deionized water, and stir evenly to form a precursor dispersion. At this time, the mass ratio of graphene oxide, composite catalyst, sodium alginate, and PVA is 1:5:10:50, and the concentration of PVA is 8% (w / v).

[0077] 5. Weigh a certain amount of anhydrous calcium chloride and boric acid to prepare a mixed solution C of 20g / L and 30g / L; weigh a certain amount of sodium sulfate to prepare a 1M solution D.

[0078] 6. Add the precursor solution dropwise into the mixed solution C, gently stir for 20 minutes, take it out and place it in solution D and continue stirring for 2 hours. Take it out and wash it to form hydrogel balls containing the catalyst.

[0079] 7. Figure 2 These are optical photographs and scanning electron microscope images of the hydrogel balls containing the catalyst in this example. It can be seen that the catalyst is evenly dispersed inside the three-dimensional gel balls and forms a special macroporous structure, which provides a large-aperture channel for water purification and improves the adsorption characteristics.

[0080] 8. Figure 3 This is a comparison of the hydrogel balls containing catalysts before and after photocatalytic degradation of wastewater in this example. As can be seen from the figure, it is explained that the composite of graphene and titanium oxide greatly improves the utilization efficiency of visible light, and can degrade organic pollutants in the original wastewater under visible light conditions.

[0081] Embodiment five:

[0082] Reference Figure 1 , a method for preparing a graphene-based hydrogel spherical catalytic material, comprising the following steps:

[0083] 1. Dissolve PVA in deionized water at 94°C with stirring to form a 10% (w / v) PVA aqueous solution;

[0084] 2. Weigh a certain amount of sodium alginate and dissolve it in the above PVA aqueous solution to form a mixed solution A, where the mass ratio of sodium alginate to PVA is 1:5.

[0085] 3. Weigh a certain amount of graphene oxide and graphene-titanium oxide composite catalyst and ultrasonically disperse them in deionized water to form a mixed solution B, where the mass ratio of graphene oxide to catalyst is 1:10.

[0086] 4. Mix the mixed solutions A and B, add a certain amount of deionized water, and stir evenly to form a precursor dispersion. At this time, the mass ratio of graphene oxide, composite catalyst, sodium alginate, and PVA is 1:10:5:25, and the concentration of PVA is 8% (w / v).

[0087] 5. Weigh a certain amount of anhydrous calcium chloride and boric acid to prepare a mixed solution C of 20g / L and 30g / L; weigh a certain amount of sodium sulfate to prepare a 1M solution D.

[0088] 6. Add the precursor solution dropwise into the mixed solution C, gently stir for 20 minutes, take it out and place it in solution D and continue stirring for 2 hours. Take it out and wash it to form hydrogel balls containing the catalyst.

[0089] 7. Figure 2 These are optical photographs and scanning electron microscope images of the hydrogel balls containing the catalyst in this example. It can be seen that the catalyst is evenly dispersed inside the three-dimensional gel balls and forms a special macroporous structure, which provides a large-aperture channel for water purification and improves the adsorption characteristics.

[0090] 8. Figure 3 This is a comparison of the hydrogel balls containing catalysts before and after photocatalytic degradation of wastewater in this example. As can be seen from the figure, it is explained that the composite of graphene and titanium oxide greatly improves the utilization efficiency of visible light, and can degrade organic pollutants in the original wastewater under visible light conditions.

Claims

1. A graphene-based hydrogel spherical catalytic material, characterized in that: The method comprises adding graphene oxide and graphene-titanium oxide composite catalyst solution into sodium alginate polyvinyl alcohol solution to obtain a precursor solution; The precursor solution is added dropwise into a calcium chloride boric acid solution, and after the spherical gel is formed, it is transferred into a sodium sulfate solution to obtain catalyst-containing hydrogel spheres.

2. The method for preparing the graphene-based hydrogel spherical catalytic material according to claim 1, characterized in that: The specific production steps are: (1) Preparing a precursor solution: mixing a polyvinyl alcohol sodium alginate solution with a mixed solution containing graphene oxide and a graphene-titanium oxide composite catalyst to obtain a precursor solution; (2) Preparation of spherical gel: adding the precursor solution dropwise into the calcium chloride boric acid solution to react and obtain a spherical gel; (3) Preparation of graphene-based hydrogel spherical catalytic material: adding the spherical gel into a sodium sulfate solution and allowing the reaction to fully proceed, then taking out and washing to obtain a graphene-based hydrogel spherical catalytic material.

3. The method for preparing the graphene-based hydrogel spherical catalytic material according to claim 2, characterized in that: In the polyvinyl alcohol sodium alginate solution, the mass volume concentration of polyvinyl alcohol is 3-15%, and the mass ratio of sodium alginate to polyvinyl alcohol is 1:4-15.

4. The method for preparing the graphene-based hydrogel spherical catalytic material according to claim 2, characterized in that: The mass ratio of graphene oxide, graphene-titanium oxide composite catalyst and polyvinyl alcohol is 1:5-40:40-80.

5. The method for preparing the graphene-based hydrogel spherical catalytic material according to claim 2, characterized in that: The concentration of calcium chloride in the calcium chloride boric acid solution is 20 g / L, and the concentration of boric acid is 30 g / L.

6. The method for preparing the graphene-based hydrogel spherical catalytic material according to claim 2, characterized in that: The concentration of the sodium sulfate solution is 1M.

7. Use of the graphene-based hydrogel spherical catalytic material according to claim 1 in the degradation and treatment of organic pollutants in water.

8. The use according to claim 7, characterized in that: The graphene-based hydrogel catalytic material is placed in a photodegradation device and directly poured into wastewater containing organic pollutants for treatment.

9. The use according to claim 7, characterized in that: The organic pollutants are one or more of dyes, animal and plant oils, and antibiotics, and the mass concentration is 0-100 mg / L and is not equal to 0.