A method for preparing magnesium oxide

Through the desulfurization reaction of magnesium sulfate and calcium nitrate and the concentration crystallization roasting process, the problem of low magnesium oxide purity is solved, the preparation of high-purity magnesium oxide and the recycling of resources are realized, and the production cost and environmental pollution are reduced.

CN116282092BActive Publication Date: 2024-11-19CHINA ENFI ENG CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310328304.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-11-19
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

In the existing magnesium oxide preparation process, magnesium oxide has low purity and consumes a large amount of acid and alkali raw materials, resulting in high production costs and high environmental pollution.

Method used

By mixing the aqueous magnesium sulfate solution with the aqueous calcium nitrate solution for desulfurization, an aqueous magnesium nitrate solution with impurities and an impurity-containing calcium sulfate residue was obtained. Then, it was concentrated and crystallized and calcined to obtain high-purity magnesium oxide and recovered through neutralization reaction. Recycled calcium nitrate aqueous solution.

Benefits of technology

The high purity preparation of magnesium oxide is achieved, the production process is simplified, the cost is reduced, the waste liquid and waste residue is reduced, and the production efficiency and purity is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116282092B_ABST
    Figure CN116282092B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing magnesium oxide. The preparation method comprises: step S1, mixing a magnesium sulfate aqueous solution and a calcium nitrate aqueous solution and performing a desulfurization reaction to obtain a magnesium nitrate aqueous solution from which impurities are removed and a calcium sulfate slag containing impurities; step S2, concentrating and crystallizing the magnesium nitrate aqueous solution to obtain a magnesium nitrate slurry, filtering the magnesium nitrate slurry to obtain magnesium nitrate crystals; step S3, roasting the magnesium nitrate crystals to obtain nitrogen dioxide gas and magnesium oxide. The present application uses magnesium sulfate as a raw material, and the solubility of magnesium sulfate and the intermediate product magnesium nitrate is relatively high, so that a large amount of magnesium oxide can be purified in a unit production volume of a leaching device, thereby obtaining a higher yield. At the same time, the leaching selectivity of calcium nitrate is good, and a relatively pure magnesium nitrate solution can be obtained, and the precipitation of calcium sulfate is good and the solubility is low, and most of the calcium ions will precipitate and will not be mixed into the magnesium nitrate, and the magnesium oxide finally prepared has a high purity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic chemical industry, and in particular to a method for preparing magnesium oxide. Background Art

[0002] The general process of preparing magnesium oxide using magnesium sulfate obtained by leaching serpentine tailings with strong acids such as sulfuric acid or magnesium sulfate waste liquid produced in other mines is: adding alkali or carbonate to precipitate magnesium ions to prepare magnesium hydroxide or magnesium carbonate, and thermally decomposing magnesium carbonate to obtain magnesium oxide. However, the magnesium oxide produced in this process has low purity and consumes a large amount of acid and alkali raw materials, which cannot be recycled. Not only is the cost high, but the acid leaching residue is also highly acidic, which still pollutes the environment greatly.

[0003] The Chinese patent with publication number CN102079533A discloses a process for preparing basic magnesium carbonate and high-purity magnesium oxide using natural alkali, which has the advantages of sufficient raw materials and low production cost, and has a strong competitive advantage in the production of high-purity magnesium oxide. However, due to the strong alkalinity of lime milk raw materials, it is very easy to react with CO in the process medium. 2 , HCO 3 -、CO 3 2- ; Calcium carbonate is generated and brought into MgO in the form of solid impurities, seriously affecting the purity and application range of MgO. Summary of the invention

[0004] The main purpose of the present invention is to provide a method for preparing magnesium oxide to solve the problem of low purity of magnesium oxide prepared in the prior art.

[0005] In order to achieve the above-mentioned object, according to one aspect of the present invention, there is provided a method for preparing magnesium oxide, the method comprising: step S1, mixing an aqueous magnesium sulfate solution and an aqueous calcium nitrate solution and carrying out a desulfurization reaction to obtain an aqueous magnesium nitrate solution from which impurities are removed and an impurity-containing calcium sulfate slag; step S2, concentrating and crystallizing the aqueous magnesium nitrate solution to obtain a magnesium nitrate slurry, filtering the magnesium nitrate slurry to obtain magnesium nitrate crystals; step S3, roasting the magnesium nitrate crystals to obtain nitrogen dioxide gas and magnesium oxide.

[0006] Furthermore, in step S1, the magnesium content in the magnesium sulfate solution is 10 to 80 g / L, and the concentration of the calcium nitrate aqueous solution is preferably 1 to 3 mol / L.

[0007] Furthermore, in step S1, the molar ratio of magnesium sulfate in the magnesium sulfate aqueous solution to calcium nitrate in the calcium nitrate aqueous solution is 1:1 to 1:2.

[0008] Furthermore, in step S1, stirring is performed while the desulfurization reaction is carried out, and the stirring speed is 150-200 r / min.

[0009] Furthermore, in step S1, the temperature of the desulfurization reaction is 20 to 35°C, and the desulfurization reaction time is preferably 0.5 to 2 hours.

[0010] Furthermore, step S1 comprises: adding a calcium nitrate aqueous solution into a magnesium sulfate aqueous solution for mixing and performing a desulfurization reaction to obtain a magnesium nitrate aqueous solution from which impurities have been removed and a calcium sulfate slag containing impurities; preferably, the calcium nitrate aqueous solution is added for 1 to 30 minutes, more preferably for 5 to 15 minutes.

[0011] Furthermore, in step S2, the temperature of concentrated crystallization is 80-120°C, and the water content of the magnesium nitrate slurry is preferably 50-80%.

[0012] Furthermore, in step S3, the calcination temperature is 300-600° C., and the calcination time is preferably 1-4 hours.

[0013] Furthermore, the purity of magnesium oxide is 98% or more.

[0014] Furthermore, in step S2, condensed water is produced during the concentration and crystallization process, and the preparation method also includes: neutralizing the calcium sulfate slag in step S1, part of the condensed water in step S2, and the nitrogen dioxide gas in step S3 to obtain a regenerated calcium nitrate aqueous solution, and returning the regenerated calcium nitrate aqueous solution to step S1 for recycling as at least part of the calcium nitrate aqueous solution.

[0015] Applying the technical scheme of the present invention, the preparation method of the present application is simple, the production cycle is short and the productivity is high. Compared with magnesium bicarbonate commonly used in the prior art, the present application uses magnesium sulfate as a raw material, and the solubility of magnesium sulfate and the intermediate product magnesium nitrate is relatively high, and a large amount of magnesium oxide can be purified in the unit production volume of the leaching equipment, thereby obtaining a higher yield. At the same time, the leaching selectivity of calcium nitrate is good, and impurity ions will not be leached, and a relatively pure magnesium nitrate solution can be obtained, and the precipitation of calcium sulfate is good, and the solubility is low, and most of the calcium ions will precipitate and will not be mixed in magnesium nitrate, so the magnesium oxide finally prepared has a higher purity. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0017] Figure 1 The flowchart of preparing magnesium oxide according to Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0019] As analyzed in the background art, the magnesium oxide prepared in the prior art has the problem of low purity. In order to solve this problem, the present application provides a method for preparing magnesium oxide.

[0020] In a typical embodiment of the present application, a method for preparing magnesium oxide is provided, such as Figure 1 As shown, the preparation method includes: step S1, mixing a magnesium sulfate aqueous solution and a calcium nitrate aqueous solution and performing a desulfurization reaction to obtain a magnesium nitrate aqueous solution from which impurities are removed and a calcium sulfate slag containing impurities; step S2, concentrating and crystallizing the magnesium nitrate aqueous solution to obtain a magnesium nitrate slurry, filtering the magnesium nitrate slurry to obtain magnesium nitrate crystals; step S3, roasting the magnesium nitrate crystals to obtain nitrogen dioxide gas and magnesium oxide.

[0021] The present invention uses magnesium sulfate as raw material and calcium nitrate as precipitant to carry out desulfurization reaction to obtain magnesium nitrate solution. The reaction formula of the desulfurization reaction is: MgSO 4 +Ca(NO 3 ) 2 →Mg(NO 3 ) 2 +CaSO 4 ↓, filter to obtain magnesium nitrate solution and calcium slag (gypsum); then concentrate the magnesium nitrate solution, crystallize and roast to obtain nitrogen dioxide and magnesium oxide; the reaction during the roasting process is: 2Mg(NO 3 ) 2 →2MgO+4NO 2 ↑+O 2 ↑.

[0022] The preparation method of the present application is simple, has a short production cycle and high productivity. Compared with magnesium bicarbonate commonly used in the prior art, the present application uses magnesium sulfate as a raw material, and the solubility of magnesium sulfate and the intermediate product magnesium nitrate is relatively high, and a large amount of magnesium oxide can be purified in the unit production volume of the leaching equipment, thereby obtaining a higher yield. At the same time, the leaching selectivity of calcium nitrate is good, and impurity ions will not be leached, and a relatively pure magnesium nitrate solution can be obtained, and the precipitation of calcium sulfate is good, and the solubility is low, and most of the calcium ions will precipitate and will not be mixed in magnesium nitrate, so the magnesium oxide finally prepared has a higher purity.

[0023] In order to purify more magnesium oxide per unit volume, in some embodiments, in step S1, the magnesium content in the magnesium sulfate solution is 10-80 g / L, and in order to make the calcium ions in the calcium nitrate, the concentration of the calcium nitrate aqueous solution is preferably 1-3 mol / L.

[0024] In order to allow magnesium sulfate and calcium nitrate solution to react fully, in some embodiments, in step S1, the molar ratio of magnesium sulfate in the magnesium sulfate aqueous solution to calcium nitrate in the calcium nitrate aqueous solution is 1:1 to 1:2. The calcium nitrate aqueous solution can be slightly excessive so that magnesium sulfate is completely converted into magnesium nitrate solution. However, in order for the calcium ions in the calcium nitrate to precipitate and not mix into the magnesium nitrate during the reaction, the calcium nitrate content cannot be too much.

[0025] In order to allow the magnesium sulfate solution and the calcium nitrate solution to fully contact and react, in some embodiments, in step S1, stirring is performed while the desulfurization reaction is carried out, and the stirring speed is 150-200 r / min.

[0026] The present application has no particular restriction on the temperature of the desulfurization reaction, and the reaction can be carried out at room temperature. In some embodiments, in step S1, the temperature of the desulfurization reaction is 20 to 35°C, and the present application has no particular restriction on the time of the desulfurization reaction, which can be determined according to the precipitation formation during the reaction process, and the preferred time of the desulfurization reaction is 0.5 to 2 hours.

[0027] In some embodiments, a calcium nitrate aqueous solution is added to a magnesium sulfate aqueous solution for mixing and performing a desulfurization reaction to obtain a magnesium nitrate aqueous solution from which impurities have been removed and a calcium sulfate slag containing impurities; when performing the desulfurization reaction, the calcium nitrate aqueous solution is preferably added to the magnesium sulfate aqueous solution to fully precipitate calcium ions. The calcium nitrate aqueous solution is preferably added for 1 to 30 minutes, more preferably for 5 to 15 minutes.

[0028] The present application has no particular restrictions on the conditions for concentrated crystallization, as long as the water can be evaporated. In some embodiments, in step S2, the temperature for concentrated crystallization is 80-120°C, and the water content of the magnesium nitrate slurry is preferably 50-80%. The water content of the magnesium nitrate slurry within this range is helpful for actual operation and roasting process to ensure product quality.

[0029] The present application has no particular limitation on the filtering method, and any commonly used filtering method in the art can be applied to the present application, for example, suction filtration, pressure filtration, etc.

[0030] In some embodiments, in step S3, the calcination temperature is 300-600° C., and the calcination time is preferably 1-3 hours. Under this calcination condition, magnesium nitrate can be converted into magnesium oxide. If the calcination temperature is too high, the properties of MgO will be changed. If the calcination temperature is too low, N will remain, thereby affecting the purity of MgO.

[0031] The magnesium oxide prepared in the present application has a relatively high purity. In some embodiments, the purity of the magnesium oxide is above 98%.

[0032] In some embodiments, in step S2, condensed water is produced during the concentration and crystallization process, and the preparation method further comprises: neutralizing the calcium sulfate slag in step S1, part of the condensed water in step S2, and the nitrogen dioxide gas in step S3 to obtain a regenerated calcium nitrate aqueous solution, and returning the regenerated calcium nitrate aqueous solution to step S1 as at least part of the calcium nitrate aqueous solution for recycling. The intermediate products calcium slag and nitrogen dioxide can be recycled, theoretically without loss, which can greatly reduce costs; at the same time, no waste liquid or waste residue is generated during the entire reaction process, and energy consumption is low.

[0033] The calcium slag that has been recycled for a long time can also be washed to remove impurities to obtain regenerated raw gypsum.

[0034] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0035] Example 1

[0036] like Figure 1 As shown in the flow chart, 40 g / L magnesium sulfate solution and 1 mol / L calcium nitrate solution are first prepared, and the calcium nitrate and magnesium sulfate solution are measured at a molar ratio of 1:1, and then the calcium nitrate solution is added to the magnesium sulfate solution for 5 minutes. At room temperature (25°C), the desulfurization reaction is stirred for 0.5 hours at a stirring speed of 180 r / min, filtered, evaporated and concentrated at 100°C to a water content of 60%, and filtered to obtain Mg(NO 3 ) 2 crystals; then calcined at 400°C for 3 hours to obtain magnesium oxide with a purity of 98.9%.

[0037] Example 2

[0038] Prepare 40g / L magnesium sulfate solution and 1mol / L calcium nitrate solution, measure calcium nitrate and magnesium sulfate solution with a molar ratio of 1:1, and then add the calcium nitrate solution to the magnesium sulfate solution for 5 minutes. Stir and carry out desulfurization reaction for 0.5h at room temperature (25°C) at a stirring speed of 180r / min, filter, evaporate and concentrate at 100°C to a water content of 80%, and filter to obtain Mg(NO 3 ) 2 Crystals; then calcined at 350°C for 3 hours to obtain magnesium oxide with a purity of 98.2%.

[0039] Example 3

[0040] Prepare 40g / L magnesium sulfate solution and 3mol / L calcium nitrate solution, measure calcium nitrate and magnesium sulfate solution with a molar ratio of 1:1, and then add the calcium nitrate solution to the magnesium sulfate solution for 10 minutes. Stir and carry out desulfurization reaction for 0.5h at room temperature (25°C) at a stirring speed of 180r / min, filter, evaporate and concentrate at 100°C to a water content of 80%, and filter to obtain Mg(NO 3 ) 2 Crystallization; then calcination at 350°C for 4 hours to obtain magnesium oxide with a purity of 98.6%.

[0041] Example 4

[0042] Prepare 10g / L magnesium sulfate solution and 1mol / L calcium nitrate solution, measure calcium nitrate and magnesium sulfate solution with a molar ratio of 1:2, and then add the calcium nitrate solution to the magnesium sulfate solution for 1 minute. Stir and carry out desulfurization reaction for 2 hours at room temperature (20°C) at a stirring speed of 150r / min, filter, evaporate and concentrate at 80°C to a water content of 50%, and filter to obtain Mg(NO 3 ) 2 crystals; then calcined at 300°C for 1 hour to obtain magnesium oxide with a purity of 99.3%.

[0043] Example 5

[0044] Prepare 80g / L magnesium sulfate solution and 2mol / L calcium nitrate solution, measure calcium nitrate and magnesium sulfate solution with a molar ratio of 1:1, and then add the calcium nitrate solution to the magnesium sulfate solution for 30 minutes. Stir and carry out desulfurization reaction for 1 hour at room temperature (35°C) at a stirring speed of 200r / min, filter, evaporate and concentrate at 120°C to a water content of 60%, and filter to obtain Mg(NO 3 ) 2 crystals; and then calcined at 600°C for 3 hours to obtain magnesium oxide with a purity of 98.2%.

[0045] Example 6

[0046] Different from Example 1, the concentration of the magnesium sulfate solution is 90 g / L.

[0047] Example 7

[0048] Different from Example 1, the concentration of the magnesium sulfate solution is 5 g / L.

[0049] Example 8

[0050] The difference from Example 1 is that the concentration of calcium nitrate is 0.5 mol / L.

[0051] Example 9

[0052] The difference from Example 1 is that the concentration of calcium nitrate is 3.5 mol / L.

[0053] Example 10

[0054] The difference from Example 1 is that the evaporation concentration is performed to a water content of 45%.

[0055] Embodiment 11

[0056] The difference from Example 1 is that the calcination temperature is 650°C.

[0057] Example 12

[0058] Prepare 40g / L magnesium sulfate solution and 3mol / L calcium nitrate solution, measure calcium nitrate and magnesium sulfate solution with a molar ratio of 1:1, and then add the calcium nitrate solution to the magnesium sulfate solution for 5 minutes. Stir and carry out desulfurization reaction for 0.5h at room temperature (25°C) at a stirring speed of 180r / min, filter, evaporate and concentrate to a water content of 120%, and filter to obtain Mg(NO 3 ) 2 Crystallization; then calcination at 300°C for 2 hours to obtain magnesium oxide with a purity of 97.2%.

[0059] Comparative Example 1

[0060] The difference from Example 1 is that the precipitant is 1 mol / L calcium chloride.

[0061] The purity of the magnesium oxide prepared in the above embodiments and comparative examples is shown in Table 1.

[0062] Table 1

[0063]

[0064]

[0065] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0066] The preparation method of the present application is simple, has a short production cycle and high productivity. Compared with magnesium bicarbonate commonly used in the prior art, the present application uses magnesium sulfate as a raw material, and the solubility of magnesium sulfate and the intermediate product magnesium nitrate is relatively high, and a large amount of magnesium oxide can be purified in the unit production volume of the leaching equipment, thereby obtaining a higher yield. At the same time, the leaching selectivity of calcium nitrate is good, and impurity ions will not be leached, and a relatively pure magnesium nitrate solution can be obtained, and the precipitation of calcium sulfate is good, and the solubility is low, and most of the calcium ions will precipitate and will not be mixed in magnesium nitrate, so the magnesium oxide finally prepared has a higher purity.

[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing magnesium oxide, characterized in that: The preparation method comprises: Step S1, mixing a magnesium sulfate aqueous solution and a calcium nitrate aqueous solution and performing a desulfurization reaction to obtain a magnesium nitrate aqueous solution from which impurities are removed and a calcium sulfate slag containing impurities; Step S2, concentrating and crystallizing the magnesium nitrate aqueous solution to obtain magnesium nitrate slurry, and filtering the magnesium nitrate slurry to obtain magnesium nitrate crystals; Step S3, roasting the magnesium nitrate crystals to obtain nitrogen dioxide gas and the magnesium oxide; The magnesium content in the magnesium sulfate aqueous solution is 10-80 g / L; The water content of the magnesium nitrate slurry is 50-80%; The step S1 comprises: The calcium nitrate aqueous solution is added to the magnesium sulfate aqueous solution for mixing and performing a desulfurization reaction to obtain a magnesium nitrate aqueous solution from which impurities are removed and a calcium sulfate slag containing impurities; The calcium nitrate aqueous solution is added for 1 to 30 minutes; The purity of the magnesium oxide is above 98%.

2. The preparation method according to claim 1, characterized in that: In step S1, the concentration of the calcium nitrate aqueous solution is 1-3 mol / L.

3. The preparation method according to claim 1 or 2, characterized in that: In the step S1, the molar ratio of magnesium sulfate in the magnesium sulfate aqueous solution to calcium nitrate in the calcium nitrate aqueous solution is 1:1 to 1:

2.

4. The preparation method according to claim 1 or 2, characterized in that: In the step S1, stirring is performed while the desulfurization reaction is carried out, and the stirring speed is 150-200 r / min.

5. The preparation method according to claim 1 or 2, characterized in that: In step S1, the temperature of the desulfurization reaction is 20-35°C.

6. The preparation method according to claim 1 or 2, characterized in that: The desulfurization reaction time is 0.5~2h.

7. The preparation method according to claim 1 or 2, characterized in that: The calcium nitrate aqueous solution is added for 5 to 15 minutes.

8. The preparation method according to claim 1 or 2, characterized in that: In the step S2, the temperature of the concentrated crystallization is 80-120°C.

9. The preparation method according to claim 1 or 2, characterized in that: In the step S3, the calcination temperature is 300-600°C.

10. The preparation method according to claim 1 or 2, characterized in that: The calcination time is 1 to 4 hours.

11. The preparation method according to claim 1 or 2, characterized in that: In the step S2, condensed water is produced during the concentration and crystallization process, and the preparation method further comprises: The calcium sulfate slag in step S1, part of the condensed water in step S2, and the nitrogen dioxide gas in step S3 are subjected to a neutralization reaction to obtain a regenerated calcium nitrate aqueous solution, and the regenerated calcium nitrate aqueous solution is returned to step S1 as at least part of the calcium nitrate aqueous solution for recycling.