A method for producing industrial calcium chloride using rare earth smelting high-salt wastewater
Through multi-step treatment of high-salt wastewater from rare earth smelting and the use of technologies such as lime slurry and flocculants, the problem of waste of calcium chloride resources and environmental pollution in rare earth smelting wastewater has been successfully solved, and the production and resource recycling of high-purity calcium chloride have been achieved. , improving process safety and efficiency.
Patent Information
- Application Number
- CN202211692818.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-28
AI Technical Summary
The high-concentration calcium chloride and high-salt wastewater generated during the rare earth smelting process will lead to waste of resources and environmental pollution if it is directly treated to meet the standards. The traditional evaporation concentration process has high impurity concentrations, which limits the application scope of calcium chloride.
Calcium chloride is recovered from high-salt wastewater from rare earth smelting, and technical steps such as lime slurry neutralization, calcium polysulfide co-precipitation, electroflocculation and PAM flocculation are used to achieve the production of high-purity calcium chloride, including lime slurry adjustment of pH to precipitate magnesium ions, Multi-step treatment such as polyacrylamide flocculation, electrocoagulation and calcium carbonate sand filtration removes heavy metals and radioactive elements, and finally obtains industrial grade calcium chloride through MVR evaporation and concentration.
It achieves the production of high-purity calcium chloride, avoids heavy metal and radioactive pollution, promotes resource recycling, reduces environmental pollution, and improves process safety and production efficiency.
Smart Images

Figure CN116282118B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical preparation field of industrial calcium chloride, and particularly relates to a method for producing industrial calcium chloride by utilizing rare earth metallurgical high-salt wastewater. Background Art
[0002] In the process of rare earth smelting and separation, the organic phase is usually first subjected to saponification treatment to form an alkaline metal ion-loaded organic phase that is more difficult to extract than rare earths, and then undergoes an extraction exchange reaction with a rare earth chloride solution to form an organic phase loaded with rare earth ions. The currently more mature calcium saponification, magnesium saponification, and lime-to-ammonia saponification processes will produce high-concentration calcium chloride high-salt wastewater in the saponification process or the supporting saponification process. As an important industrial salt, calcium chloride is not only a waste of resources but also has a certain impact on the environment if it is directly treated and discharged in compliance with the standards. The calcium chloride crystals produced by the traditional direct evaporation and concentration process are severely restricted in their application scope due to the high impurity concentration, and individual indicators that do not meet the standards may also cause environmental pollution.
[0003] Invention patent CN201910813191.6 discloses a method for treating rare earth industrial wastewater. For the acidic wastewater containing calcium chloride generated in the rare earth extraction and separation process, activated carbon and other adsorbents are used for adsorption and oil removal, and concentrated sulfuric acid is used as a calcium precipitation agent. Anionic surfactants are added for precipitation and calcium removal. The solution after calcium removal is eutectic precipitated with barium chloride to remove Mg in the solution. 2+ , Mn 2+ and radioactive elements, etc., and the impurities such as residual aluminum and rare earth ions are removed by sand filtration using iron alum sand as a purifier, and then pure acid is obtained to return to the rare earth ingredients or to prepare concentrated acid. However, when using activated carbon to adsorb oily substances in wastewater, the solid waste generated after activated carbon adsorbs organic matter belongs to the national hazardous waste list. Subsequent treatment is generally carried out by qualified units for incineration, and there are environmental risks during transportation and incineration. In addition, the purchase of activated carbon, the loss of extraction agents, and the cost of outsourcing treatment all cause burdens to enterprises, which is not conducive to large-scale promotion. Summary of the invention
[0004] Aiming at the problem that high-concentration calcium chloride and high-salt wastewater is generated in the existing rare earth smelting process, and the direct treatment and discharge after reaching the standard causes waste of resources and further pollution to the environment, the present invention provides a method for producing industrial calcium chloride by utilizing high-salt wastewater from rare earth smelting, which directly utilizes the wastewater generated in the rare earth smelting process to recycle calcium chloride and produce high-purity industrial calcium chloride, thereby promoting the recycling of resources, reducing waste of resources and reducing pollution to the environment.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for producing industrial calcium chloride using rare earth smelting high-salt wastewater comprises the following steps:
[0007] (1) Take the wastewater from rare earth smelting extraction and separation, add lime slurry to adjust the pH to 9.5-11, and obtain a neutralized solution;
[0008] (2) The neutralized liquid is transferred to a thickening tank for clarification, and the bottom mud is pumped to a plate and frame filter press for filtration to form a neutralized residue; the supernatant is transferred to a decontamination reaction tank, and a calcium polysulfide aqueous solution of 1-5 times the amount of heavy metals is added, and then 50-500g / m 3 adding an aqueous solution of barium chloride to carry out a co-precipitation reaction;
[0009] (3) The impurity removal liquid after the co-precipitation reaction is pumped to the thickening tank for clarification. Before the impurity removal liquid enters the thickening tank, a polyacrylamide solution with a mass concentration of 0.15% is added to the impurity removal liquid at a ratio of 1%-5% of the impurity removal liquid volume through a pipeline mixer for flocculation. The clarified sludge in the thickening tank is pumped to a plate and frame filter press for filtration to form slag, and the supernatant is transferred to the electro-flocculation deep weight removal system;
[0010] (4) A direct current of 500-800A is applied to the anode and cathode plates of the electrocoagulation deweighting system for electrolytic flocculation. After the electrocoagulation liquid is discharged, it is adsorbed by PAM flocculant. The adsorbed scum is sent to a plate and frame filter press for filtration to form slag, and the clear liquid is transferred to a sand pool for filtration;
[0011] (5) Filtering the suspended matter through a 50-100 mesh calcium carbonate sand filter in a sand pool, adding hydrochloric acid to the sand filtrate to adjust the pH to 4-6, and then removing the heavy metal ions through adsorption by a leaching resin to obtain a leachate;
[0012] (6) The eluted liquid is slowly filtered through a 20-200 mesh calcium carbonate sand filter to obtain a calcium chloride solution, which is then concentrated to 50% by MVR evaporation and packaged to obtain an industrial calcium chloride product.
[0013] Preferably, the wastewater extracted and separated from rare earth smelting is one of the rare earth soap wastewater from the calcium saponification process, the alkali conversion wastewater from the magnesium saponification process, and the deaminated rare earth soap wastewater in the lime conversion-ammonia saponification process.
[0014] Preferably, before the reaction in step (1) is carried out on the wastewater obtained by extraction and separation of rare earth smelting, the magnesium ion content in the wastewater is analyzed and controlled to be ≥0.5%. If the magnesium ion content in the wastewater is <0.5%, magnesium chloride wastewater is added or light calcium oxide is added in the saponification process to make the magnesium ion content in the wastewater reach 0.5%-1%.
[0015] Preferably, the mixing time of the two phases in the pipeline mixer in step (3) is less than 2 s.
[0016] The invention uses wastewater rich in calcium chloride, such as rare earth soap wastewater from calcium saponification process in rare earth smelting extraction and separation with a magnesium ion concentration of ≥0.5%, alkali conversion wastewater from magnesium saponification process, and deaminated rare earth soap wastewater from lime conversion-ammonia saponification process, to prepare industrial-grade calcium chloride. First, lime slurry is added to a reaction tank to adjust the pH of the wastewater, so that the magnesium ions in the wastewater are completely precipitated to form magnesium hydroxide precipitates. While removing the magnesium ions, a small amount of organic matter in the wastewater is adsorbed and removed by active magnesium hydroxide precipitates, so as to achieve efficient oil removal and deoiling, and eliminate organic matter such as solvent oil in the wastewater that extracts heavy metals and other impurities to affect subsequent impurity removal and form foam to interfere with equipment operation; the treated neutralized liquid is sent to a thickening tank to separate the bottom mud, a calcium polysulfide aqueous solution is added to the supernatant to form a sulfide precipitate of heavy metals, and barium chloride is added to make radioactive elements co-precipitate with barium sulfate, and polyacrylamide is added to the liquid after impurity removal through a pipeline mixer to further flocculate heavy metal and radioactive element precipitates, and the pipeline mixer is used to mix the heavy metals and radioactive elements in the liquid. The mixing time of the two phases is less than 2s, which prevents the traditional stirring and mixing process from destroying the flocculant flocculant structure, thereby improving the flocculation effect; the treated supernatant is transferred to the electro-flocculation deep weight removal system, and the electro-flocculation method is used to make the heavy metal ions in the wastewater near the cathode undergo electrolytic reaction and oxidation to become high-valent compounds that are easy to precipitate, while the anode consumes the anode aluminum plate to form aluminum hydroxide floccules, and the heavy metal precipitates are enlarged particles; after the electro-flocculation liquid is discharged, it is adsorbed by PAM, and the adsorbed liquid is transferred to the sand pool and filtered by calcium carbonate sand to remove trace suspended matter; finally, hydrochloric acid is added to the calcium carbonate sand filtrate to adjust the pH to remove high-valent ions such as iron and aluminum, and the obtained elution is filtered by calcium carbonate sand, and the pH is stabilized by calcium carbonate balance. At the same time, the carbonate ions dissociated in the pH range and trace barium generate precipitated adsorbed ions, and the radioactive elements carried are further reduced. Finally, a high-purity calcium chloride solution is obtained, and an industrial-grade high-purity calcium chloride product can be obtained after evaporation and concentration.
[0017] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0018] 1. The present invention directly utilizes rare earth smelting high-salt wastewater to produce high-purity calcium chloride, which eliminates the heavy metal and radioactive pollution problems caused by the conventional high-salt wastewater concentration production method, promotes resource recycling, reduces resource waste, and reduces environmental pollution.
[0019] 2. The production process of the present invention utilizes lime slurry to precipitate magnesium ions, and at the same time utilizes magnesium precipitate to adsorb organic matter in wastewater to achieve the purpose of oil removal, thereby eliminating the organic matter in wastewater extracting heavy metals and other impurities that affect subsequent impurity removal and form foam to interfere with equipment operation, thereby improving the safety of the entire process flow and thus improving production efficiency.
[0020] 3. The present invention applies high direct current to the anode and cathode plates through the electrocoagulation method, so that the heavy metal ions in the wastewater undergo electrolytic reaction, oxidize into high-valent easily precipitated compounds, and consume the anode aluminum plate to form aluminum hydroxide precipitation. The heavy metal precipitates are flocculated to expand the particles, and finally the suspended precipitates are removed by adsorption using flocculants such as PAM, thereby achieving deep removal of heavy metal ions and improving the purity of the calcium chloride product. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with the accompanying drawings. Example 1
[0023] A method for producing industrial calcium chloride using rare earth smelting high-salt wastewater comprises the following steps:
[0024] (1) Take the rare earth soap wastewater from the calcium saponification process in the rare earth smelting extraction and separation, first analyze and control the magnesium ion content in the wastewater to ≥0.5%. If the magnesium ion content in the wastewater is <0.5%, add magnesium chloride wastewater or add light calcium oxide in the saponification process to make the magnesium ion content in the wastewater reach 0.5%-1%, and then add lime slurry to adjust the pH to 9.5 to obtain a neutralized solution;
[0025] (2) The neutralized liquid is transferred to a thickening tank for clarification, and the bottom mud is pumped to a plate and frame filter press for filtration to form a neutralized residue; the supernatant is transferred to an impurity removal reaction tank, and a calcium polysulfide aqueous solution with a 1-fold amount of heavy metals is added, and then 50 g / m 3 adding an aqueous solution of barium chloride to carry out a co-precipitation reaction;
[0026] (3) The impurity removal liquid after the co-precipitation reaction is pumped to the thickening tank for clarification. Before the impurity removal liquid enters the thickening tank, a polyacrylamide solution with a mass concentration of 0.15% is added to the impurity removal liquid at a ratio of 1% of the impurity removal liquid volume through a pipeline mixer for flocculation. The mixing time of the two phases in the pipeline mixer is less than 2s; the bottom sludge clarified in the thickening tank is pumped to a plate and frame filter press for filtration to form slag, and the supernatant is transferred to the electro-flocculation deep weight removal system;
[0027] (4) A direct current of 500-800A is applied to the anode and cathode plates of the electrocoagulation deweighting system for electrolytic flocculation. After the electrocoagulation liquid is discharged, it is adsorbed by PAM flocculant. The adsorbed scum is sent to a plate and frame filter press for filtration to form slag, and the clear liquid is transferred to a sand pool for filtration;
[0028] (5) Filtering the suspended matter through a 50-mesh calcium carbonate sand filter in a sand pool, adding hydrochloric acid to the sand filtrate to adjust the pH to 4, and then removing the heavy metal ions through adsorption by a leaching resin to obtain a leachate;
[0029] (6) The eluted liquid is slowly filtered through a 20-mesh calcium carbonate sand filter to obtain a calcium chloride solution, which is then concentrated to 50% by MVR evaporation and packaged to obtain an industrial calcium chloride product.
[0030] The physical and chemical indicators of the industrial calcium chloride product prepared in this embodiment are shown in Table 1.
[0031] Table 1 Physical and chemical indicators
[0032] Serial number project index 1 <![CDATA[Calcium chloride (CaCL2) content w / %]]> ≥50% (as needed) 2 <![CDATA[Alkalinity [calculated as Ca(OH2)] w / %]]> ≤0.20% 3 Total alkali metal chloride (as NaCl) w / % ≤5.0% 4 Water insoluble matter w / % ≤0.10% 5 Iron (Fe) w / % ≤0.004% 6 <![CDATA[Sulfate (calculated as CaSO4) w / %]]> ≤0.05% 7 <![CDATA[Total magnesium (calculated as MgCl2) w / %]]> ≤0.5% 8 pH(10 g / L) 6.0-11.0 9 Heavy metals (as Pb) w / % ≤0.002% 10 Lead (Pb) w / % ≤0.0005% 11 Arsenic (As) w / % ≤0.0003% Example 2
[0033] A method for producing industrial calcium chloride using rare earth smelting high-salt wastewater comprises the following steps:
[0034] (1) Take the alkali wastewater from the magnesium saponification process in rare earth smelting extraction and separation, first analyze and control the magnesium ion content in the wastewater to ≥0.5%. If the magnesium ion content in the wastewater is <0.5%, add magnesium chloride wastewater or add light calcium oxide in the saponification process to make the magnesium ion content in the wastewater reach 0.5%-1%, and then add lime slurry to adjust the pH to 11 to obtain a neutralized solution;
[0035] (2) The neutralized liquid is transferred to a thickening tank for clarification, and the bottom mud is pumped to a plate and frame filter press for filtration to form a neutralized residue; the supernatant is transferred to a decontamination reaction tank, and a calcium polysulfide aqueous solution 5 times the amount of heavy metals is added, and then 500g / m 3 adding an aqueous solution of barium chloride to carry out a co-precipitation reaction;
[0036] (3) The impurity removal liquid after the co-precipitation reaction is pumped to the thickening tank for clarification. Before the impurity removal liquid enters the thickening tank, a polyacrylamide solution with a mass concentration of 0.15% is added to the impurity removal liquid at a ratio of 5% of the impurity removal liquid volume through a pipeline mixer for flocculation. The mixing time of the two phases in the pipeline mixer is less than 2s; the bottom sludge clarified in the thickening tank is pumped to a plate and frame filter press for filtration to form slag, and the supernatant is transferred to the electro-flocculation deep weight removal system;
[0037] (4) A direct current of 800A is applied to the anode and cathode plates of the electro-flocculation deweighting system for electrolytic flocculation. After the electro-flocculation liquid is discharged, it is adsorbed by PAM flocculant. The adsorbed scum is sent to a plate and frame filter press for filtration to form slag, and the clear liquid is transferred to a sand pool for filtration;
[0038] (5) Filtering the suspended matter through a 100-mesh calcium carbonate sand filter in a sand pool, adding hydrochloric acid to the sand filtrate to adjust the pH to 4-6, and then removing the heavy metal ions through adsorption by a leaching resin to obtain a leachate;
[0039] (6) The eluted liquid is slowly filtered through a 200-mesh calcium carbonate sand filter to obtain a calcium chloride solution, which is then concentrated to 50% by MVR evaporation and packaged to obtain an industrial calcium chloride product. Example 3
[0040] A method for producing industrial calcium chloride using rare earth smelting high-salt wastewater comprises the following steps:
[0041] (1) Take the deaminated rare earth soap wastewater from the lime transformation-ammonia saponification process in rare earth smelting extraction and separation, first analyze and control the magnesium ion content in the wastewater to ≥0.5%. If the magnesium ion content in the wastewater is <0.5%, add magnesium chloride wastewater or add light calcium oxide in the saponification process to make the magnesium ion content in the wastewater reach 0.5%-1%, and then add lime slurry to adjust the pH to 10.0 to obtain a neutralized solution;
[0042] (2) The neutralized liquid is transferred to a thickening tank for clarification, and the bottom mud is pumped to a plate and frame filter press for filtration to form a neutralized residue; the supernatant is transferred to a decontamination reaction tank, and a calcium polysulfide aqueous solution 3 times the amount of heavy metals is added, and then 100g / m 3 adding an aqueous solution of barium chloride to carry out a co-precipitation reaction;
[0043] (3) The impurity removal liquid after the co-precipitation reaction is pumped to the thickening tank for clarification. Before the impurity removal liquid enters the thickening tank, a polyacrylamide solution with a mass concentration of 0.15% is added to the impurity removal liquid at a ratio of 2% through a pipeline mixer for flocculation. The mixing time of the two phases in the pipeline mixer is less than 2s; the bottom sludge clarified in the thickening tank is pumped to a plate and frame filter press for filtration to form slag, and the supernatant is transferred to the electro-flocculation deep weight removal system;
[0044] (4) A 650A direct current is applied to the anode and cathode plates of the electro-flocculation deweighting system for electrolytic flocculation. After the electro-flocculation liquid is discharged, it is adsorbed by PAM flocculant. The adsorbed scum is sent to a plate and frame filter press for filtration to form slag, and the clear liquid is transferred to a sand pool for filtration;
[0045] (5) Filtering the suspended solids through a 60-mesh calcium carbonate sand filter in a sand pool, adding hydrochloric acid to the sand filtrate to adjust the pH to 5.5, and then removing the heavy metal ions through adsorption by a leaching resin to obtain a leachate;
[0046] (6) The eluted liquid is slowly filtered through an 80-mesh calcium carbonate sand filter to obtain a calcium chloride solution, which is then concentrated to 50% by MVR evaporation and packaged to obtain an industrial calcium chloride product.
[0047] The above embodiments are only exemplary embodiments of the present invention and are not intended to limit the present invention. The protection scope of the present invention is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present invention, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present invention.
Claims
1. A method for producing industrial calcium chloride using rare earth smelting high-salt wastewater, characterized in that: The following steps are involved: (1) Take the wastewater from rare earth smelting extraction and separation, add lime slurry to adjust the pH to 9.5-11, and obtain a neutralized solution; The wastewater extracted and separated from rare earth smelting is one of the rare earth soap wastewater from the calcium saponification process, the alkali conversion wastewater from the magnesium saponification process, and the deaminated rare earth soap wastewater in the lime conversion-ammonia saponification process; (2) The neutralized liquid is transferred to a thickening tank for clarification, and the bottom mud is pumped to a plate and frame filter press for filtration to form a neutralized residue; the supernatant is transferred to a decontamination reaction tank, and a calcium polysulfide aqueous solution of 1-5 times the amount of heavy metals is added, and then 50-500g / m 3 adding an aqueous solution of barium chloride to carry out a co-precipitation reaction; (3) The impurity removal liquid after the co-precipitation reaction is pumped to the thickening tank for clarification. Before the impurity removal liquid enters the thickening tank, a polyacrylamide solution with a mass concentration of 0.15% is added to the impurity removal liquid at a ratio of 1%-5% of the impurity removal liquid volume through a pipeline mixer for flocculation. The clarified sludge in the thickening tank is pumped to a plate and frame filter press for filtration to form slag, and the supernatant is transferred to the electro-flocculation deep weight removal system; (4) A direct current of 500-800A is applied to the anode and cathode plates of the electro-flocculation deweighting system for electrolytic flocculation. After the electro-flocculation liquid is discharged, it is adsorbed by PAM flocculant. The adsorbed scum is sent to a plate and frame filter press for filtration to form slag, and the clear liquid is transferred to a sand pool for filtration; (5) Filtering the suspended matter through a 50-100 mesh calcium carbonate sand filter in a sand pool, adding hydrochloric acid to the sand filtrate to adjust the pH to 4-6, and then removing the heavy metal ions through adsorption by a leaching resin to obtain a leachate; (6) The eluted liquid is slowly filtered through a 20-200 mesh calcium carbonate sand filter to obtain a calcium chloride solution, which is then concentrated to 50% by MVR evaporation and packaged to obtain an industrial calcium chloride product.
2. The method for producing industrial calcium chloride by using rare earth smelting high-salt wastewater according to claim 1, characterized in that: Before the reaction in step (1) is carried out on the wastewater obtained by the extraction and separation of rare earth smelting, the magnesium ion content in the wastewater is first analyzed and controlled to be ≥0.5%. If the magnesium ion content in the wastewater is <0.5%, magnesium chloride wastewater is added to make the magnesium ion content in the wastewater reach 0.5%-1%.
3. The method for producing industrial calcium chloride by using rare earth smelting high-salt wastewater according to claim 1, characterized in that: The mixing time of the two phases in the pipeline mixer described in step (3) is less than 2s.