A method for preparing high-strength foamed concrete using engineering slag

By modifying engineering muck and combining it with specific materials, high-strength foamed concrete is prepared, which solves the problem of low utilization rate of engineering muck in traditional treatment methods and achieves high-strength and low water absorption concrete with good performance Excellent thermal insulation performance and wide market application prospects.

CN116283112BActive Publication Date: 2024-10-29HUNAN RONGCHENG ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310277364.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-21
Publication Date
2024-10-29
Estimated Expiration
2043-03-21

AI Technical Summary

Technical Problem

Traditional engineering waste treatment methods are difficult to meet the needs of large-scale engineering waste treatment, and their comprehensive utilization rate and added value in building materials are low. It is difficult to prepare high-strength foamed concrete with existing technology.

Method used

By modifying the engineering residue and combining activated kaolin, fly ash, quicklime, expanded perlite, reinforcing fibers, polymer emulsion and specific additives, high-strength foamed concrete is prepared to form a three-dimensional network structure and improve mechanical properties and reduce water absorption.

Benefits of technology

It has achieved high strength and low water absorption of foamed concrete, with a 28-day compressive strength of more than 5.5MPa, good thermal insulation performance, and broad market application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116283112B_ABST
    Figure CN116283112B_ABST
Patent Text Reader

Abstract

The invention relates to the field of building materials, and in particular to a method for preparing high-strength foamed concrete from engineering slag. The engineering slag is modified, and the modified engineering slag, cement, quicklime, expanded perlite, reinforcing fiber, polymer emulsion, and an external additive are added into water and stirred evenly to prepare slurry. A foaming agent is added, and the slurry is quickly stirred to prepare a foaming slurry, which is poured into a mold, foaming is stopped, demoulding is performed, and curing is performed to a specified age. The foamed concrete prepared by the invention has higher mechanical properties and lower water absorption rate, a 28-day compressive strength of more than 5.5MPa, good thermal insulation performance, and broad market application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building materials, in particular to a method for preparing high-strength foamed concrete from engineering slag. Background Art

[0002] In urban construction projects, especially the development process of large-scale, deep underground space (foundation excavation projects such as various buildings, pipelines, etc.), a huge amount of construction waste will be generated, which accounts for more than 70% of the total construction waste, and the environmental and safety problems it brings are gradually becoming prominent.

[0003] Traditional methods of treating construction waste include direct backfilling, dumping in abandoned pits, and throwing in sea reclamation. However, facing the increasing volume of construction waste and severe environmental protection situation, traditional treatment methods are increasingly unable to meet social needs. Therefore, in order to improve the comprehensive utilization rate and added value of construction waste, Liu Chun et al. ① The influence of slag on the mechanical properties of C50 concrete was studied. Wang Hailiang et al. ② The feasibility of using slag as a mineral admixture and the effect of slag content on concrete performance were studied. ③ The effect of cementitious component mix ratio on bulk density, compressive strength, pore size, etc. of activated sludge and slag foam concrete was studied. Although there are many reports on the application of engineering sludge in building materials, the results are generally not ideal.

[0004] ① Liu Chun, Wang Anhui, Yu Pei, Rong Hui. Effect of slag on mechanical properties of C50 concrete[J]. Bulletin of the Silicate Society, 2016, (No. 4);

[0005] ② Wang Hailiang, Li Chao, Rong Hui, Song Weijun, Qi Zhanguo, Li Xianghai, Di Zhikun. Effect of slag on the performance of C30 concrete [J]. Bulletin of the Silicate Society, 2016, (Issue 9);

[0006] ③ Gao Ping, Xin Xiaoting, Guo Shuhui, Li Shaobin. Influence of cementitious materials on the performance of modified slag foam concrete [J]. Guangdong Building Materials, 2019, (Issue 7). Summary of the invention

[0007] Purpose of the invention: In view of the above technical problems, the present invention proposes a method for preparing high-strength foamed concrete using engineering slag.

[0008] The technical solutions adopted are as follows:

[0009] A method for preparing high-strength foamed concrete using engineering slag:

[0010] The construction waste is modified, the modified construction waste is added into water with cement, quicklime, expanded perlite, reinforcing fiber, polymer emulsion and external additives, stirred evenly to prepare slurry, then a foaming agent is added, stirred rapidly to prepare a foaming slurry, poured into a mold, allowed to foam, demolded and cured to a specified age.

[0011] Furthermore, the water content of the engineering slag is ≤55%, the organic matter content is ≤12%, and the plasticity index is 21-28%.

[0012] Furthermore, the mass ratio of the modified engineering slag to cement, quicklime, expanded perlite, reinforcing fiber, polymer emulsion and external additives is 66-70:36-40:4-6:8-10:2-4:2-4:1.

[0013] Furthermore, the modification treatment method of the construction slag is as follows:

[0014] The construction waste is mixed with activated kaolin, fly ash, soda ash and water, and then the organic colloid component is added. The mixture is stirred continuously to make it evenly dispersed and then transferred to a mold for pressing. The obtained embryo is steamed, dried and crushed.

[0015] Furthermore, the preparation method of the activated kaolin is as follows:

[0016] Mix sodium hydroxide and kaolin and grind them, then calcine at 550-600℃ for 30-60min and cool to room temperature.

[0017] Furthermore, the organic colloid component includes xanthan gum, guar gum, and hydroxypropyl methylcellulose;

[0018] The mass ratio of the xanthan gum, guar gum and hydroxypropyl methylcellulose is 5-10:3-5:1.

[0019] Furthermore, the added additives include polycarboxylate water reducer, accelerating setting agent, and calcium stearate;

[0020] The mass ratio of the polycarboxylate water reducer, the accelerating setting agent and the calcium stearate is 3-5:1:1.

[0021] Further, the foaming agent includes limonene, manganese dioxide and hydrogen peroxide;

[0022] The dosage of the limonene and manganese dioxide is 20-35% and 0.5-2% of the mass of the hydrogen peroxide respectively.

[0023] Furthermore, the polymer emulsion is a silicone-modified fluorinated styrene-acrylic emulsion.

[0024] Furthermore, the preparation method of the organosilicon-modified fluorinated styrene-acrylic emulsion is as follows:

[0025] Mix the emulsifier, potassium perfluorobutyl sulfonate and water, stir until dissolved, then add methyl methacrylate, butyl acrylate, styrene and acrylic acid, stir at high speed to form a uniform pre-emulsion, take part of the pre-emulsion and mix with part of the initiator solvent under protective gas, stir and heat to 80-90°C, react for 1.5-2h, then drop the remaining pre-emulsion, hexafluorobutyl methacrylate, remaining initiator solvent and sodium bicarbonate solution, keep warm for 2-4h after dropping, and cool naturally to 40 ℃ below, adjust the pH of the system to neutral with ammonia water to obtain a fluorinated styrene-acrylic emulsion, under protective gas, mix hydroquinone and methyl methacrylate, stir and heat to 60-70 ℃, add chloroplatinic acid / isopropanol solution and toluene, stir evenly, then heat to 85-90 ℃ and react for 30-50 min, add hydrogen-containing silicone oil, keep warm for 30-50 min, then heat to 130 ℃, keep warm and react for 3-6 h, remove the solvent by distillation under reduced pressure, add the obtained product to the fluorinated styrene-acrylic emulsion and mix evenly.

[0026] Beneficial effects of the present invention:

[0027] The invention provides a method for preparing high-strength foamed concrete from engineering slag. Kaolin belongs to layered silicate minerals. After being activated, it releases a large amount of silicon and aluminum monomers to form silicon and aluminum oligomers, which can form a gel phase with engineering slag and fly ash. The organic colloid component is used as a thickening and viscosity-promoting component to promote the formation of the gel phase. During the steam cooking process, the gel phase hardens to form a three-dimensional network structure, which can be used as a reinforcing component in concrete. Quicklime can stimulate the activity of cement to improve the mechanical strength of the foamed concrete. Ca 2+ Compared with the low-priced Na in construction waste + , K + An ion exchange reaction occurs, the double electric layer is thinned, the radius of hydrated ions is reduced, flocculation and coagulation are promoted, and the "shaft-holding" phenomenon generated during the stirring process is effectively avoided. During the concrete hardening process, the polymer emulsion forms an organic hydrophobic film on the surface of the hydration product of the capillary wall through the physical effects of demulsification and spreading, thereby reducing the overall water absorption capacity and having a certain supporting capacity for the internal pores. Manganese dioxide can be used as a catalyst to promote the decomposition of hydrogen peroxide, and limonene can improve the stability of the formed foam and improve the uniformity of the pores. The foamed concrete prepared by the present invention has higher mechanical properties and lower water absorption rate, and the 28-day compressive strength reaches more than 5.5MPa, and the thermal insulation performance is good, and the market application prospect is broad. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a cross-sectional photograph of the foamed concrete prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0029] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The technologies not mentioned in the present invention are all referenced to the prior art.

[0030] Embodiment 1:

[0031] A method for preparing high-strength foamed concrete using engineering slag:

[0032] 10g of sodium hydroxide and 100g of kaolin were mixed and ground and placed in a muffle furnace, and then calcined at 580°C for 50min, and naturally cooled to room temperature to obtain activated kaolin. 1000g of engineering slag with a moisture content of 54.4%, an organic matter content of 8.25%, and a plasticity index of 27.5 was mixed with 80g of activated kaolin, 10g of fly ash, 25g of soda ash, and 25L of water, and then 10g of xanthan gum, 4g of guar gum, and 1g of hydroxypropyl methylcellulose were added. After continuing to stir to make it evenly dispersed, it was transferred to a mold and pressed at 10MPa for 20s. The resulting embryo was steamed for 5h and then dried at 80°C and crushed to 200 mesh to obtain modified engineering slag. 680g of the modified engineering slag was taken and mixed with 400g of cement, 50g of quicklime, 100g of expanded perlite, 30g of glass fiber, 30g of silicone-modified fluorinated styrene-acrylic emulsion, 6g of polycarboxylic acid water reducer, and 2g of TA-CS1 type quick-setting agent and 2g calcium stearate are added into water and stirred evenly. After the slurry is prepared, 35g of foaming agent composed of limonene, manganese dioxide and hydrogen peroxide is added, wherein the amount of limonene and manganese dioxide is 28% and 0.5% of the mass of hydrogen peroxide respectively. Stir rapidly for 40s to prepare the foaming slurry, pour it into the mold, stop foaming, demould and cure to the specified age.

[0033] The preparation method of the organosilicon-modified fluorinated styrene-acrylic emulsion is as follows:

[0034] 6.4 g of emulsifier OP-10 and 100 mL of water were mixed and stirred until dissolved. Then 12.7 g of methyl methacrylate, 27.5 g of butyl acrylate, 28.3 g of styrene and 2.7 g of acrylic acid were added and stirred at high speed to form a uniform pre-emulsion. Under protective gas, 1 / 3 of the pre-emulsion was mixed with 5 mL of 5 wt% ammonium persulfate solution, stirred and heated to 90°C. After reacting for 1.5 h, the remaining pre-emulsion, 6.5 g of hexafluorobutyl methacrylate, 5 mL of 5 wt% ammonium persulfate solution and 25 mL of 5 wt% sodium bicarbonate solution were added dropwise. After the addition was completed, the mixture was kept warm for 3 h and naturally cooled to below 40°C. The pH of the system was adjusted to neutral with aqueous ammonia to obtain a fluorinated styrene-acrylic emulsion. Under protective gas, 2 g of hydroquinone and 100 g of methyl methacrylate were mixed, stirred and heated to 70°C, and 3.5 g of 2wt% chloroplatinic acid / isopropanol solution and 55mL toluene are stirred evenly, then heated to 90℃ and reacted for 40min. 100g hydrogenated silicone oil is added, and the temperature is raised to 130℃ after keeping warm for 50min. The temperature is kept warm for 5h. The solvent is removed by distillation under reduced pressure, and 10g of the obtained product is added to the fluorinated styrene-acrylic emulsion and mixed evenly.

[0035] Embodiment 2:

[0036] A method for preparing high-strength foamed concrete using engineering slag:

[0037] 10g of sodium hydroxide and 100g of kaolin were mixed and ground and placed in a muffle furnace, and then calcined at 600℃ for 60min, and naturally cooled to room temperature to obtain activated kaolin. 1000g of engineering slag with a moisture content of 54.4%, an organic matter content of 8.25%, and a plasticity index of 27.5 was mixed with 80g of activated kaolin, 10g of fly ash, 25g of soda ash, and 25L of water, and then 10g of xanthan gum, 4g of guar gum, and 1g of hydroxypropyl methylcellulose were added. After continuing to stir to make it evenly dispersed, it was transferred to a mold and pressed at 10MPa for 20s. The resulting embryo was steamed for 5h and then dried at 80℃ and crushed to 200 mesh to obtain modified engineering slag. 700g of the modified engineering slag was mixed with 400g of cement, 60g of quicklime, 100g of expanded perlite, 40g of glass fiber, 40g of silicone-modified fluorinated styrene-acrylic emulsion, 6g of polycarboxylic acid water reducer, and 2g of TA-CS1 type quick-setting agent and 2g calcium stearate are added into water and stirred evenly. After the slurry is prepared, 35g of a foaming agent composed of limonene, manganese dioxide and hydrogen peroxide is added, wherein the amount of limonene and manganese dioxide is 35% and 2% of the mass of hydrogen peroxide respectively. Rapidly stir for 40s to prepare a foaming slurry, pour it into the mold, stop foaming, demould, and cure to the specified age.

[0038] The preparation method of the organosilicon-modified fluorinated styrene-acrylic emulsion is the same as that in Example 1.

[0039] Embodiment 3:

[0040] A method for preparing high-strength foamed concrete using engineering slag:

[0041] 10g of sodium hydroxide and 100g of kaolin were mixed and ground and placed in a muffle furnace, and then calcined at 550°C for 30min, and naturally cooled to room temperature to obtain activated kaolin. 1000g of engineering slag with a moisture content of 54.4%, an organic matter content of 8.25%, and a plasticity index of 27.5 was mixed with 80g of activated kaolin, 10g of fly ash, 25g of soda ash, and 25L of water, and then 10g of xanthan gum, 4g of guar gum, and 1g of hydroxypropyl methylcellulose were added. After continuing to stir to make it evenly dispersed, it was transferred to a mold and pressed at 10MPa for 20s. The resulting embryo was steamed for 5h and then dried at 80°C and crushed to 200 mesh to obtain modified engineering slag. 660g of the modified engineering slag was mixed with 360g of cement, 40g of quicklime, 80g of expanded perlite, 20g of glass fiber, 20g of silicone-modified fluorinated styrene-acrylic emulsion, 6g of polycarboxylic acid water reducer, and 2g of TA-CS1 type quick-setting agent and 2g calcium stearate are added into water and stirred evenly. After the slurry is prepared, 35g of a foaming agent composed of limonene, manganese dioxide and hydrogen peroxide is added, wherein the amount of limonene and manganese dioxide is 20% and 0.5% of the mass of hydrogen peroxide respectively. Stir rapidly for 40s to prepare a foaming slurry, pour it into the mold, stop foaming, demould, and cure to the specified age.

[0042] The preparation method of the organosilicon-modified fluorinated styrene-acrylic emulsion is the same as that in Example 1.

[0043] Embodiment 4:

[0044] A method for preparing high-strength foamed concrete using engineering slag:

[0045] 10g of sodium hydroxide and 100g of kaolin were mixed and ground and placed in a muffle furnace, and then calcined at 600℃ for 30min, and naturally cooled to room temperature to obtain activated kaolin. 1000g of engineering slag with a moisture content of 54.4%, an organic matter content of 8.25%, and a plasticity index of 27.5 was mixed with 80g of activated kaolin, 10g of fly ash, 25g of soda ash, and 25L of water, and then 10g of xanthan gum, 4g of guar gum, and 1g of hydroxypropyl methylcellulose were added. After continuing to stir to make it evenly dispersed, it was transferred to a mold and pressed at 10MPa for 20s. The resulting embryo was steamed for 5h and then dried at 80℃ and crushed to 200 mesh to obtain modified engineering slag. 700g of the modified engineering slag was mixed with 360g of cement, 60g of quicklime, 80g of expanded perlite, 40g of glass fiber, 20g of silicone-modified fluorinated styrene-acrylic emulsion, 6g of polycarboxylic acid water reducer, and 2g of TA-CS1 type quick-setting agent and 2g calcium stearate are added into water and stirred evenly. After the slurry is prepared, 35g of foaming agent composed of limonene, manganese dioxide and hydrogen peroxide is added, wherein the amount of limonene and manganese dioxide is 35% and 0.5% of the mass of hydrogen peroxide respectively. Stir rapidly for 40s to prepare the foaming slurry, pour it into the mold, stop foaming, demould and cure to the specified age.

[0046] The preparation method of the organosilicon-modified fluorinated styrene-acrylic emulsion is the same as that in Example 1.

[0047] Embodiment 5:

[0048] A method for preparing high-strength foamed concrete using engineering slag:

[0049] 10g of sodium hydroxide and 100g of kaolin were mixed and ground and placed in a muffle furnace, and then calcined at 550°C for 60min, and naturally cooled to room temperature to obtain activated kaolin. 1000g of engineering slag with a moisture content of 54.4%, an organic matter content of 8.25%, and a plasticity index of 27.5 was mixed with 80g of activated kaolin, 10g of fly ash, 25g of soda ash, and 25L of water, and then 10g of xanthan gum, 4g of guar gum, and 1g of hydroxypropyl methylcellulose were added. After continuing to stir to make it evenly dispersed, it was transferred to a mold and pressed at 10MPa for 20s. The resulting embryo was steamed for 5h and then dried at 80°C and crushed to 200 mesh to obtain modified engineering slag. 660g of the modified engineering slag was mixed with 400g of cement, 40g of quicklime, 100g of expanded perlite, 20g of glass fiber, 40g of silicone-modified fluorinated styrene-acrylic emulsion, 6g of polycarboxylic acid water reducer, and 2g of TA-CS1 type quick-setting agent and 2g calcium stearate are added into water and stirred evenly. After the slurry is prepared, 35g of foaming agent composed of limonene, manganese dioxide and hydrogen peroxide is added, wherein the amount of limonene and manganese dioxide is 20% and 2% of the mass of hydrogen peroxide respectively. Stir rapidly for 40s to prepare the foaming slurry, pour it into the mold, stop foaming, demould and cure to the specified age.

[0050] The preparation method of the organosilicon-modified fluorinated styrene-acrylic emulsion is the same as that in Example 1.

[0051] Comparative Example 1:

[0052] It is basically the same as Example 1, except that the kaolin is not activated.

[0053] Comparative Example 2:

[0054] It is basically the same as Example 1, except that the construction waste soil is not modified.

[0055] Comparative Example 3:

[0056] The method is basically the same as Example 1, except that the silicone-modified fluorinated styrene-acrylic emulsion is not added.

[0057] Comparative Example 4:

[0058] The method is substantially the same as Example 1, except that limonene is not added to the foaming agent.

[0059] Performance Testing:

[0060] The foamed concrete prepared in Examples 1-5 of the present invention and Comparative Examples 1-4 were used as samples for performance testing;

[0061] Dry density, compressive strength and water absorption: Tested in accordance with JG / T266-2011 "Foamed Concrete";

[0062] Thermal conductivity: refer to the method disclosed in GB / T10294-2008 "Determination of steady-state thermal resistance and related properties of insulation materials - Guarded hot plate method", and use a foam concrete thermal conductivity tester (Shanghai Hesheng Instrument Technology Co., Ltd., HS-DR-1) for testing;

[0063] The test results are shown in Table 1 below:

[0064] Table 1:

[0065]

[0066] It can be seen from Table 1 above that the foamed concrete prepared by the present invention has higher mechanical properties and lower water absorption, the 28-day compressive strength reaches above 5.5 MPa, the thermal insulation performance is good, and the market application prospect is broad.

[0067] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing high-strength foamed concrete from engineering slag, characterized in that: The engineering slag is modified, and the modified engineering slag, cement, quicklime, expanded perlite, reinforcing fiber, polymer emulsion, and external additives are added to water, stirred evenly, and after preparing slurry, a foaming agent is added, stirred quickly, and a foaming slurry is prepared, poured into a mold, and the foaming is stopped, demolded, and cured to a specified age; The modification treatment method of the engineering slag is as follows: After the construction waste is mixed with activated kaolin, fly ash, soda ash and water, the organic colloid component is added, and the mixture is stirred to make it evenly dispersed, and then the mixture is transferred to a mold for pressing. The obtained embryo is steamed, dried and crushed. The preparation method of the activated kaolin is as follows: Mix sodium hydroxide and kaolin, grind them together, calcine at 550-600℃ for 30-60min, and cool to room temperature; The added additives include polycarboxylate water reducer, accelerating setting agent and calcium stearate; The mass ratio of the polycarboxylate water reducer, the accelerating setting agent and the calcium stearate is 3-5:1:1; The foaming agent includes limonene, manganese dioxide and hydrogen peroxide; The dosage of the limonene and manganese dioxide is 20-35% and 0.5-2% of the mass of the hydrogen peroxide respectively; The polymer emulsion is a silicone-modified fluorinated styrene-acrylic emulsion; The organic colloid component includes xanthan gum, guar gum and hydroxypropyl methylcellulose; The mass ratio of the xanthan gum, guar gum and hydroxypropyl methylcellulose is 5-10:3-5:

1.

2. The method for preparing high-strength foamed concrete from construction slag as claimed in claim 1, characterized in that: The water content of the engineering slag is ≤55%, the organic matter content is ≤12%, and the plasticity index is 21-28%.

3. The method for preparing high-strength foamed concrete from construction slag as claimed in claim 1, characterized in that: The mass ratio of the modified engineering slag to cement, quicklime, expanded perlite, reinforcing fiber, polymer emulsion and external additives is 66-70:36-40:4-6:8-10:2-4:2-4:

1.

4. The method for preparing high-strength foamed concrete from construction waste as claimed in claim 1, characterized in that: The preparation method of the organosilicon-modified fluorinated styrene-acrylic emulsion is as follows: Mix the emulsifier, potassium perfluorobutyl sulfonate and water, stir until dissolved, then add methyl methacrylate, butyl acrylate, styrene and acrylic acid, stir at high speed to form a uniform pre-emulsion, take part of the pre-emulsion and mix with part of the initiator solvent under protective gas, stir and heat to 80-90°C, react for 1.5-2h, then drop the remaining pre-emulsion, hexafluorobutyl methacrylate, remaining initiator solvent and sodium bicarbonate solution, keep warm for 2-4h after dropping, and cool naturally to 40 ℃ below, adjust the pH of the system to neutral with ammonia water to obtain a fluorinated styrene-acrylic emulsion, under protective gas, mix hydroquinone and methyl methacrylate, stir and heat to 60-70 ℃, add chloroplatinic acid / isopropanol solution and toluene, stir evenly, then heat to 85-90 ℃ and react for 30-50 min, add hydrogen-containing silicone oil, keep warm for 30-50 min, then heat to 130 ℃, keep warm and react for 3-6 h, remove the solvent by distillation under reduced pressure, add the obtained product to the fluorinated styrene-acrylic emulsion and mix evenly.

Citation Information

Patent Citations

  • Method for manufacturing foamed bricks based on construction waste soil

    CN105712683A

  • Aluminum tobermorite containing refuse-oil based autoclaved aerated concrete block and production method

    CN106810169A