Coating composition, method for producing the same, and coating film

By dispersing inorganic oxide particles and zinc cyanurate particles in a liquid medium in the coating composition, the problem of uneven dispersion of zinc cyanurate particles is solved, achieving high adhesion to the substrate and stability and uniformity of the multifunctional coating composition.

CN116285692BActive Publication Date: 2024-10-29NISSAN CHEM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310190980.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-18
Publication Date
2024-10-29
Estimated Expiration
2040-09-18

AI Technical Summary

Technical Problem

When zinc cyanurate particles are dispersed in a medium, they tend to form an uneven slurry, which makes it difficult to process when mixed with resin and to form a coating composition with high adhesion to the substrate and good functionality.

Method used

By dispersing inorganic oxide particles and zinc cyanurate particles as dispersants in a liquid medium to form a stable dispersion, and then combining it with a resin emulsion, a coating composition is prepared, ensuring good dispersibility and maintaining a stable state.

Benefits of technology

It achieves excellent adhesion between the coating composition and the substrate, improves durability, scratch resistance, corrosion resistance and prevents substrate color changes, while maintaining the uniformity and stability of the coating film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The problem is to provide a coating composition, a method for producing the same, and a coating film that can fully exert the function of zinc cyanurate in preventing corrosion of metal surfaces. The solution is a coating composition comprising a coating additive and a resin, wherein the coating additive comprises a dispersion obtained by dispersoid particles dispersed in a liquid medium, wherein the dispersoid particles comprise inorganic oxide particles and zinc cyanurate particles.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a Chinese patent application filed on September 18, 2020, with application number 202080064965.0 and invention name “Dispersion and coating composition containing inorganic oxide particles and zinc cyanurate particles”. Technical Field

[0002] The present invention relates to a coating composition comprising a coating additive and a resin, a coating film formed by the coating composition, a method for producing the coating composition, and a coating additive added to the coating composition. The coating additive comprises a dispersion containing inorganic oxide particles and zinc cyanurate particles.

[0003] The present invention also relates to a dispersion containing an inorganic oxide powder among the inorganic oxide particles and zinc cyanurate particles, and a dispersion containing specific colloidal metal oxide particles among the inorganic oxide particles and zinc cyanurate particles. Background Art

[0004] Zinc cyanurate is known as an anticorrosive agent for the metal surface of iron-based metals, and various methods have been disclosed regarding the production method thereof.

[0005] For example, Patent Document 1 discloses the following production method as a method for producing lead and zinc cyanurate, which are known as anticorrosion protective agents for metal surfaces: PbO or ZnO and cyanuric acid are mixed into a paste at 100°C to 180°C, and a shearing action is applied to the obtained paste at 50°C to 250°C.

[0006] In addition, Patent Document 2 discloses an anti-corrosion coating material using zinc salt and / or lead salt of an organic compound such as barbituric acid or cyanuric acid as an anti-corrosion coating agent for metal surfaces based on zinc salt and / or lead salt of an organic compound.

[0007] Patent Document 3 discloses a method for producing needle-shaped or plate-shaped basic zinc cyanurate particles by wet dispersing a mixed slurry of zinc oxide or basic zinc carbonate, cyanuric acid, and water. The needle-shaped or plate-shaped basic zinc cyanurate particles are characterized in that an average particle size D measured by a laser diffraction method is 50 The surface area is 80nm to 900nm and the specific surface area is 20m 2 / g~100m 2 / g, and the length ratio of the major axis / minor axis (axis ratio) is 5-25.

[0008] Patent Document 4 discloses a method for producing basic zinc cyanurate powder by heat-treating a mixed powder containing zinc oxide, cyanuric acid and water in a closed or open state, and discloses a rust-proof pigment composition containing the basic zinc cyanurate powder.

[0009] In addition to the purpose of coloring the object (coated surface), the coating also has various effects required such as the above-mentioned rust prevention effect and weather resistance. For example, if it is a metal substrate (aluminum, iron, etc.), it is required to have an anti-corrosion function, if it is a resin substrate and wood, it is required to have durability, weather resistance, scratch resistance, corrosion resistance, prevention of color change, etc., and if it is a glass substrate and silicon substrate, it is required to have improved strength and light resistance.

[0010] Prior art literature

[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 59-031779

[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 54-123145

[0013] Patent Document 3: International Publication No. 2011 / 162353

[0014] Patent Document 4: International Publication No. 2016 / 006585 Summary of the invention

[0015] It has been known that zinc cyanurate can provide a high anti-corrosion function to a metal surface. However, the zinc cyanurate obtained by the above-mentioned production method has a needle-like or plate-like particle shape and a relatively large particle size. When it is dispersed in a medium, it becomes an uneven slurry. Therefore, it is difficult to handle when mixed with a resin as a binder to form a coating composition.

[0016] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a coating composition capable of forming a coating film having high adhesion to a substrate, and thereby to provide a coating composition capable of fully exerting the functions of zinc cyanurate in preventing corrosion of metal surfaces, etc., and capable of exerting effects such as improving durability, improving scratch resistance, improving corrosion resistance of the substrate, and preventing color changes of the substrate (less likely to cause poor appearance) on PET substrates and wood, etc.

[0017] The inventors of the present invention have repeatedly studied intensively to solve the above-mentioned problems, and as a result, have found that, by using a dispersion obtained by dispersing both inorganic oxide particles and zinc cyanurate particles as dispersoids in a liquid medium as a coating additive, and combining it with a resin component such as a resin emulsion, a coating composition having good dispersibility and being able to maintain a stable dispersion state can be surprisingly obtained. In addition, it has been found that the above-mentioned coating composition can obtain a coating film that not only has excellent adhesion to the substrate (coated surface), but also has small curing shrinkage and excellent followability to the deformation of the substrate. Therefore, in addition to the anti-corrosion effect on the metal surface, various functions of the coating can be expected: the durability, scratch resistance, and corrosion resistance of the substrate are improved, and the color tone of the substrate is prevented from changing, thereby completing the present invention.

[0018] That is, as a first aspect of the present invention, there is provided a coating composition comprising a coating additive and a resin, wherein the coating additive comprises a dispersion in which dispersoid particles are dispersed in a liquid medium, and the dispersoid particles comprise inorganic oxide particles and zinc cyanurate particles.

[0019] As a second aspect, the coating composition described in the first aspect, wherein the coated surface is at least one selected from an aluminum substrate, an iron substrate, a copper substrate, a gold substrate, a silver substrate, a platinum substrate, a mirror material, a glass substrate, a silicon substrate, wood, a resin film and a resin molded product.

[0020] As a third aspect, the present invention relates to a coating composition according to the first aspect or the second aspect, wherein the resin is in the form of a resin emulsion, which is in the form of an oil-in-water emulsion or a water-in-oil emulsion, and is a resin emulsion containing one or more resin components selected from acrylic resins, acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, styrene resins, olefin resins, ethylene-vinyl acetate resins, ester resins, epoxy resins, phenolic resins, amide resins, vinyl alcohol resins, fluorine resins, polyurethane resins, melamine resins, phthalic acid resins, silicone resins, alkyd resins and vinyl chloride resins.

[0021] As a fourth aspect, the present invention relates to the coating composition according to the first aspect or the second aspect, wherein the resin is in the form of a water-soluble polymer or a colloidal dispersion, and is a water-soluble resin or a colloidal dispersion comprising one or more resin components selected from acrylic resins, acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, styrene resins, olefin resins, ethylene-vinyl acetate resins, ester resins, epoxy resins, phenolic resins, amide resins, vinyl alcohol resins, fluorine resins, polyurethane resins, melamine resins, phthalic acid resins, silicone resins, alkyd resins and vinyl chloride resins.

[0022] As a fifth aspect, the present invention relates to a coating composition according to any one of the first to fourth aspects, wherein the inorganic oxide particles are oxides of at least one atom selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

[0023] As a sixth aspect, the coating composition relates to the coating composition described in the fifth aspect, wherein the inorganic oxide particles are a composite oxide or a mixed oxide of two or more atoms selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

[0024] As a seventh aspect, the present invention relates to a coating composition according to any one of the first to fifth aspects, wherein the inorganic oxide particles are colloidal oxides of at least one atom selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

[0025] As an eighth aspect, the coating composition relates to the seventh aspect, wherein the inorganic oxide particles are colloidal composite oxides or colloidal mixed oxides of two or more atoms selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

[0026] According to a ninth aspect, in the coating composition according to any one of the first to eighth aspects, the zinc cyanurate particles have a primary particle major axis of 400 nm to 3,000 nm and a primary particle minor axis of 10 nm to 300 nm, and a ratio of the major axis to the minor axis of 1.3 to 300 when measured using a transmission electron microscope.

[0027] According to a tenth aspect, the coating composition according to any one of the first to ninth aspects is characterized in that the dispersoid particles in the dispersion have an average particle size of 80 nm to 5,000 nm when measured by laser diffraction, and the solid content concentration of the dispersoid particles in the dispersion is 0.1 to 50% by mass.

[0028] As an eleventh aspect, the present invention relates to the coating composition according to any one of the first to tenth aspects, wherein the dispersoid particles in the dispersion liquid contain inorganic oxide particles and zinc cyanurate particles at a mass ratio of 1:0.01 to 100, and the solid content concentration of the dispersoid particles in the dispersion liquid is 0.1 to 50 mass %.

[0029] As a twelfth aspect, the present invention relates to the coating composition according to any one of the first aspect to the eleventh aspect, wherein the liquid medium is water or an organic solvent.

[0030] As a 13th aspect, the present invention relates to the coating composition described in any one of the 1st aspect to the 12th aspect, wherein the ratio of the solid content in the dispersion to the resin is 1:0.1 to 20 in terms of the mass ratio of (solid content in the dispersion):(resin), and the ratio of the total solid content in the coating composition is 1 to 70 mass%.

[0031] As a fourteenth aspect, the coating composition according to any one of the first aspect to the thirteenth aspect further comprises a slurry of an inorganic oxide powder, wherein the solid content concentration of the slurry is 0.1 to 50% by mass.

[0032] As the 15th aspect, it relates to the coating composition recorded in the 14th aspect, wherein the ratio of the solid content in the dispersion, the resin and the solid content of the slurry of the inorganic oxide powder is 1:0.1~20:0.1~1 in terms of mass ratio of (solid content in the dispersion):(resin):(solid content of the slurry), and the proportion of the total solid content in the coating composition is 1~70 mass %.

[0033] As a 16th aspect, it relates to a coating film of the coating composition recorded in any one of the 1st aspect to the 15th aspect, which is formed on at least one substrate selected from an aluminum substrate, an iron-based substrate, a copper-based substrate, a gold-based substrate, a silver-based substrate, a platinum-based substrate, a mirror material, a glass substrate, a silicon substrate, wood, a resin film and a resin molded product.

[0034] As a seventeenth aspect, the present invention relates to a coating film, which is a coating film of the coating composition according to any one of the first aspect to the fifteenth aspect, and has a film thickness of 0.1 μm to 100 μm.

[0035] As an eighteenth aspect, the present invention relates to the coating film according to the seventeenth aspect, wherein the coating film is a spin coating film, a bar coating film, a roll coating film, or a dip coating film.

[0036] As a 19th aspect, it relates to a method for producing a coating composition described in any one of the 1st aspect to the 15th aspect, comprising a step of mixing a dispersion and a resin using a liquid disperser, wherein the dispersion is obtained by dispersoid particles containing inorganic oxide particles and zinc cyanurate particles being dispersed in a liquid medium.

[0037] As a 20th aspect, a method for producing a coating composition according to the 14th aspect or the 15th aspect comprises the step of mixing a dispersion, the resin and a slurry of the inorganic oxide powder using a liquid disperser, wherein the dispersion is obtained by dispersoid particles containing inorganic oxide particles and zinc cyanurate particles being dispersed in a liquid medium.

[0038] As a 21st aspect, it relates to the production method described in the 19th aspect or the 20th aspect, wherein the liquid disperser is a stirrer, a rotary shearing stirrer, a colloid mill, a roller mill, a high-pressure jet disperser, an ultrasonic disperser, a container-driven mill, a medium stirring mill or a kneader.

[0039] As a 22nd aspect, the method for producing a coating composition according to any one of the 19th to 21st aspects further comprises a step of mixing a mixed solution of inorganic oxide particles and zinc cyanurate particles or a slurry thereof using a pulverizing device before the step of mixing using the liquid disperser.

[0040] As a 23rd aspect, the present invention relates to the production method according to the 22nd aspect, wherein the pulverizing device is a ball mill, a bead mill or a sand mill.

[0041] As a 24th aspect, the method for producing a coating composition according to any one of the 19th to 21st aspects further comprises a step of mixing a mixed liquid of the pre-crushed inorganic oxide powder and zinc cyanurate particles or a slurry thereof using a pulverizing device before the mixing step using the liquid disperser.

[0042] As a twenty-fifth aspect, the present invention relates to a dispersion liquid obtained by dispersing dispersoid particles including inorganic oxide particles and zinc cyanurate particles in a liquid medium, wherein the inorganic oxide particles are inorganic oxide powders, and the specific surface area of ​​the inorganic oxide powders is 1 to 800 m 2 / g and the loose bulk density is 0.03~3.0g / cm 3 .

[0043] As the 26th aspect, relating to the dispersion recorded in the 25th aspect, the inorganic oxide powder is an oxide of at least one atom selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

[0044] According to a 27th aspect, in the dispersion according to the 25th aspect or the 26th aspect, the dispersoid particles have an average particle size of 200 nm to 5,000 nm when measured by laser diffraction, and the solid content concentration of the dispersoid particles in the dispersion is 0.1 to 50% by mass.

[0045] As a twenty-eighth aspect, the present invention relates to a dispersion liquid obtained by dispersing dispersoid particles including inorganic oxide particles and zinc cyanurate particles in a liquid medium, wherein the inorganic oxide particles are colloidal metal oxide particles excluding particles containing colloidal silica as a main component.

[0046] As a 29th aspect, the present invention relates to the dispersion described in the 28th aspect, wherein the colloidal metal oxide particles contain an oxide of at least one atom selected from Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

[0047] According to a 30th aspect, in the dispersion according to the 28th aspect or the 29th aspect, the dispersoid particles have an average particle size of 80 nm to 2,000 nm when measured by laser diffraction, and a solid content concentration of the dispersoid particles in the dispersion is 0.1 to 50% by mass.

[0048] The present invention also relates to a dispersion liquid containing an inorganic oxide powder and zinc cyanurate particles. That is, the present invention includes the following aspects [1] to

[21] . [1]

[0050] A dispersion liquid is obtained by dispersing dispersoid particles containing inorganic oxide powder and zinc cyanurate particles in a liquid medium, wherein the specific surface area of ​​the inorganic oxide powder is 1 to 800 m 2 / g and the loose bulk density is 0.03~3.0g / cm 3 . [2]

[0052] According to the dispersion described in [1], the inorganic oxide powder is an oxide of at least one atom selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce. [3]

[0054] According to the dispersion described in [2], the inorganic oxide powder is a composite oxide or mixed oxide of two or more atoms selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce. [4]

[0056] The dispersion according to any one of [1] to [3], wherein the zinc cyanurate particles have a primary particle major axis of 400 nm to 3,000 nm and a primary particle minor axis of 10 nm to 300 nm, and a ratio of the major axis to the minor axis of 1.3 to 300, when measured using a transmission electron microscope. [5]

[0058] The dispersion according to any one of [1] to [4], wherein the dispersoid particles have an average particle size of 200 nm to 5,000 nm when measured by laser diffraction, and the solid content concentration of the dispersoid particles in the dispersion is 0.1 to 50% by mass. [6]

[0060] The dispersion according to any one of [1] to [5], wherein the dispersoid particles include inorganic oxide particles and zinc cyanurate particles at a mass ratio of 1:0.01 to 100, and the solid content concentration of the dispersoid particles in the dispersion is 0.1 to 50 mass %. [7]

[0062] The dispersion according to any one of [1] to [6], wherein the liquid medium is water or an organic solvent. [8]

[0064] A coating composition comprising the dispersion according to any one of [1] to [7] and a resin. [9]

[0066] According to the coating composition described in [8], the resin is in the form of a resin emulsion, which is in the form of an oil-in-water emulsion or an oil-in-water emulsion, and is a resin emulsion containing one or more resin components selected from acrylic resins, acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, styrene resins, olefin resins, ethylene-vinyl acetate resins, ester resins, epoxy resins, phenolic resins, amide resins, vinyl alcohol resins, fluorine resins, polyurethane resins, melamine resins, phthalic acid resins, silicone resins, alkyd resins and vinyl chloride resins.

[10]

[0068] According to the coating composition described in [8], the resin is in the form of a water-soluble polymer or a colloidal dispersion, and is a water-soluble resin or a colloidal dispersion containing one or more resin components selected from acrylic resins, acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, styrene resins, olefin resins, ethylene-vinyl acetate resins, ester resins, epoxy resins, phenolic resins, amide resins, vinyl alcohol resins, fluorine resins, polyurethane resins, melamine resins, phthalic acid resins, silicone resins, alkyd resins and vinyl chloride resins.

[11]

[0070] The coating composition according to any one of [8] to

[10] , wherein the ratio of the solid content in the dispersion to the resin is 1:0.1 to 20 in terms of the mass ratio of (solid content in the dispersion):(resin), and the ratio of the total solid content in the coating composition is 1 to 70 mass %.

[12]

[0072] The coating composition according to any one of [8] to

[11] , further comprising a slurry of the inorganic oxide powder, wherein the slurry has a solid content concentration of 0.1 to 50% by mass.

[13]

[0074] According to the coating composition described in

[12] , the ratio of the solid content in the dispersion, the resin and the solid content of the slurry of the inorganic oxide powder is 1:0.1~20:0.1~1 in terms of the mass ratio of (solid content in the dispersion):(resin):(solid content of the slurry), and the proportion of the total solid content in the coating composition is 1~70% by mass.

[14]

[0076] A coating film of the coating composition according to any one of [8] to

[13] , wherein the film thickness is 0.1 μm to 100 μm.

[15]

[0078] The coating film according to

[14] is a spin coating film, a bar coating film, a roller coating film or a dip coating film.

[16]

[0080] The method for producing a dispersion according to any one of [1] to [7], further comprising the step of mixing the inorganic oxide powder and the zinc cyanurate particles or the slurry thereof in a liquid medium using a pulverizing device.

[17]

[0082] According to the production method described in

[16] , the pulverizing device is a ball mill, a bead mill or a sand mill.

[18]

[0084] The method for producing a dispersion according to any one of [1] to [7], further comprising the step of mixing the pre-crushed inorganic oxide powder and the zinc cyanurate particles or the slurry thereof in a liquid medium using a pulverizing device.

[19]

[0086] The method for producing a coating composition according to any one of [8] to

[13] , comprising the step of mixing the dispersion according to any one of [1] to [7] and the resin using a liquid disperser.

[20]

[0088] The method for producing a coating composition according to

[12] or

[13] comprises the step of mixing the dispersion according to any one of [1] to [7], the resin and the slurry of the inorganic oxide powder using a liquid disperser. [twenty one]

[0090] According to the method for producing a coating composition described in

[19] or

[20] , the liquid disperser is a stirrer, a rotary shearing stirrer, a colloid mill, a roller mill, a high-pressure jet disperser, an ultrasonic disperser, a container-driven mill, a medium stirring mill or a kneader.

[0091] Furthermore, the present invention relates to a dispersion liquid containing specific colloidal metal oxide particles and zinc cyanurate particles. That is, the present invention includes the following <1> ~ <17> way.

[0092] <1>

[0093] A dispersion liquid is obtained by dispersing dispersoid particles containing colloidal metal oxide particles and zinc cyanurate particles in a liquid medium, wherein the colloidal metal oxide particles are colloidal metal oxide particles excluding particles containing colloidal silicon dioxide as a main component.

[0094] <2>

[0095] according to <1> The dispersion described above, wherein the colloidal metal oxide particles contain an oxide of at least one atom selected from the group consisting of Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

[0096] <3>

[0097] according to <2> The dispersion described above, wherein the colloidal metal oxide particles contain a composite oxide or a mixed oxide of two or more atoms selected from Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

[0098] <4>

[0099] according to <1> ~ <3> The dispersion according to any one of the above, wherein the zinc cyanurate particles have a primary particle major axis of 400 nm to 3,000 nm and a primary particle minor axis of 10 nm to 300 nm, and a ratio of the major axis to the minor axis of 1.3 to 300 when measured using a transmission electron microscope.

[0100] <5>

[0101] according to <1> ~ <4> The dispersion according to any one of the above, wherein the dispersoid particles in the dispersion have an average particle size of 80 nm to 5,000 nm when measured by laser diffraction, and the solid content concentration of the dispersoid particles in the dispersion is 0.1 to 50% by mass.

[0102] <6>

[0103] according to <1> ~ <5> The dispersion according to any one of the above, wherein the dispersoid particles include inorganic oxide particles and zinc cyanurate particles at a mass ratio of 1:0.01 to 100, and the solid content concentration of the dispersoid particles in the dispersion is 0.1 to 50% by mass.

[0104] <7>

[0105] according to <1> ~ <6> The dispersion according to any one of items , wherein the liquid medium is water or an organic solvent.

[0106] <8>

[0107] A coating composition comprising <1> ~ <7> The dispersion according to any one of items and a resin.

[0108] <9>

[0109] according to <8> The coating composition described herein is a resin emulsion in the form of an oil-in-water emulsion or a water-in-oil emulsion, and is a resin emulsion containing one or more resin components selected from acrylic resins, acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, styrene resins, olefin resins, ethylene-vinyl acetate resins, ester resins, epoxy resins, phenolic resins, amide resins, vinyl alcohol resins, fluorine resins, polyurethane resins, melamine resins, phthalic acid resins, silicone resins, alkyd resins and vinyl chloride resins.

[0110] <10>

[0111] according to <8> The coating composition described herein is a water-soluble polymer or a colloidal dispersion, wherein the resin is in the form of a water-soluble polymer or a colloidal dispersion, and is a water-soluble resin or a colloidal dispersion containing one or more resin components selected from acrylic resins, acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, styrene resins, olefin resins, ethylene-vinyl acetate resins, ester resins, epoxy resins, phenolic resins, amide resins, vinyl alcohol resins, fluorine resins, polyurethane resins, melamine resins, phthalic acid resins, silicone resins, alkyd resins and vinyl chloride resins.

[0112] <11>

[0113] according to <8> ~ <10> The coating composition according to any one of the above, wherein the ratio of the solid content in the dispersion to the resin is 1:0.1 to 20 in terms of the mass ratio of (solid content in the dispersion):(resin), and the total solid content in the coating composition is 1 to 70 mass %.

[0114] <12>

[0115] A coating film is <8> ~ <11> The coating film of the coating composition according to any one of the above has a film thickness of 0.1 μm to 100 μm.

[0116] <13>

[0117] according to <12> The coating film described is a spin coating film, a bar coating film, a roller coating film or a dip coating film.

[0118] <14>

[0119] according to <1> ~ <7> The method for producing a dispersion according to any one of the above, comprising the step of mixing colloidal metal oxide particles and zinc cyanurate particles or a slurry thereof in a liquid medium using a pulverizing device.

[0120] <15>

[0121] according to <14> The production method described herein, wherein the pulverizing device is a ball mill, a bead mill or a sand mill.

[0122] <16>

[0123] according to <8> ~ <11> The method for producing a coating composition according to any one of the preceding claims, comprising using a liquid disperser to <1> ~ <7> A step of mixing the dispersion described in any one of items and the resin.

[0124] <17>

[0125] according to <16> The method for producing a coating composition described herein, wherein the liquid disperser is a stirrer, a rotary shearing type stirrer, a colloid mill, a roll mill, a high-pressure jet disperser, an ultrasonic disperser, a container-driven mill, a media stirring mill or a kneader.

[0126] The coating composition of the present invention can uniformly contain zinc cyanurate particles and inorganic oxide particles in a coating film obtained by applying the coating composition to a coating surface, and can obtain a coating film having excellent adhesion and excellent hardness.

[0127] The coating additive used in the coating composition of the present invention is in the form of a dispersion liquid with high dispersion stability of both inorganic oxide particles and zinc cyanurate particles as dispersoid particles, and has high dispersibility that no precipitate is seen even when left to stand for several days at room temperature. Moreover, the coating additive (dispersion liquid) obtained by dispersing inorganic oxide particles and zinc cyanurate particles in a liquid medium has the following effects: even after mixing it with a resin component such as a resin emulsion, it also maintains good stability, and has high operability when manufacturing a coating composition, etc. Moreover, in the obtained coating composition, zinc cyanurate particles and inorganic oxide particles maintain a stable dispersion state, and in the coating film obtained by applying it to the coated surface, zinc cyanurate particles and inorganic oxide particles can be uniformly present, and the above-mentioned coating film with excellent adhesion can be obtained. Furthermore, in the case of using a substrate with high transparency such as a resin film such as a PET film or glass, a coating film with excellent adhesion can be obtained while maintaining the transparency of the substrate.

[0128] In addition, the coating film of the coating composition of the present invention exhibits the corrosion protection and other functions inherent in zinc cyanurate, the hydrophilicity, lubricity, insulation, thermal conductivity, photocatalysis and other functions possessed by the inorganic oxide particles, and the weather resistance, light resistance, water resistance, scratch resistance, substrate corrosion resistance, prevention of substrate color change and other functions of the coating composition, and can be expected to contribute to the prevention of substrate degradation. BRIEF DESCRIPTION OF THE DRAWINGS

[0129] Figure 1 This is a graph showing an approximate curve obtained based on the measured value of the zeta potential (mV) of the inorganic oxide particles relative to the pH value (pH 2 to 10 (horizontal axis)) of the water-dispersed slurry in which the inorganic oxide powder is silica powder (fumed silica A, fumed silica B, silica powder C) or titanium dioxide powder (titanium dioxide powder). DETAILED DESCRIPTION

[0130] The present invention relates to a coating composition comprising a coating additive and a resin emulsion. The coating additive comprises a dispersion liquid, and the dispersion liquid is obtained by dispersing dispersoid particles comprising inorganic oxide particles and zinc cyanurate particles in a liquid medium.

[0131] [Coating Additives]

[0132] The coating additive used in the coating composition of the present invention includes a dispersion liquid, wherein dispersoid particles including inorganic oxide particles and zinc cyanurate particles are dispersed in a liquid medium.

[0133] Furthermore, when the coating additive of the present invention is composed only of a dispersion obtained by dispersoid particles containing inorganic oxide particles and zinc cyanurate particles being dispersed in a liquid medium, the dispersion can be treated as a coating additive. Therefore, in this case, the coating additive is sometimes interpreted as the dispersion in the following description.

[0134] <Inorganic Oxide Particles>

[0135] As inorganic oxide particles constituting the dispersoid particles, there can be mentioned particles of oxides of at least one atom selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce. The inorganic oxide particles are particles of oxides of atoms having a valence of 2 to 6, and examples of the oxide forms of these atoms include SiO2, TiO2, Fe2O3, CuO, ZnO, Y2O3, ZrO2, Nb2O5, MoO3, In2O3, SnO2, Sb2O5, Ta2O5, WO3, PbO, Bi2O3, CeO2, etc. These inorganic oxides can be used alone or in combination of multiple types.

[0136] As a combination method, a method of mixing a plurality of the above-mentioned inorganic oxides, a method of compositely forming two or more of the above-mentioned inorganic oxides, or a method of solid-solutionizing two or more of the above-mentioned inorganic oxides at the atomic level can be cited. That is, the inorganic oxide particles can be particles of a single oxide of one atom selected from the above-mentioned atomic groups, particles of a composite oxide of two or more atoms selected from the same group, and any mixture of these particles (a mixture of single oxide particles, a mixture of composite oxide particles, a mixture of single oxide particles and composite oxide particles, etc., which are collectively referred to as mixed oxides).

[0137] As the above-mentioned composite oxide particles, for example, TiO2-SnO2 composite oxide particles in which TiO2 particles and SnO2 particles are chemically bonded at their interfaces to form a composite, SnO2-WO3 composite oxide particles in which SnO2 particles and WO3 particles are chemically bonded at their interfaces to form a composite, SnO2-SiO2 composite oxide particles in which SnO2 particles and SiO2 particles are chemically bonded at their interfaces to form a composite, SnO2 particles, WO3 particles and SiO2 particles are chemically bonded at their interfaces to form a composite, and SnO2-SnO2 composite oxide particles in which SnO2 particles, WO3 particles and SiO2 particles are chemically bonded at their interfaces to form a composite. SnO2-WO3-SiO2 composite oxide particles, SnO2 particles, MoO3 particles and SiO2 particles formed by chemical bonds at their interfaces to form a composite SnO2-MoO3-SiO2 composite oxide particles, Sb2O5 particles and SiO2 particles formed by chemical bonds at their interfaces to form a composite Sb2O5-SiO2 composite oxide particles, TiO2-SnO2-ZrO2 composite oxide particles obtained by forming a solid solution of TiO2, SnO2 and ZrO2 at the atomic level, etc., but are not limited to these.

[0138] The inorganic oxide particles include inorganic oxide powders, colloidal inorganic oxide particles (also referred to as inorganic oxide colloidal particles), and the like, and any of the forms can be used.

[0139] The inorganic oxide powder mentioned here may have a specific surface area of ​​1 to 800 m 2 / g, loose bulk density is 0.03~3.0g / cm 3 For example, a powder having a specific surface area of ​​10 to 700 m 2 / g, 30~500m 2 / g, 40~300m 2 / g, and for example, the loose bulk density is 0.03 to 1.0 g / cm 3 , 0.05~0.8m 2 / g, 0.05~0.5m 2 / g, 0.05~0.2m 2 The loose bulk density is defined as the ratio of the mass of the powder sample in an uncompacted (loose) state to the volume of the powder including the factor of the inter-particle gap volume.

[0140] Alternatively, the colloidal inorganic oxide particles may be used in the form of an inorganic oxide sol in which the inorganic oxide particles are dispersed in a liquid medium.

[0141] The inorganic oxide particles can be produced by selecting an appropriate production method according to their type, and can be produced by a known method, which can be roughly divided into a liquid phase method (hydrolysis method, sol-gel method, hydrothermal method, coprecipitation method, freeze drying method, etc.), a gas phase method (melting method, spray drying method, gas phase reaction method (combustion hydrolysis, etc.), etc.

[0142] When the inorganic oxide particles are colloidal inorganic oxide particles, the particles can be produced by a known method (eg, ion exchange method, deflocculation method, hydrolysis method, reaction method (oxidation method), etc.) Furthermore, the obtained colloidal particles can be dried before use.

[0143] As an example of the above-mentioned ion exchange method, there can be mentioned a method of treating the acid salt of the above-mentioned atom with a hydrogen-type ion exchange resin, or a method of treating the basic salt of the above-mentioned atom with a hydroxyl-type anion exchange resin. As an example of the above-mentioned deflocculation method, there can be mentioned a method of neutralizing the acid salt of the above-mentioned atom with a base, or washing the gel obtained by neutralizing the basic salt of the above-mentioned atom with an acid and then deflocculating with an acid or a base. As an example of the above-mentioned hydrolysis method, there can be mentioned a method of hydrolyzing the alcohol salt of the above-mentioned atom, or a method of removing unnecessary acid after hydrolyzing the basic salt of the above-mentioned atom under heating. As an example of the above-mentioned reaction method (oxidation method), there can be mentioned a method of reacting the above-mentioned atom or inorganic oxide powder with an acid (for example, hydrogen peroxide).

[0144] The inorganic oxide particles may be in the form of modified inorganic oxide particles (surface-treated) having the inorganic oxide particles as cores and at least a portion of the surface thereof covered with a covering composed of other inorganic oxide particles.

[0145] In this case, the inorganic oxide particles serving as the coating may be any of the above-mentioned inorganic oxides (single oxide, composite oxide, mixed oxide), and the production method thereof may be appropriately selected from the above-mentioned known production methods.

[0146] The modified inorganic oxide particles can be produced by a conventionally known method, for example, a method of heating after mixing the inorganic oxide particles A as the core and the other inorganic oxide particles B as the coating. In this case, for example, the inorganic oxide particles A as the core and the other inorganic oxide particles B as the coating are mixed at a temperature of 0 to 100° C., for example, at room temperature to 60° C., and the heating after mixing can be performed at, for example, 70 to 300° C.

[0147] Among these inorganic oxide particles (in the case of modified inorganic oxide particles, the inorganic oxide particles serving as the core thereof) there can be mentioned oxide particles of at least one atom selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce, preferably oxide particles of at least one atom selected from Si, Al, Ti, Zr, Sn, Cu and Zn, composite oxide particles of two or more atoms selected from the above, or particles of mixed oxides.

[0148] The shape of the inorganic oxide particles is not particularly limited, and may be spherical, polyhedral, square, hollow, core-shell, porous, rod-shaped, plate-shaped or amorphous, and preferably spherical, hollow, core-shell or porous.

[0149] The average particle size of the inorganic oxide particles (in the case of modified inorganic oxide particles, the entire particle consisting of a core and a coating) can be measured by a laser diffraction method or a dynamic light scattering method.

[0150] For example, when the inorganic oxide particles are in the form of inorganic oxide powder, the powder can be dispersed in a suitable medium and measured by laser diffraction. The average particle size of the inorganic oxide powder obtained by laser diffraction can be, for example, in the range of 500 nm to 100 μm, 1.0 μm to 80 μm, or 1.0 μm to 50 μm.

[0151] In addition, for example, when the inorganic oxide particles are in the form of colloidal inorganic oxide particles, the dynamic light scattering method (DLS method) can be used for measurement. The average particle size of the colloidal inorganic oxide particles obtained by the dynamic light scattering method is, for example, in the range of 5 nm to 500 nm, or can be in the range of 5 nm to 200 nm, or 5 nm to 100 nm, or 5 nm to 50 nm, or 3 nm to 300 nm, 3 nm to 200 nm, or 3 nm to 100 nm.

[0152] As described above, the inorganic oxide particles can be used in the form of colloidal inorganic oxide particles or in the form of an inorganic oxide sol in which the colloidal inorganic oxide particles are dispersed in a liquid medium. The concentration of the inorganic oxide in the inorganic oxide sol can be in the range of 0.1 mass % to 40 mass %, or 0.1 mass % to 20 mass %, or 0.1 mass % to 10 mass %.

[0153] As the liquid medium, a medium used in the dispersion described below, that is, an aqueous medium such as water, an organic solvent such as alcohol, glycol, ester, ketone, nitrogen-containing solvent, aromatic solvent, or a mixed solvent of an organic solvent and water can be used.

[0154] As the inorganic oxide particles, commercially available products can be used. Examples thereof include the following products, but the present invention is not limited thereto.

[0155] For example, commercially available inorganic oxide powders include AEROSIL (registered trademark) series (silicon oxide), AEROXIDE (registered trademark) Alu series (aluminum oxide), AEROXIDE (registered trademark) TiO2 series (titanium oxide), and AEROXIDE (registered trademark) STX series (titanium oxide (core)-silicon oxide (shell) composite) manufactured by AEROSIL Co., Ltd. of Japan; Cab-O-SIL (registered trademark) series (silicon oxide) and SpectrAl (registered trademark) series (aluminum oxide) manufactured by Cabot Corporation; NanoTek (registered trademark) (aluminum oxide, titanium oxide, tin oxide, zirconium oxide, zinc oxide, and copper oxide) manufactured by CIKNanoTek Co., Ltd.; Sylysia (registered trademark) series (silicon oxide) manufactured by Fuji Silicon Chemical Co., Ltd.; Reolosil (registered trademark) series and EXCELICA (registered trademark) series (silicon oxide) manufactured by Tokuyama Co., Ltd.; and WACKER HDK (registered trademark) series (silicon oxide) manufactured by SILICONE Co., Ltd.; AKP (registered trademark) series (alumina) manufactured by Sumitomo Chemical Co., Ltd.; Taimicron series (alumina) manufactured by Daming Chemical Co., Ltd.; DISPERAL (registered trademark) series and DISPAL (registered trademark) series (alumina) manufactured by Sasol; titanium oxide and zinc oxide manufactured by Sakai Chemical Co., Ltd.; titanium oxide, zinc oxide, and tin oxide manufactured by Ishihara Sangyo Co., Ltd.; zirconium oxide manufactured by Dai-ichi Rare Element Chemical Co., Ltd.; zirconium oxide manufactured by Shin Nippon Electric Industries, Ltd., etc.

[0156] Examples of commercially available colloidal inorganic oxide particles include Snowtex (registered trademark) (silica sol) ST-N-40, ST-XS, ST-OXS, ST-S, T-OS, ST-30, ST-O, ST-N, ST-C, ST-30L, ST-OL, ST-OYL, ST-ZL, etc. manufactured by Nissan Chemical Co., Ltd., and alumina sol 100 (AS-100), AS-200 (AS-200), AS-520-A (AS-520A0) ( Alumina water dispersion), NanoUse (registered trademark) (zirconium dioxide sol) ZR-30BS, same as ZR-30AH, ZR-40BL, same as ZR-30AL, etc.; NanoTek (registered trademark) manufactured by CIKNanoTek (Co., Ltd.) (alumina, titanium oxide, tin oxide, zirconium oxide, zinc oxide, copper oxide: solvent dispersion), etc.; titanium oxide sol, SN-100D (antimony-doped tin oxide water dispersion sol), etc. manufactured by Ishihara Sangyo Co., Ltd.; silica manufactured by Nippon Chemical Industry Co., Ltd. doll (registered trademark), etc.; ADELITE (registered trademark) AT series manufactured by ADEKA Co., Ltd.; Cataloid (registered trademark) S series manufactured by Nikko Catalysts & Chemicals Co., Ltd.; Quartron (registered trademark), etc. manufactured by Fuso Chemical Co., Ltd.; titanium oxide, etc. manufactured by Tayca Co., Ltd.; alumina sol, etc. manufactured by Kawaken Fine Chemicals Co., Ltd.; neededal (cerium oxide aqueous dispersion), etc. manufactured by Taki Chemical Co., Ltd.; Cataloid (registered trademark) A series (alumina aqueous dispersion sol), Neosunveil (registered trademark) PW (titanium oxide aqueous dispersion sol), etc. manufactured by Nikko Catalysts & Chemicals Co., Ltd.

[0157] Furthermore, when the above-mentioned inorganic oxide particles are in the form of inorganic oxide powder or in the form of a mixture of inorganic oxide powder and inorganic oxide colloidal particles, the above-mentioned inorganic oxide powder can be replaced by inorganic nitrides, inorganic oxynitrides, inorganic sulfides, inorganic hydrides, inorganic carbides, inorganic chlorides, (poorly soluble) inorganic hydroxides, poorly soluble organic polymer particles, organic polymer-coated inorganic powders, inorganic fibers (glass fibers), and powders of inorganic clay minerals, and these powders and inorganic oxide powders can be used in combination.

[0158] The above-mentioned inorganic powder may contain various atoms listed in the aforementioned inorganic oxide powder (inorganic oxide particles), that is, at least one atom selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi, and Ce.

[0159] The specific surface area, apparent bulk density, shape and average particle size of these powders may be those listed for the above-mentioned inorganic oxide powders.

[0160] <Zinc Cyanurate Particles>

[0161] Cyanuric acid is a tribasic acid, and acid salts, neutral salts, and basic salts can be produced by reacting with divalent zinc. For example, when the molar ratio of (zinc oxide) / (cyanuric acid) is 1.0, an acid salt equivalent to Zn(C3N3O3H) is formed. When the molar ratio of (zinc oxide) / (cyanuric acid) is 1.5, a neutral salt equivalent to Zn3(C3N3O3)2 is formed. When the molar ratio of (zinc oxide) / (cyanuric acid) is 2.5, a basic salt equivalent to Zn3(C3N3O3)2·2ZnO is formed. These salts may contain water of crystallization, and may, for example, form monohydrated salts, dihydrated salts, and trihydrated salts.

[0162] In the present invention, the zinc cyanurate particles can use particles having a molar ratio of (zinc oxide) / (cyanuric acid) of 1.0 to 5.0.

[0163] As the zinc source, zinc oxide or basic zinc carbonate can be mentioned, and they can be used in the above-mentioned molar ratio when converted into zinc oxide. As zinc oxide, for example, two types of zinc oxide manufactured by Sakai Chemical Industry Co., Ltd. can be used.

[0164] In the present invention, it is preferred to use a basic salt, for example, Zn3(C3N3O3)2·2ZnO·3H2O can be used.

[0165] The zinc cyanurate particles have a needle-like or plate-like elongated particle shape. In the present invention, it is preferred to use zinc cyanurate particles whose major axis length of the primary particles is 400 nm to 3,000 nm and whose minor axis length is 10 nm to 300 nm when measured by transmission electron microscopy, and whose major axis to minor axis length ratio (major axis / minor axis) is 1.3 to 300. In addition, zinc cyanurate particles whose specific surface area is, for example, 10 m 2 / g~100m 2 / g of particles.

[0166] For example, zinc cyanurate particles can be preferably used in which the length of the major axis of the primary particle is 400 nm to 1,000 nm, or 400 nm to 800 nm, or 400 nm to 600 nm, in which case the length of the minor axis of the primary particle diameter is 10 to 300 nm, or 10 nm to 90 nm, or 30 nm to 90 nm, and in which the length ratio of the major axis to the minor axis (major axis / minor axis) is 1.3 to 100. Furthermore, the length ratio of the major axis to the minor axis can be selected from any combination of the lower limit of 1.3 or 4.4 and the upper limit of 12, 20, 80 or 100.

[0167] In addition, for example, zinc cyanurate particles can be preferably used in which the length of the major axis of the primary particle is 1,000 nm to 3,000 nm, or 2,000 nm to 3,000 nm, the length of the minor axis of the primary particle diameter is 80 to 300 nm, or 100 nm to 300 nm, and the length ratio of the major axis to the minor axis (major axis / minor axis) is 3.3 to 37.5. Furthermore, the length ratio of the major axis to the minor axis can be selected from any combination of 3.3 as the lower limit and 20 or 37.5 as the upper limit.

[0168] The zinc cyanurate particles can be dispersed in pure water or a dispersion containing the particles, and the average particle size of the zinc cyanurate particles in the aqueous dispersion can be measured using a laser diffraction particle size distribution analyzer (for example, SALD-7500nano, manufactured by Shimadzu Corporation).

[0169] When measured by laser diffraction method, the average particle size of the zinc cyanurate particles in the aqueous dispersion is 80 nm to 20,000 nm.

[0170] There are two methods for producing zinc cyanurate particles: a method of subjecting the raw materials to a liquid phase reaction in a slurry state dispersed in water, and a method of subjecting the raw materials to a solid phase reaction in a powder state.

[0171] The manufacturing method of subjecting the raw materials to a liquid phase reaction in a slurry state dispersed in water is, for example, the following method: zinc oxide or basic zinc carbonate, cyanuric acid and water are prepared so that the cyanuric acid concentration becomes 0.1 mass % to 10.0 mass %, and the mixed slurry is wet dispersed at a temperature of 5° C. to 55° C. using a liquid disperser, thereby reacting and dispersing the product to obtain a slurry (dispersion liquid) of zinc cyanurate particles.

[0172] Furthermore, cyanuric acid dissolved in water reacts rapidly with zinc oxide and basic zinc carbonate to promote particle growth, so the resulting zinc cyanurate particles tend to become larger. Therefore, the reaction is preferably performed at 55°C or lower or 45°C or lower.

[0173] Wet dispersion is performed using a dispersion medium. By performing wet dispersion using a dispersion medium, mechanical energy generated by collision of the dispersion medium can cause at least one selected from zinc oxide and basic zinc carbonate to undergo a mechanochemical reaction with cyanuric acid. The so-called mechanochemical reaction refers to the application of mechanical energy to zinc oxide, basic zinc carbonate, and cyanuric acid from multiple aspects through collision of the dispersion medium to cause a chemical reaction.

[0174] As the dispersion medium, for example, stabilized zirconia beads, fused silica beads, soda-lime glass beads, alumina beads, and mixtures thereof can be mentioned. In consideration of the contamination caused by the breakage of the dispersion medium due to the collision of the dispersion media with each other, glass beads or stabilized zirconia beads are preferably used as the dispersion medium. The size of the dispersion medium can be, for example, a diameter of 0.1 mm to 10 mm, preferably a diameter of 0.5 mm to 2.0 mm. When the diameter of the dispersion medium is less than 0.1 mm, the collision energy between the grinding media is small, and there is a tendency for the mechanochemical reaction to weaken. In addition, when the diameter of the dispersion medium is greater than 10 mm, the collision energy between the dispersion media is too large, the dispersion medium breaks, and the contamination increases, so it is not preferred.

[0175] As the apparatus (grinding apparatus) for wet dispersion using a dispersion medium, there is no particular limitation as long as it is an apparatus capable of causing a mechanochemical reaction between zinc oxide and / or basic zinc carbonate and cyanuric acid by adding a mixed slurry to a container containing the dispersion medium and then stirring to cause the dispersion medium to collide with zinc oxide, basic zinc carbonate, and / or cyanuric acid. For example, a sand mill (manufactured by AIMEX Co., Ltd.), Apex Mill (manufactured by Hiroshima Metal & Machinery Co., Ltd. (formerly manufactured by Hisa Industries Co., Ltd.)), Attritor mill (manufactured by Nippon Coke & Engineering Co., Ltd.), pearl mill (manufactured by Ashizawa Finetech Co., Ltd.), and other ball mills, bead mills, sand mills, etc. can be mentioned. Furthermore, the rotation speed, reaction time, etc. of the apparatus for stirring the dispersion medium can be appropriately adjusted in accordance with the desired particle size, etc.

[0176] In the obtained zinc cyanurate particle dispersion, the zinc cyanurate particles are contained in the dispersion (slurry) as a solid component in a range of 0.10% by mass to 50% by mass, 0.1% by mass to 20% by mass, 0.1% by mass to 10% by mass, or 0.1% by mass to 5% by mass.

[0177] In addition, in order to reduce the particle size of the obtained zinc cyanurate particles, a grinding treatment step can be performed on the zinc cyanurate particles using the above-mentioned grinding treatment apparatus. Furthermore, the rotation speed, reaction time, etc. of the apparatus for stirring the dispersion medium can be appropriately adjusted in accordance with the desired particle size, etc.

[0178] When the zinc cyanurate particles obtained by this production method are measured by observation with a transmission electron microscope, for example, the major axis length of the primary particles is 100 nm to 800 nm, and the minor axis length of the primary particles is 10 nm to 60 nm, and the length ratio of the major axis to the minor axis (major axis / minor axis) is 5 to 25, and the average particle size measured by the laser diffraction method is 80 nm to 900 nm. The specific surface area of the zinc cyanurate particles obtained by drying the aqueous dispersion slurry of the zinc cyanurate particles at 110 °C is 10 m 2 / g to 100 m 2 / g.

[0179] In addition, a manufacturing method in which the raw materials undergo a solid phase reaction in a powder state, for example, a method in which a mixed powder is heated at 30°C to 300°C in a closed or open state, wherein the mixed powder is composed of zinc oxide with a sieve residue of less than 1% at a mesh size of 1,000 μm, cyanuric acid, and water, the molar ratio of zinc oxide to cyanuric acid is 2 to 3, and the moisture content of the mixed powder is 9% to 18% by mass.

[0180] The obtained zinc cyanurate particles contain about 10% by mass of water, so they are heat-treated in an open state to remove the water, forming zinc cyanurate particles having a water content of less than 1.0% by mass (a commercial product is, for example, the trade name Star Fine manufactured by Nissan Chemical Co., Ltd.), which can be used for the dispersion (coating additive) described later. In the case of industrial large-scale production, the heat treatment is preferably carried out using a powder mixer having a mixing unit and a heating unit. As specific examples, a vibration dryer, a Henschel mixer, a Loedige mixer, a Nauta conical screw mixer, a rotary kiln, and the like can be cited as a heated reaction tank that can be stirred and mixed in an open or closed manner.

[0181] In order to reduce the particle size of the obtained zinc cyanurate particles, the zinc cyanurate particles may be subjected to a pulverization step using the pulverization device. The rotation speed of the device for stirring the dispersion medium, the reaction time, etc. may be appropriately adjusted in accordance with the desired particle size, etc.

[0182] The zinc cyanurate particles obtained by the production method have a sieve residue of, for example, 400 μm mesh less than 10% by mass, a major axis length of the primary particles of 400 nm to 3,000 nm when measured by a transmission electron microscope, a minor axis length of the primary particles of 10 nm to 300 nm, a length ratio of the major axis to the minor axis (major axis / minor axis) of 1.3 to 300, and an average particle size of 0.5 μm to 20 μm when measured by a laser diffraction method. In addition, the specific surface area of ​​the obtained zinc cyanurate particles is, for example, 10 m 2 / g~100m 2 / g.

[0183] The surface charge of the obtained zinc cyanurate particles is negative in the pH range of 3 to 10 in an aqueous system. Therefore, not only is the dispersibility in water good in the acidic to alkaline region, but also the compatibility with synthetic resins and emulsions when preparing an aqueous rust-proof paint (paint composition, etc.) is good, and a stable aqueous rust-proof paint can be obtained.

[0184] <Method for producing dispersion (coating additive)>

[0185] The method for producing the above-mentioned dispersion is not particularly limited, and the above-mentioned dispersion can be obtained, for example, by mixing inorganic oxide particles with zinc cyanurate particles or a slurry thereof in a liquid medium using a pulverizing device. Furthermore, when an inorganic oxide powder is used as the inorganic oxide particles, it can be pre-pulverized and mixed with zinc cyanurate or a slurry thereof in a liquid medium using a pulverizing device to form a dispersion.

[0186] As an apparatus for mixing the inorganic oxide particles and the zinc cyanurate particles to obtain a dispersion, i.e., a coating additive, the same apparatus (crushing apparatus, dispersion medium) as the apparatus for wet dispersion of zinc cyanurate using the aforementioned dispersion medium can be used. Specifically, a ball mill, a bead mill, a sand mill, etc. such as a sand mill (manufactured by AIMEX Co., Ltd.), Apex Mill (manufactured by Hiroshima Metal & Machinery Co., Ltd. (manufactured by Harajuku Industry Co., Ltd.), Attritor mill (manufactured by Nippon Coke Industry Co., Ltd.), and a pearl mill (manufactured by Ashizawa Finetech Co., Ltd.) can be used. In addition, the rotation speed of the apparatus for stirring the dispersion medium, the reaction time, etc. can be appropriately adjusted in accordance with the desired particle size, etc.

[0187] In the dispersion (paint additive) obtained by dispersoid particles containing the obtained inorganic oxide particles and zinc cyanurate particles being dispersed in a liquid medium, the average particle size of the dispersoid particles when measured by laser diffraction method can be, for example, 80nm to 5,000nm, 80nm to 2,000nm, 200nm to 5,000nm, 80nm to 1,000nm or 10nm to 500nm.

[0188] In addition, when the inorganic oxide particles are in the form of inorganic oxide powder, in the dispersion obtained by dispersoid particles containing the obtained inorganic oxide powder and zinc cyanurate particles being dispersed in a liquid medium, the average particle size of the dispersoid particles when measured by laser diffraction method can be, for example, 200nm to 5,000nm, 300nm to 5,000nm, 1,000nm to 5,000nm, 1,000nm to 3,000 or 1,000nm to 2,000nm.

[0189] In the dispersion (coating additive), the inorganic oxide particles and the zinc cyanurate particles may be, for example, in a ratio of 1:0.01 to 100, 1:0.1 to 10, or 1:1 to 10 in terms of the mass ratio of the inorganic oxide to the zinc cyanurate. In addition, in the dispersion (coating additive), the concentration of the solid content (solid content of the dispersoid particles) of the total of the inorganic oxide particles and the zinc cyanurate particles may be, for example, 0.1% to 50% by mass, 0.1% to 30% by mass, 0.1% to 20% by mass, or 0.1% to 10% by mass.

[0190] The B-type viscosity of the dispersion (coating additive) may be, for example, 1 mPa·s to 500 mPa·s, 5 mPa·s to 500 mPa·s, 10 mPa·s to 300 mPa·s, or 50 mPa·s to 300 mPa·s.

[0191] Furthermore, zinc cyanurate dissolves in an acidic liquid, so when mixing zinc cyanurate particles and inorganic oxide particles, it is preferred to adjust the pH of the liquid to alkaline to neutral and perform a mixing operation (wet pulverization process) of these particles. In addition, the zeta potential of zinc cyanurate particles is -10 mV to -1 mV when the pH value is alkaline to neutral.

[0192] In addition, when obtaining the above-mentioned dispersion, for example, when using inorganic oxide particles having an isoelectric point at pH 5 to 12 and a zeta potential of -80 mV to +80 mV in this pH range, by adjusting the pH value so that the pH range becomes -5 mV to -80 mV, a dispersion with excellent dispersibility can be obtained.

[0193] Alternatively, when obtaining the above-mentioned dispersion, by using inorganic oxide particles that do not have an isoelectric point at pH 5 to 12 and have a zeta potential of -5 mV to -50 mV in the pH range, a dispersion having excellent dispersibility can be obtained.

[0194] In addition, when obtaining the above-mentioned dispersion, when inorganic oxide particles that do not have an isoelectric point at a pH value of 5 to 12 and have a zeta potential of +5 mV to +80 mV in this pH range are mixed with zinc cyanurate particles, a dispersion with excellent dispersibility can be obtained by adjusting the concentration of dispersoid particles containing the inorganic oxide particles and the cyanuric acid particles to 0.1 mass % to 20 mass % or 0.1 mass % to 10 mass %.

[0195] For example, when the inorganic oxide particles mixed with the zinc cyanurate particles are silica powder in the form of an inorganic oxide powder, the concentration of the dispersoid particles containing silica powder and zinc cyanurate particles is 0.1% to 20% by mass, and the mass ratio of silica to zinc cyanurate (silicon dioxide: zinc cyanurate) is adjusted to 1:0.1 to 10 to perform the mixing operation. In the case of titanium oxide powder, when it is mixed with zinc cyanurate particles in an alkaline region relative to the isoelectric point, the concentration of the dispersoid particles containing titanium oxide powder and zinc cyanurate particles is 0.1% to 20% by mass, and the mass ratio of titanium oxide to zinc cyanurate (titanium oxide: zinc cyanurate) is adjusted to 1:0.1 to 10. In the case of aluminum oxide powder, when it is mixed with zinc cyanurate particles in an acidic region relative to the isoelectric point, the concentration of the dispersoid particles containing aluminum oxide powder and zinc cyanurate particles is 0. .1 mass % to 10 mass %, and the mass ratio of aluminum oxide to zinc cyanurate (aluminum oxide: zinc cyanurate) is adjusted to 1: 1 to 10. In addition, in the case of zirconium oxide powder, when mixed with zinc cyanurate particles in an alkaline region closer to the isoelectric point, the concentration of the dispersoid particles containing zirconium oxide powder and zinc cyanurate particles is 0.1 mass % to 20 mass %, and the mass ratio of zirconium oxide to zinc cyanurate (zirconium oxide: zinc cyanurate) is adjusted to 1: 0.1 to 10, and the mixing operations are carried out separately.

[0196] For example, when the inorganic oxide particles to be mixed with the zinc cyanurate particles are alumina sol in the form of colloidal oxide particles [metal oxide particles (metal oxide sol)], when mixed with the zinc cyanurate particles in an acidic region closer to the isoelectric point, the concentration of the dispersoid particles containing the alumina particles and the zinc cyanurate particles is 0.1% by mass to 20% by mass, and the mixing operation is performed with the mass ratio of alumina to zinc cyanurate (alumina:zinc cyanurate) adjusted to 1:1 to 10. In the case of zirconium oxide sol, when it is mixed with zinc cyanurate particles in an alkaline region relative to the isoelectric point, the concentration of dispersed particles including zirconium oxide particles and zinc cyanurate particles is 0.1 mass % to 30 mass %, and the mass ratio of zirconium oxide to zinc cyanurate (zirconia: zinc cyanurate) is adjusted to 1:0.1 to 10. In the case of titanium dioxide sol, when it is mixed with zinc cyanurate particles in an alkaline region relative to the isoelectric point, the concentration of dispersed particles including titanium dioxide particles and zinc cyanurate particles is 0. 1 mass % to 30 mass %, and the mass ratio of titanium dioxide to zinc cyanurate (titanium dioxide: zinc cyanurate) is adjusted to 1:0.1 to 10. In addition, in the case of tin oxide sol, when mixed with zinc cyanurate particles in an alkaline region closer to the isoelectric point, the concentration of dispersoid particles containing tin oxide particles and zinc cyanurate particles is 0.1 mass % to 30 mass %, and the mass ratio of tin oxide to zinc cyanurate (tin oxide: zinc cyanurate) is adjusted to 1:0.1 to 10, and the mixing operation can be carried out separately.

[0197] In the dispersion (coating additive) obtained by dispersoid particles containing the obtained inorganic oxide particles and zinc cyanurate particles are dispersed in a liquid medium, the liquid medium can be selected from an aqueous medium or an organic solvent, and the aqueous medium can be replaced with an organic solvent by an evaporation method performed by a rotary evaporator or the like.

[0198] Examples of the aqueous medium include water.

[0199] As organic solvents, alcohols, ethylene glycol, esters, ketones, nitrogen-containing solvents, and aromatic solvents can be used. As these solvents, for example, organic solvents such as methanol, ethanol, propanol, ethylene glycol, propylene glycol, glycerol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, propylene glycol monoethyl ether acetate, acetone, methyl ethyl ketone, dimethylformamide, N-methyl-2-pyrrolidone, toluene, xylene, and dimethylethane can be exemplified. In addition, reactive diluent solvents containing polyethylene glycol, silicone oil, free radical polymerizable vinyl or epoxy groups, etc. can also be used.

[0200] Furthermore, the surface of the inorganic oxide particles can be treated with a silane coupling agent, and the silane coupling agent is tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethoxydiphenylsilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, decyltrimethoxysilane, octyltriethoxysilane, trimethylmonoethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane , 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-isocyanatepropyltriethoxysilane, hexamethyldisilazane, etc.

[0201] Furthermore, the object of the present invention also includes a mode in which the inorganic oxide particles in the dispersion liquid in which the dispersoid particles containing inorganic oxide particles and zinc cyanurate particles are dispersed in a liquid medium are the inorganic oxide powder. That is, the object of the present invention is a dispersion liquid in which the dispersoid particles containing inorganic oxide powder and zinc cyanurate particles are dispersed in a liquid medium, and the specific surface area of ​​the inorganic oxide powder is 1 to 800 m 2 / g, and the loose bulk density is 0.03~3.0g / cm 3 .

[0202] As described above, the above-mentioned inorganic oxide powder is a powder of an oxide of at least one atom selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

[0203] The inorganic oxide powder and zinc cyanurate particles contained in the present dispersion, their types and average particle sizes, the production method (apparatus, sequence, etc.), the mixing ratio in the dispersion, the type of liquid medium, etc. are as described above in the description of the inorganic oxide particles and cyanuric acid particles, etc.

[0204] In addition, the average particle size of the dispersoid particles in the present dispersion, the solid content concentration, the method for producing the dispersion, etc. are also as described above. Preferably, when measured by laser diffraction, the dispersoid particles are particles having an average particle size of 200 nm to 5,000 nm, and the solid content concentration of the dispersoid particles in the dispersion is 0.1 to 50% by mass.

[0205] Furthermore, the above dispersion may be mixed with a resin emulsion described later to produce a coating composition.

[0206] The present invention also includes an embodiment in which dispersoid particles including inorganic oxide particles and zinc cyanurate particles are dispersed in the dispersion liquid, and the inorganic oxide particles are colloidal metal oxide particles excluding particles containing colloidal silica as a main component.

[0207] That is, the object of the present invention is a dispersion liquid in which dispersoid particles containing colloidal metal oxide particles and zinc cyanurate particles are dispersed in a liquid medium, and the colloidal metal oxide particles exclude particles containing colloidal silica as a main component.

[0208] The colloidal metal oxide particles described above exclude particles having colloidal silica as a main component among the colloidal inorganic oxide particles, that is, the colloidal metal oxide particles are particles containing an oxide of at least one atom selected from the group consisting of Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

[0209] The colloidal metal oxide particles contained in the present dispersion exclude particles containing colloidal silicon dioxide as a main component from the colloidal inorganic oxide particles, and the types, average particle diameters, production methods, proportions in the dispersion, etc. of the colloidal metal oxide particles are as described in the description of the inorganic oxide particles. In addition, the types, average particle diameters, production methods (devices, procedures, etc.), blending ratios in the dispersion, types of liquid media, etc. of the zinc cyanurate particles are also as described above.

[0210] In addition, the average particle size of the dispersoid particles in the present dispersion, the solid content concentration, the method for producing the dispersion, etc. are also as described above. Preferably, when measured by laser diffraction, the dispersoid particles are particles having an average particle size of 80 nm to 2,000 nm, and the solid content concentration of the dispersoid particles in the dispersion is 0.1 to 50% by mass.

[0211] Furthermore, particles mainly composed of colloidal silica that are not included in the above-mentioned colloidal metal oxide particles refer to colloidal particles composed only of silica (SiO2) and colloidal particles whose main component (e.g., 50% by mass) of the particles is silica, and these particles are excluded in this embodiment. However, silica may be contained as a component of the composite oxide particles and as a component of the coating mentioned in the modified inorganic oxide particles. In this case, the silica content may be a ratio of more than 0% by mass and less than 30% by mass relative to the composite oxide particles and the modified inorganic oxide particles.

[0212] Furthermore, the above dispersion may be mixed with a resin emulsion described later to produce a coating composition.

[0213] [Resin]

[0214] Examples of the resin used in the coating composition of the present invention include one or more of acrylic resins, acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, styrene resins, olefin resins (ethylene resins, acrylic resins), ethylene-vinyl acetate resins, ester resins, epoxy resins, phenolic resins, amide resins, vinyl alcohol resins, fluorine resins, polyurethane resins, melamine resins, phthalic acid resins, silicone resins, alkyd resins and vinyl chloride resins.

[0215] Furthermore, for example, "acrylic resin" refers to a resin having a structure derived from acrylate (and methacrylate) in the resin, and the resin may also have a structure derived from other polymerizable compounds. As an example, acrylic resins composited with polysiloxane (referred to as "acrylic (polysiloxane composite)") and acrylic resins having a structure derived from vinyl acetate (referred to as "acetic acid-acrylic resins") can be classified as acrylic resins. In addition, there are resins having structures derived from epoxy and ester (referred to as "epoxy-ester resins"), which can be classified as epoxy resins or ester resins, but are classified as epoxy resins in this specification.

[0216] For example, "acrylic-styrene resin" can be described as "styrene-acrylic resin", and even when the names of the resins before and after are replaced, they can be regarded as synonyms.

[0217] [Resin form]

[0218] Generally speaking, as the form (classification) of the resin component used in the coating, for example, a water-soluble polymer (also referred to as a water-soluble polymer, a water-soluble resin) or a water-dispersible polymer can be cited. The form of the water-dispersible polymer can be cited, for example, as a colloid dispersion or a resin emulsion, and the resin emulsion can be cited as an oil-in-water emulsion or an oil-in-water emulsion. The resin composition of the present invention can also use the above various forms, and can use the above various resins as the resin component.

[0219] Generally, water-soluble polymers have a particle size of 0.01 μm or less and a molecular weight of 10 3 ~10 4 When used in coating compositions, a high-gloss film can be obtained and it is used for applications requiring high-temperature sintering. For example, the colloidal dispersion has a particle size of 0.01 to 0.1 μm and a molecular weight of 10 4 ~10 6 When used in coating compositions, a high-gloss film can be obtained, and it is used for applications requiring high-temperature sintering and room-temperature drying. For example, the resin emulsion has a particle size of 0.05 μm or more and a molecular weight of 10 3As described above, the coating composition has high drying properties, can obtain a highly water-resistant film, and is used for applications requiring sintering and applications requiring room temperature drying.

[0220] The form of the resin can be appropriately selected according to the application of the coating composition. From the perspective of stability and handling of the coating composition, it is preferably used in the form of a resin emulsion, and more preferably in the form of an oil-in-water resin emulsion (also called an aqueous resin emulsion).

[0221] Among them, as a preferred resin emulsion, an aqueous resin emulsion can be exemplified, wherein the pH value of the resin emulsion is 7 to 10 or 3 to 6.5, the solid content (ratio of resin component) in the resin emulsion is 30% to 65% by mass, and the viscosity is in the range of about 20 mPa·s to 20,000 mPa·s.

[0222] Examples of acrylic resin emulsions include Movinyl DM772, Movinyl 6520, and Movinyl 6530 (all of which are anionic resin emulsions) manufactured by Japan Coating Resin Co., Ltd., and VONCOAT 40-418EF manufactured by DIC Co., Ltd.; and examples of acrylic (polysiloxane composite) resin emulsions that can be classified as acrylic resin emulsions include CERANATE WHW-822 manufactured by DIC Co., Ltd.; and examples of acetic acid-acrylic resin emulsions that can also be classified as acrylic resin emulsions include VONCOAT CF-2800 manufactured by DIC Co., Ltd.

[0223] Examples of the acrylic-styrene resin emulsion include trade names Movinyl DM60, Movinyl 749E, and LDM6740 (all of which are anionic resin emulsions) manufactured by Japan Coating Resin Co., Ltd. and VONCOAT CG-8680 manufactured by DIC Corporation.

[0224] Examples of the acrylic-silicone resin emulsion include LDM7523 (anionic resin emulsion) manufactured by Japan Coating Resin Co., Ltd. and VONCOAT SA-6360 manufactured by DIC Corporation.

[0225] Examples of the vinyl acetate resin emulsion include Movinyl 206 (nonionic resin emulsion) manufactured by Japan Coating Resin Co., Ltd. and POLYSOLS-65 manufactured by Showa Denko K.K.

[0226] Examples of the ethylene-vinyl acetate resin emulsion include Movinyl 109E (nonionic resin emulsion), a trade name manufactured by Japan Coating Resin Co., Ltd., and the like.

[0227] Examples of the ester resin emulsion include Elitel KA-3556 manufactured by Unitika Co., Ltd. and the like.

[0228] Examples of epoxy resin emulsions include EPICLON H-502-42W manufactured by DIC Corporation, and examples of epoxy-ester resin emulsions that can be classified as epoxy resin emulsions include WATERSOLE FD-5530 manufactured by DIC Corporation.

[0229] Examples of the olefin-based (ethylene-based) resin emulsion include PE-381 manufactured by Naruse Chemical Co., Ltd. and the like.

[0230] Examples of the fluorine-based emulsion include SIFCLEAR F-104 manufactured by E-TEC Co., Ltd. and the like.

[0231] Examples of the polyurethane resin emulsion include HYDRAN HW-171 (trade name) manufactured by DIC Corporation and NeoRez R-967 (trade name) manufactured by DSM Coating Resins.

[0232] Examples of the alkyd resin emulsion include WATERSOL S-118 manufactured by DIC Corporation.

[0233] Examples of the vinyl chloride resin emulsion include Vinyblan VE-701 manufactured by Nissin Chemical Industry Co., Ltd.

[0234] Among the above-mentioned resin emulsions, preferred emulsions include acrylic resin emulsions, acrylic-styrene resin emulsions, acrylic-silicone resin emulsions, vinyl acetate resin emulsions, epoxy resin emulsions, and polyurethane resin emulsions.

[0235] In addition, the coating composition of the present invention may further contain a slurry of inorganic oxide powder.

[0236] The inorganic oxide powder used in the slurry may include particles in powder form among the inorganic oxide particles used in the coating additive. The atomic species of the inorganic oxide particles used in the coating additive (dispersion liquid) may be the same as or different from the atomic species of the inorganic oxide powder used in the slurry, and one or more inorganic oxide powders may be used in the slurry. In addition, the medium used in the slurry may include the same medium as the liquid medium used in the coating additive.

[0237] The slurry can be prepared by mixing the inorganic oxide powder in a liquid medium using a liquid disperser described below, or by mixing using a pulverizing device similar to the device for wet dispersion of zinc cyanurate using a dispersion medium, or by using a combination of these.

[0238] In the slurry of the inorganic oxide powder, the solid content concentration may be 0.1% by mass to 50% by mass, for example, 0.1% by mass to 30% by mass or 0.1% by mass to 20% by mass.

[0239] The coating composition can be prepared as follows, so that the ratio of the solid content in the dispersion (coating additive) to the solid content in the resin (in the case of a resin emulsion, the resin component in the emulsion) and the inorganic oxide powder slurry is (solid content in the dispersion): (resin (in the case of a resin emulsion, the resin component in the emulsion)): (solid content in the slurry) is 1:0.1 to 20:0 to 1, for example, 1:0.1 to 15:0 to 1 or 1:0.1 to 10:0 to 0.5, and the ratio of the total solid content in the coating composition is 1% to 70% by mass, 1% to 50% by mass, or 1% to 30% by mass. In addition, in the case of containing an inorganic oxide powder slurry, the lower limit of the ratio of the solid content in the slurry can be 0.1 relative to the solid content (mass ratio) 1 in the dispersion (coating additive).

[0240] The coating composition of the present invention can be obtained by mixing the inorganic oxide particles and zinc cyanurate particles (coating additive), the resin (eg resin emulsion) and the slurry of the inorganic oxide powder when used using a liquid disperser.

[0241] Examples of the liquid dispersing machine used for producing the coating composition include a stirrer, a rotary shearing type stirrer, a colloid mill, a roll mill, a high-pressure jet disperser, an ultrasonic disperser, a container-driven mill, a media stirring mill or a kneader.

[0242] A mixer is the simplest dispersing device that can disperse the target material through speed fluctuations near the stirring blades and collisions with the stirring blades.

[0243] A rotary shearing mixer is a device that disperses the target material by passing it through a narrow gap between high-speed rotating blades and an outer cylinder. The target material can be dispersed by shear flow and speed fluctuations in the gap.

[0244] The colloid mill can disperse the target material through the shear flow in the narrow gap between the high-speed rotating disk and the fixed disk.

[0245] A roll mill can disperse a target object by utilizing the shearing force and compression force in the gap between two or three rotating rolls.

[0246] The high-pressure jet disperser can disperse the target object by jetting the processing liquid at high pressure and causing the processing liquid to collide with the fixed plate and the processing liquid.

[0247] Ultrasonic dispersers can disperse target materials through ultrasonic vibration.

[0248] The container-driven mill is a device that disperses a target material by the collision and friction of media (balls) inserted into a fixed container, and examples thereof include a rotary mill, a vibration mill, and a planetary mill.

[0249] The media stirring mill is a device that uses balls or beads as media to disperse a target substance by the collision force and shear force of the media, and examples thereof include an attritor attritor and a bead mill.

[0250] The coating composition obtained by mixing the above-mentioned inorganic oxide particles, the dispersion liquid of zinc cyanurate particles (coating additive) and the resin (and the slurry of inorganic oxide powder when used) can be produced, for example, in the range of pH 7 to 10. In addition, by adding ammonia water as an alkaline component at a ratio of 100ppm to 10,000ppm, the pH value can be adjusted to the range of 10 to 11. In addition, the coating composition mixed with a resin (such as a resin emulsion) with a pH value of 3 to 6.5 can be produced in the range of pH 3 to 6.5. When mixing the inorganic oxide particles and the zinc cyanurate particles (when preparing the dispersion), it is preferably adjusted to alkaline to neutral, and the coating composition can be produced and used under alkaline to acidic conditions.

[0251] [Other additives]

[0252] The coating composition of the present invention may further contain, in addition to the above-mentioned dispersion of inorganic oxide particles and zinc cyanurate particles and resin (and slurry of inorganic oxide powder when used), conventional additives used in conventional coatings (compositions) within a range that does not impair the effects of the present invention, such as catalysts for accelerating curing, pigments, leveling agents, antioxidants, ultraviolet absorbers, light stabilizers, plasticizers, surfactants, and other various additives used in the technical field.

[0253] In addition, the coating composition of the present invention, for example, when it is desired to further increase the hardness of the coating film, can add a curing agent, a thickener, a dispersant, a defoaming agent as optional components, appropriately adjust (increase) the content of inorganic oxide particles, and select the resin type of the resin emulsion from fluorine-based and epoxy-based resins (or use a mixture of these resin types), etc., and appropriately adjust its composition and compounding ingredients according to the purpose.

[0254] Furthermore, the B-type viscosity of the coating composition may be, for example, 10 mPa·s to 100 mPa·s. In addition, depending on the application and substrate of the coating composition, for example, when it is desired to increase the film thickness, a high-viscosity resin variety (for example, a resin variety as a resin emulsion) may be selected, and the viscosity may be increased by adding a thickener.

[0255] [Applicable parts]

[0256] The coating object of the coating composition of the present invention, that is, the coated surface is not particularly limited, and examples thereof include aluminum substrates, iron substrates, copper substrates, gold substrates, silver substrates, platinum substrates, mirror materials, glass substrates, silicon substrates, wood, resin films, and resin molded products.

[0257] For these substrates, the coating composition can be applied and dried, and then subjected to appropriate curing treatment (thermosetting / photocuring) to form a coating film. In the coating film of the above-mentioned coating composition, the film thickness also varies according to the viscosity of the coating composition, and can be set in the range of 0.1 μm to 100 μm, for example. The above-mentioned coating film is not particularly limited as long as it has a hardness that does not cause adverse conditions in the processing steps of the substrate, and its hardness can be appropriately set according to the type of substrate.

[0258] Examples of coating methods include spin coating, bar coating, roll coating, and dip coating. By using these methods, a spin coating film, a bar coating film, a roll coating film, or a dip coating film can be obtained.

[0259] Hereinafter, for each substrate, an example of application, a preferred resin type in the coating composition, and drying conditions after coating the substrate are exemplified, but are not limited thereto.

[0260] Aluminum substrates are used in applications such as building materials, home appliances, and interior panels.

[0261] Examples of the types of resins in the preferred coating composition for an aluminum substrate include acrylic resins (including acrylic (polysiloxane composite) resins, acetic acid-acrylic resins, etc.), acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, olefin resins (ethylene resins, etc.), ester resins, epoxy resins (including epoxy-ester resins, etc.), fluorine resins, polyurethane resins, alkyd resins, vinyl chloride resins, and the like.

[0262] In addition, the drying conditions may be 200° C. to 300° C. (heat drying).

[0263] The iron-based substrate includes not only a substrate composed only of iron (Fe), but also a substrate containing iron (Fe) and other elements (carbon (C), silicon (Si), manganese (Mn), chromium (Cr), molybdenum (Mo), phosphorus (P), sulfur (S), tungsten (W), vanadium (V), nickel (Ni), aluminum (Al), niobium (Nb), nitrogen (N), etc.).

[0264] The iron-based substrates are used in applications such as building materials, structures, home appliances, and machinery (steel plate types: stainless steel plates, mild steel plates, galvanized steel plates, electromagnetic steel plates, etc.).

[0265] Examples of the preferred resin types in the coating composition for iron-based substrates include acrylic resins (including acrylic (polysiloxane composite) resins, acetic acid-acrylic resins, etc.), acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, styrene resins, olefin resins (ethylene resins, etc.), ester resins, epoxy resins, fluorine resins, polyurethane resins, alkyd resins, and the like.

[0266] In addition, the drying conditions may be 20°C to 400°C (normal temperature drying, heating drying).

[0267] The copper-based / silver-based substrates also include substrates that have undergone metal surface treatment.

[0268] Copper-based / silver-based substrates are used in applications such as electronic materials (substrates, wirings, bonding wires), electromagnetic wave shielding materials, and electric wires.

[0269] Examples of the preferred resin types in the coating composition for copper / silver substrates include acrylic resins (including acrylic (polysiloxane composite) resins, acetic acid-acrylic resins, etc.), acrylic-styrene resins, vinyl acetate resins, styrene resins, olefin resins (ethylene resins, propylene resins, etc.), phenol resins, epoxy resins, fluorine resins, polyurethane resins, etc.

[0270] Examples of drying / curing conditions include curing by ultraviolet irradiation, curing by electron beam irradiation, and curing by thermal polymerization (40 to 230° C.).

[0271] The gold-based substrate also includes a substrate that has undergone metal surface treatment.

[0272] Gold-based substrates are used in applications such as electronic materials (ICs, LSIs, and transistor bonding wires).

[0273] Examples of the preferred resin types in the coating composition for a metal-based substrate include acrylic resins, styrene resins, olefin resins (ethylene resins, propylene resins, etc.), epoxy resins, and fluorine resins.

[0274] Examples of drying / curing conditions include curing by ultraviolet irradiation, curing by electron beam irradiation, and curing by thermal polymerization (40 to 80° C.).

[0275] The platinum-based substrates also include substrates that have undergone metal surface treatment.

[0276] Platinum-based substrates are used in applications such as sensors, electrodes, and catalysts.

[0277] Examples of the preferred resin types in the coating composition for a platinum-based substrate include fluorine-based resins and polyurethane-based resins.

[0278] In addition, the drying conditions may be 100° C. to 400° C. (heat drying).

[0279] Mirror materials are used for mirrors and other purposes.

[0280] Examples of the preferred resin types in the coating composition for mirror materials include acrylic resins, phenolic resins, alkyd resins, ester resins, epoxy resins, and polyurethane resins.

[0281] In addition, the drying condition may be 150°C to 200°C (heat drying).

[0282] Glass substrates are used in smartphones, solar cells, semiconductors, building materials, car windows, and more.

[0283] Examples of the preferred resin types in the coating composition for a glass substrate include acrylic resins, phenolic resins, fluorine resins, epoxy resins, and silicone resins.

[0284] In addition, the drying conditions may be 80°C to 400°C (heat drying).

[0285] Silicone substrates are used in solar cells, semiconductors, and other applications.

[0286] Examples of the preferred resin types in the coating composition for silicone substrates include acrylic resins, ester resins, polyurethane resins, styrene resins, amide resins, vinyl alcohol resins, and vinyl acetate resins.

[0287] Examples of drying / curing conditions include curing by ultraviolet irradiation, curing by electron beam irradiation, and curing by thermal polymerization (100 to 300° C.).

[0288] Wood is used for building materials, furniture, etc.

[0289] Examples of the preferred resin types in the coating composition for wood include acrylic resins (including acetic acid-acrylic resins, etc.), acrylic-styrene resins, vinyl acetate resins, olefin resins (ethylene resins, etc.), phenol resins, ester resins, epoxy resins, fluorine resins, polyurethane resins, silicone resins, alkyd resins, etc.

[0290] In addition, the drying conditions may be 20°C to 50°C or 20°C to 100°C (heat drying).

[0291] Examples of the resin species in the resin film / resin molded product include epoxy, melamine, polyurethane, polyimide, polyamide-imide, polyethylene, polypropylene, Teflon (registered trademark) (polytetrafluoroethylene), acrylic acid, acrylonitrile styrene (AS), acrylonitrile butadiene styrene (ABS), polyvinyl chloride, polycarbonate, polyester, PET, and cycloolefin.

[0292] Resin films and resin molded products are used in smartphones, agricultural films, electronic materials (substrates and seals), etc.

[0293] Examples of preferred resin types in coating compositions for resin films / resin molded products include acrylic resins (including acrylic (polysiloxane composite) resins, acetic acid-acrylic resins, etc.), acrylic-styrene resins, vinyl acetate resins, styrene resins, olefin resins (ethylene resins, propylene resins, etc.), phenolic resins, epoxy resins, polyurethane resins, fluorine resins, alkyd resins, and the like.

[0294] Examples of drying / curing conditions include curing by ultraviolet irradiation or electron beam irradiation, and curing by thermal polymerization (40 to 80° C.), and heating drying at 40 to 60° C. may be employed.

[0295] Furthermore, in the aforementioned coating composition comprising a dispersion in which dispersoid particles containing inorganic oxide powder and zinc cyanurate particles are dispersed in a liquid medium and a resin (e.g., a resin emulsion), and in the coating composition comprising a dispersion in which dispersoid particles containing colloidal metal oxide particles excluding particles having colloidal silica as a main component and zinc cyanurate particles are dispersed in a liquid medium and a resin (e.g., a resin emulsion), the usable resins (resin types, resin forms), the proportions of the components in the composition, the method for manufacturing the composition (apparatus, sequence, etc.), other components that can be formulated, additives, and applicable parts can be applied to the contents listed in the aforementioned coating composition.

[0296] Example

[0297] The present invention will be described in detail by the following examples, but the present invention is not limited to these examples.

[0298] The components used in the dispersion and coating composition were prepared by the following steps, and the average particle size of the inorganic oxide particles and dispersoid particles, the specific surface area, loose bulk density and zeta potential of the inorganic oxide powder, and the viscosity of the coating composition were measured.

[0299] (1) The following inorganic oxide particles were prepared.

[0300] Colloidal silica: Aqueous carbon dioxide silica sol (manufactured by Nissan Chemical Co., Ltd., trade name Snowtex ST-N-40, specific surface area as determined by the BET method: 122.5 m 2 / g, pH 9.4, solid content 40.4% by mass, and average particle size as determined by dynamic light scattering method 34.5 nm)

[0301] Silica powder: Fumed silica A (manufactured by AEROSIL Co., Ltd., Japan, trade name AEROSIL (registered trademark) 300, with a specific surface area of ​​253.2 m2 as measured by the BET method) 2 / g)

[0302] Silica powder: Fumed silica B (manufactured by AEROSIL Co., Ltd., Japan, trade name AEROSIL (registered trademark) 50, with a specific surface area of ​​45.8 m2 as determined by the BET method) 2 / g)

[0303] Silica powder: Silica powder C (manufactured by Fuji Silica Co., Ltd., trade name Sylysia 380, with a specific surface area of ​​229.7 m2 as measured by the BET method) 2 / g)

[0304] Titanium dioxide powder: Titanium dioxide powder (Sakai Chemical Industry Co., Ltd., trade name R-25, specific surface area by BET method 44.2 m 2 / g and surface treated with Al2O3)

[0305] Aqueous alumina sol (colloidal alumina) (manufactured by Nissan Chemical Co., Ltd., trade name AS-200, pH 4.6, solid content 10.3% by mass, average particle size 244 nm as determined by dynamic light scattering)

[0306] Aqueous zirconium dioxide sol (colloidal zirconium dioxide) (manufactured by Nissan Chemical Co., Ltd., trade name NanoUse (registered trademark) ZR-30BS, pH 9.8, solid content 30.5% by mass, average particle size 60.2 nm as determined by dynamic light scattering)

[0307] ·Aqueous titanium dioxide sol (colloidal titanium dioxide)

[0308] 126.2g of pure water was added to a 1-liter container, and 17.8g of metastannic acid (containing 15g in terms of SnO2), 284g of tetraisopropoxide titanium (containing 80g in terms of TiO2), 84g of oxalic acid dihydrate (70g in terms of oxalic acid), and 438g of a 35% by mass aqueous solution of tetraethylammonium hydroxide were added under stirring. In the obtained mixed solution, the molar ratio of oxalic acid / titanium atom was 0.78, and the molar ratio of tetraethylammonium hydroxide / titanium atom was 1.04. 950g of the mixed solution was maintained at 80°C for 2 hours, and then the pressure was reduced to 580Torr and maintained for 2 hours to prepare a titanium mixed solution. The pH value of the modulated titanium mixed solution was 4.7, the conductivity was 27.2mS / cm, and the TiO2 concentration was 8.4% by mass.

[0309] 950 g of the titanium mixed solution and 950 g of pure water were placed in a 3-liter glass-lined autoclave container and hydrothermally treated at 140° C. for 5 hours. After cooling to room temperature, the solution after hydrothermally treated was taken out to be a light milky white aqueous titanium dioxide sol. The pH value of the aqueous titanium dioxide sol obtained was 3.9, the conductivity was 19.7 mS / cm, the TiO2 concentration was 4.2% by mass, the tetraethylammonium hydroxide was 4.0% by mass, the oxalic acid was 1.8% by mass, and the particle size by dynamic light scattering was 16 nm.

[0310] ·Aqueous tin oxide sol (tin oxide sol)

[0311] Dissolve 37.5 kg of oxalic acid ((COOH)2·2H2O) in 220 kg of pure water and place it in a 0.5 m 3 In a GL container, heat to 70°C while stirring, then add 150 kg of 35% hydrogen peroxide and 75 kg of metal tin powder (AT-SnNO200N, manufactured by Yamaishi Metal Co., Ltd., containing 99.7% SnO2). The addition of hydrogen peroxide and metal tin is performed alternately 15 times. First add 10 kg of 35% hydrogen peroxide, then add 5 kg of metal tin. Wait for the reaction to end (10 to 15 minutes) and repeat this operation.

[0312] The time required for the addition was 2.5 hours. After the addition was completed, the reaction was terminated by heating for 1 hour while maintaining the liquid temperature at 90°C. The ratio of hydrogen peroxide to metallic tin was a H2O2 / Sn molar ratio of 2.44. The specific gravity of the obtained aqueous tin oxide was 1.22, the pH value was 1.49, the SnO2 was 26.1% by mass, the oxalic acid concentration from the feed was 7.6% by mass, and the (COOH)2 / SnO2 molar ratio was 0.47.

[0313] The particle size of the tin oxide colloid is 10 to 15 nm under an electron microscope, and it is a spherical particle with good dispersibility. 230 kg of tin dioxide sol was dispersed in 1100 kg of water, and then 3.0 kg of isopropylamine was added thereto. Then, the liquid was passed through a column filled with a hydroxyl type anion exchange resin to make it alkaline. The sol was then heated and aged at 90°C and passed through a column filled with an anion exchange resin again, thereby obtaining 1431 kg of alkaline aqueous tin oxide sol. The obtained sol was a stable and very transparent tin dioxide sol with a specific gravity of 1.034, a pH of 11.33, a SnO2 content of 4.04 mass%, an isopropylamine content of 0.21 mass%, and a dynamic light scattering particle size of 20 nm.

[0314] (2) Prepare zinc cyanurate particles (CA particles).

[0315] Zinc cyanurate particles A: manufactured by Nissan Chemical Co., Ltd., trade name Starfine (registered trademark) (average particle size measured by laser diffraction method: 1.7 μm, primary particle major axis: 400 to 600 nm, minor axis: 50 to 70 nm, major axis / minor axis ratio: 5.7 to 12, specific surface area: 15 m 2 / g and the molar ratio of (zinc oxide) / (cyanuric acid) is 2.5)

[0316] Zinc cyanurate particles B: manufactured by Nissan Chemical Co., Ltd., trade name Starfine (registered trademark) (average particle size measured by laser diffraction method: 55 μm, primary particle major axis: 1,000 to 2,000 nm, minor axis: 100 to 300 nm, major axis / minor axis ratio: 3.3 to 20, specific surface area: 10 m 2 / g and the molar ratio of (zinc oxide) / (cyanuric acid) is 2.5)

[0317] (3) Prepare an oil-in-water resin emulsion.

[0318] Acrylic resin emulsion: manufactured by DIC Corporation, trade name VONCOAT40-418EF, resin concentration 55.5 mass %, pH 7.3

[0319] Acrylic-styrene resin emulsion A: manufactured by DIC Corporation, trade name VONCOAT CG-8680, resin concentration 50.0 mass % and pH 8.4

[0320] Acrylic-styrene resin emulsion B: manufactured by Japan Coating Resin Co., Ltd., trade name Movinyl DM-60, resin concentration 48.3 mass % and pH 7.5

[0321] Acrylic (polysiloxane composite) resin emulsion: manufactured by DIC Corporation, trade name CERANATE WHW-822, resin concentration 35.0 mass % and pH 8.1

[0322] ·Acrylic-silicone resin emulsion: manufactured by Japan Coating Resin Co., Ltd., trade name LDM7523, resin concentration 47.2 mass % and pH 8.0

[0323] Polyurethane resin emulsion A: manufactured by DIC Corporation, trade name Hydran HM-171, resin concentration 35.8% by mass, pH 8.2

[0324] Polyurethane resin emulsion B: manufactured by DSM Coating Resins, trade name NeoRez R-967, resin concentration 39.7 mass % and pH 8.0

[0325] Epoxy resin emulsion: manufactured by DIC Corporation, trade name EPICLON H-502-42W, resin concentration 39.3 mass % and pH 9.1

[0326] · Epoxy-ester resin emulsion: manufactured by DIC Corporation, trade name Watersol EFD-5530, resin concentration 37.0 mass % and pH 9.1

[0327] Alkyd resin emulsion: manufactured by DIC Corporation, trade name Watersol S-118, resin concentration 60.0 mass % and pH 9.2

[0328] Acetic acid-acrylic acid resin emulsion: manufactured by DIC Corporation, trade name VONCOAT CF-2800, resin concentration 50.0 mass % and pH 4.7

[0329] Vinyl acetate resin emulsion: manufactured by Showa Denko K.K., trade name Polysol S-65, resin concentration 50.5 mass % and pH 5.0

[0330] Vinyl chloride resin emulsion: manufactured by Nissin Chemical Industry Co., Ltd., trade name Vinyblan VE-701, resin concentration 30.9 mass % and pH 7.7

[0331] Olefin-based (ethylene-based) resin emulsion: manufactured by Naruse Chemical Co., Ltd., trade name PE-381, resin concentration 50.0 mass %, pH 8.0

[0332] Fluorine resin emulsion: manufactured by E-TEC Co., Ltd., trade name SIFCLEAR F-104, resin concentration 46.8 mass %, pH 7.8

[0333] · Ester resin emulsion: manufactured by Unitika Co., Ltd., trade name Elitel KA-3556, resin concentration 29.2 mass %, pH 8.0

[0334] (4) Prepare inorganic oxide powder slurry.

[0335] (4-1) Preparation of baked silica A slurry

[0336] 50 g of fumed silica A and 450 g of pure water were placed in a 500 ml polypropylene container, and a mixed slurry (SiO2 concentration 10 mass %) was prepared while stirring with a stirrer equipped with turbine blades. Next, 150 g of the slurry A and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet-milled for 30 hours to obtain fumed silica A slurry.

[0337] (4-2) Preparation of titanium dioxide powder slurry

[0338] 50 g of titanium dioxide powder and 450 g of pure water were placed in a 500 ml polypropylene container, and a mixed slurry (TiO2 concentration 10 mass %) was prepared under stirring with a stirrer equipped with turbine blades. Next, 150 g of the slurry and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill with a rotation speed set to 165 rpm, and wet pulverized for 30 hours to obtain titanium dioxide powder slurry.

[0339] (4-3) Preparation of baked silica B slurry

[0340] 50 g of fumed silica B and 450 g of pure water were placed in a 500 ml polypropylene container, and a mixed slurry (SiO2 concentration 10 mass %) was prepared while stirring with a stirrer equipped with turbine blades. Next, 150 g of the slurry and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet-milled for 30 hours to obtain fumed silica B slurry.

[0341] (4-4) Preparation of Silica Powder C Slurry

[0342] 50 g of silica powder C and 450 g of pure water were placed in a 500 ml polypropylene container, and a mixed slurry (SiO2 concentration 10 mass %) was prepared while stirring with a stirrer equipped with turbine blades. Next, 150 g of the slurry and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet pulverized for 30 hours to obtain silica powder C slurry.

[0343] (5) The average particle size of the inorganic oxide particles is measured by the following procedure.

[0344] (5-1) The average particle size of the colloidal inorganic oxide particles was measured by dynamic light scattering.

[0345] After diluting the dispersion of the colloidal inorganic oxide particles with pure water, the parameters of each inorganic oxide were measured using a dynamic light scattering measuring device: Zetasizer manufactured by Malvern Instruments Ltd.

[0346] (5-2) The average particle size of inorganic oxide powder (silicon dioxide powder, titanium dioxide powder) was measured by laser diffraction.

[0347] After dispersing the inorganic oxide powder in pure water to form a dispersion, the measurement was performed using a SALD-7500nano manufactured by Shimadzu Corporation. Here, as the substitute value of the refractive index, [1.45-0.00i] was used in the case of silicon dioxide powder, and [2.55-0.00i] was used in the case of titanium dioxide powder.

[0348] (6) The specific surface area and the loose bulk density of the inorganic oxide powder (silicon dioxide powder, titanium dioxide powder) among the inorganic oxide particles were measured.

[0349] (6-1) Specific surface area

[0350] An appropriate amount of inorganic oxide powder was placed in a quartz measuring cell, dried at 300° C. for 1 hour, and the specific surface area was measured by the BET method using Monosorb manufactured by Yuasa Ionics Co., Ltd.

[0351] (6-2) Loose bulk density

[0352] The bulk density was measured using Powder Tester PT-X manufactured by Hosokawa Micron Co., Ltd. The inorganic oxide powder was placed in the sieve of Powder Tester PT-X and the powder was dropped through a slide while vibrating. The density was measured at 100 cm. 3 Density in container.

[0353] (6-3) Zeta potential measurement

[0354] 1 g of inorganic oxide powder was added to 100 g of pure water and dispersed with a magnetic stirrer to obtain inorganic oxide powder slurry. An appropriate amount of the slurry was added to a measuring unit and the zeta potential was measured by electrophoretic light scattering method using ELSZ-2000 manufactured by Otsuka Electronics Co., Ltd.

[0355] Zeta potential was measured using an automatic titrator (ELSZ-PT manufactured by Otsuka Electronics Co., Ltd.), using 0.1 mol / L hydrochloric acid (manufactured by Kanto Chemical Co., Ltd.) and 0.1 mol / L sodium hydroxide (manufactured by Kanto Chemical Co., Ltd.) as titration reagents, adjusting the pH value of the inorganic oxide powder slurry to a range of 2 to 10, and measuring the Zeta potential at each pH value. The measurement results are shown in Table 1.

[0356] (7) The average particle size of the dispersed particles was determined by laser diffraction.

[0357] The dispersion containing the inorganic oxide particles and the zinc cyanurate particles was diluted with pure water and then measured using a product name SALD-7500nano manufactured by Shimadzu Corporation. Here, [1.70-0.2i] was used as a substitute value for the refractive index.

[0358] (8) The B-type viscosity of the coating composition was measured according to the following method.

[0359] The coating composition was poured into a 100 mL resin container, and the viscosity was measured using a B-type viscometer (BII-type viscometer manufactured by Toki Sangyo Co., Ltd.) using a No. 2 rotor.

[0360] [Example 1]

[0361] 99 g of aqueous silica sol and 261 g of pure water were placed in a 500 ml polypropylene container, and 40 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a mixed slurry (SiO2 concentration 10.0 mass%, zinc cyanurate concentration 10.0 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 1, which was used as a coating additive 1. Furthermore, after the coating additive 1 was left to stand at room temperature for 12 hours, no sedimentation layer was visually confirmed, and it was confirmed that a good dispersion state was maintained.

[0362] The solid content (silicon dioxide + zinc cyanurate) concentration of the obtained coating additive 1 was 20% by mass, and the average particle size measured by laser diffraction method was 135 nm.

[0363] 42.7 g of pure water, 0.5 g of 28% NH 3 , 29.5 g of the coating additive and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 1.

[0364] The obtained coating composition 1 had a solid content concentration of 35.5% by mass, a pH value of 9.1, and a B-type viscosity of 21 mPa·s.

[0365] [Example 2]

[0366] 16 g of fumed silica A and 344 g of pure water were placed in a 500 ml polypropylene container, and 40 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a mixed slurry (SiO2 concentration 4.0 mass%, zinc cyanurate acid concentration 10.0 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill with a rotation speed set to 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 2, which was used as a coating additive 2. Furthermore, after the coating additive 2 was left to stand at room temperature for 12 hours, no sedimentation layer was visually confirmed, and it was confirmed that a good dispersion state was maintained.

[0367] The obtained coating additive 2 had a solid content (silicon dioxide + zinc cyanurate) concentration of 14% by mass, a pH value of 6.3, and an average particle size of dispersoid particles measured by laser diffraction method of 306 nm.

[0368] 24.9 g of pure water, 0.5 g of 28% NH3, 29.5 g of the coating additive 2, 17.7 g of 10% by mass calcined silica slurry wet-milled for 30 hours using a ball mill, and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 2 hours using a stirrer equipped with turbine blades to obtain a coating composition 2.

[0369] The obtained coating composition 2 had a solid content concentration of 35.5% by mass, a pH value of 8.9, and a B-type viscosity of 56 mPa·s.

[0370] [Example 3]

[0371] 16 g of titanium dioxide powder and 344 g of pure water were placed in a 500 ml polypropylene container, and 40 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a mixed slurry (TiO2 concentration 4.0 mass%, zinc cyanurate concentration 10.0 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 3, which was used as a coating additive 3. Furthermore, after the coating additive 3 was left to stand at room temperature for 12 hours, no sedimentation layer was visually confirmed, and it was confirmed that a good dispersion state was maintained.

[0372] The obtained coating additive 3 had a solid content (titanium dioxide + zinc cyanurate) concentration of 14% by mass, a pH value of 6.2, and an average particle size of dispersoid particles measured by laser diffraction method of 1,456 nm.

[0373] 24.9 g of pure water, 0.5 g of 28% NH3, 29.5 g of the coating additive 3, 17.7 g of 10% titanium dioxide powder slurry wet-milled for 30 hours using a ball mill, and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 2 hours using a stirrer equipped with turbine blades to obtain a coating composition 3.

[0374] The obtained coating composition 3 had a solid content concentration of 35.5% by mass, a pH value of 9.3, and a B-type viscosity of 71 mPa·s.

[0375] [Comparative Example 1]

[0376] 336 g of pure water was placed in a 500 ml polypropylene container, and 64 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a zinc cyanurate particle A slurry (zinc cyanurate concentration: 16.0 mass %).

[0377] 53.8 g of pure water, 0.5 g of 28% NH 3, 18.4 g of zinc cyanurate particle A slurry (solid content 16% by mass) and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 2 hours using a stirrer equipped with turbine blades to obtain comparative coating composition 1.

[0378] The obtained comparative coating composition 1 had a solid content concentration of 33.8% by mass, a pH value of 9.6, and a B-type viscosity of 27 mPa·s.

[0379] [Comparative Example 2]

[0380] 336 g of pure water was placed in a 500 ml polypropylene container, and 64 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a slurry of zinc cyanurate particles A (the concentration of zinc cyanurate was 16.0 mass %). Next, 150 g of the slurry of zinc cyanurate particles A and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet-milled for 48 hours to obtain a comparative dispersion 2 (zinc cyanurate dispersion).

[0381] The average particle size of the obtained comparative dispersion 2 measured by laser diffraction method was 1,592 nm.

[0382] 53.8 g of pure water, 0.5 g of 28% NH3, 18.4 g of the above-mentioned zinc cyanurate dispersion (solid content 16% by mass) and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 2 hours using a stirrer equipped with turbine blades to obtain comparative coating composition 2.

[0383] The obtained comparative coating composition 2 had a solid content concentration of 33.8% by mass, a pH value of 9.5, and a B-type viscosity of 25 mPa·s.

[0384] [Reference Example 1]

[0385] 16 g of fumed silica A and 344 g of pure water were placed in a 500 ml polypropylene container, and 40 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a mixed slurry (SiO2 concentration 4.0 mass %, zinc cyanurate concentration 10.0 mass %).

[0386] The pH value of the obtained mixed slurry was 6.3, and the average particle size measured by laser diffraction method was 11,245 nm.

[0387] 41.5 g of pure water, 0.5 g of 28% NH3, 29.5 g of the mixed slurry, 1.8 g of fumed silica A and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 2 hours using a stirrer equipped with turbine blades to obtain reference coating composition 1.

[0388] The obtained reference coating composition 1 had a solid content concentration of 35.5% by mass, a pH value of 8.6, and a B-type viscosity of 450 mPa·s.

[0389] [Reference Example 2]

[0390] 16 g of fumed silica A and 344 g of pure water were placed in a 500 ml polypropylene container, and 40 g of zinc cyanurate particles A were added and mixed while stirring with a stirrer equipped with turbine blades to obtain a mixed slurry (reference dispersion) (SiO2 concentration 4.0 mass%, zinc cyanurate concentration 10.0 mass%).

[0391] The solid content (silicon dioxide + zinc cyanurate) concentration of the obtained mixed slurry (reference dispersion 2) was 14% by mass, and the average particle size of the dispersoid particles measured by laser diffraction method was 11,245 nm.

[0392] 24.9 g of pure water, 0.5 g of 28% NH3, 29.5 g of the above mixed slurry (reference dispersion 2) and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain reference coating composition 2.

[0393] The obtained reference coating composition 2 had a solid content concentration of 38.5% by mass, a pH value of 8.6, and a B-type viscosity of 450 mPa·s.

[0394] [Example 4]

[0395] Coating composition 1 prepared in the same manner as in Example 1 was diluted with pure water so as to have a solid content concentration of 22% by mass, thereby obtaining coating composition 4 having a solid content concentration of 22.0% by mass and a pH of 9.1.

[0396] [Reference Example 3]

[0397] Reference coating composition 1 prepared in the same manner as Reference Example 1 was diluted with pure water so as to have a solid content concentration of 22% by mass, thereby obtaining reference coating composition 3 having a solid content of 22.0% by mass and a pH of 8.6.

[0398] [Example 5]

[0399] 16 g of fumed silica B and 344 g of pure water were placed in a 500 ml polypropylene container, and 40 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a mixed slurry (SiO2 concentration 4.0 mass%, zinc cyanurate concentration 10.0 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill with a rotation speed set to 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 5. Furthermore, after the dispersion 5 was left to stand at room temperature for 12 hours, no sedimentation layer was visually confirmed, and it was confirmed that a good dispersion state was maintained.

[0400] The solid content (silicon dioxide + zinc cyanurate) concentration of the obtained dispersion 5 was 14 mass %, the pH value was 6.3, and the average particle size of the dispersoid particles measured by laser diffraction method was 1,707 nm. The obtained dispersion 5 was used as a coating additive 5.

[0401] 24.9 g of pure water, 0.5 g of 28% NH3, 29.5 g of the coating additive 5, 17.7 g of 10% by mass baked silica B slurry wet-milled for 30 hours using a ball mill, and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) emulsion were added to a 250 ml polypropylene container and stirred for 2 hours using a stirrer equipped with turbine blades to obtain a coating composition 5.

[0402] The obtained coating composition 5 had a solid content concentration of 35.5% by mass, a pH value of 9.3, and a B-type viscosity of 17 mPa·s.

[0403] [Example 6]

[0404] 16 g of silica powder C and 344 g of pure water were placed in a 500 ml polypropylene container, and 40 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to obtain a mixed slurry (SiO2 concentration 4.0 mass%, zinc cyanurate concentration 10.0 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill with a rotation speed set to 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 6. Furthermore, after the dispersion 6 was left to stand at room temperature for 12 hours, no sedimentation layer was visually confirmed, and it was confirmed that a good dispersion state was maintained.

[0405] The solid content (silicon dioxide + zinc cyanurate) concentration of the obtained dispersion 6 was 14% by mass, the pH value was 6.3, and the average particle size of the dispersoid particles measured by laser diffraction method was 1,204 nm. The obtained dispersion 6 was used as a coating additive 6.

[0406] 24.9 g of pure water, 0.5 g of 28% NH3, 29.5 g of the coating additive 6, 17.7 g of 10% silica powder C slurry wet-milled for 30 hours using a ball mill, and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 2 hours using a stirrer equipped with turbine blades to obtain a coating composition 6.

[0407] The obtained coating composition 6 had a solid content concentration of 35.5% by mass, a pH value of 9.0, and a B-type viscosity of 45 mPa·s.

[0408] [Example 7]

[0409] 112.5 g of aqueous alumina sol and 101.3 g of pure water were placed in a 500 ml polypropylene container, and 11.3 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a mixed slurry (Al2O3 concentration 5.1 mass %, zinc cyanurate concentration 5 mass %). Next, 150 g of the mixed slurry and 180 g of glass beads with a diameter of 0.5-0.7 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet pulverized for 30 hours to obtain dispersion 7. Furthermore, after dispersion 7 was left to stand at room temperature for 12 hours, no sedimentation layer was observed by visual observation, and it was confirmed that a good dispersion state was maintained.

[0410] The solid content (alumina + zinc cyanurate) concentration of the obtained dispersion 7 was 10.1% by mass, and the average particle size of the dispersoid particles measured by laser diffraction method was 112 nm. The obtained dispersion 7 was used as a coating additive 7.

[0411] 13.1 g of pure water, 0.5 g of 28% NH3, 59.1 g of the above-mentioned coating additive 7 and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 7.

[0412] The obtained coating composition 7 had a solid content concentration of 35.5% by mass, a pH value of 6.2, and a B-type viscosity of 100 mPa·s.

[0413] [Example 8]

[0414] 150 g of aqueous zirconium dioxide sol and 53.5 g of pure water were placed in a 500 ml polypropylene container, and 22.5 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a mixed slurry (ZrO2 concentration 20.2 mass%, zinc cyanurate concentration 10 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads with a diameter of 0.5-0.7 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 8. Furthermore, after the dispersion 8 was left to stand at room temperature for 12 hours, no sedimentation layer was visually confirmed, and it was confirmed that a good dispersion state was maintained.

[0415] The solid content (zirconium dioxide + zinc cyanurate) concentration of the obtained dispersion 8 was 30.2% by mass, and the average particle size of the dispersoid particles measured by laser diffraction method was 53 nm. The obtained dispersion 8 was used as a coating additive 8.

[0416] 42.7 g of pure water, 0.5 g of 28% NH 3 , 29.5 g of the coating additive 8 and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 8 .

[0417] The obtained coating composition 8 had a solid content concentration of 37.3% by mass, a pH value of 9.1, and a B-type viscosity of 20 mPa·s.

[0418] [Example 9]

[0419] 200 g of aqueous titanium dioxide sol and 2.5 g of pure water were placed in a 500 ml polypropylene container, and 22.5 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a mixed slurry (TiO2 concentration 3.7 mass%, zinc cyanurate concentration 10 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads with a diameter of 0.5-0.7 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 9. Furthermore, after the dispersion 9 was left to stand at room temperature for 12 hours, no sedimentation layer was visually confirmed, and it was confirmed that a good dispersion state was maintained.

[0420] The solid content (titanium dioxide + zinc cyanurate) concentration of the obtained dispersion 9 was 13.7% by mass, and the average particle size of the dispersoid particles measured by laser diffraction method was 151 nm. The obtained dispersion 9 was used as a coating additive 9.

[0421] 30.5 g of pure water, 0.5 g of 28% NH3, 29.5 g of the above-mentioned coating additive 9 and 111.8 g of acrylic-styrene resin emulsion B (trade name Movinyl DM-60) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 9.

[0422] The obtained coating composition 9 had a solid content concentration of 34.1% by mass, a pH value of 9.8, and a B-type viscosity of 22.8 mPa·s.

[0423] [Example 10]

[0424] 201.5 g of aqueous tin oxide sol and 1.0 g of pure water were placed in a 500 ml polypropylene container, and 22.5 g of zinc cyanurate particles A were added while stirring with a stirrer equipped with turbine blades to prepare a mixed slurry (SnO2 concentration 3.6 mass%, zinc cyanurate concentration 10 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads with a diameter of 0.5-0.7 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 10. Furthermore, after the dispersion 10 was left to stand at room temperature for 12 hours, no sedimentation layer was observed visually, and it was confirmed that a good dispersion state was maintained.

[0425] The solid content (tin oxide + zinc cyanurate) concentration of the obtained dispersion 10 was 13.6% by mass, and the average particle size of the dispersoid particles measured by laser diffraction method was 91 nm. The obtained dispersion 10 was used as a coating additive 10.

[0426] 30.5 g of pure water, 0.5 g of 28% NH3, 29.5 g of the above-mentioned coating additive 10 and 111.8 g of acrylic-styrene resin emulsion B (trade name Movinyl DM-60) were added to a 250 ml polypropylene container and stirred for 1 hour with a stirrer equipped with turbine blades to obtain coating composition 10.

[0427] The obtained coating composition 10 had a solid content concentration of 34.1% by mass, a pH value of 9.8, and a B-type viscosity of 21 mPa·s.

[0428] [Comparative Example 4]

[0429] 336 g of pure water was placed in a 500 ml polypropylene container, and 64 g of zinc cyanurate particles A were added thereto while stirring with a stirrer equipped with turbine blades to prepare a zinc cyanurate slurry (zinc cyanurate concentration: 16.0 mass %).

[0430] 42.7 g of pure water, 0.5 g of 28% NH3, 19.4 g of aqueous zirconium dioxide sol, 18.5 g of zinc cyanurate slurry (solid content 16% by mass) and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 2 hours using a stirrer equipped with turbine blades to obtain comparative coating composition 4.

[0431] The obtained comparative coating composition 4 had a solid content concentration of 35.5% by mass, a pH value of 9.4, and a B-type viscosity of 13 mPa·s.

[0432] [Example 11]

[0433] 99 g of aqueous silica sol and 261 g of pure water were placed in a 500 ml polypropylene container, and while stirring with a stirrer equipped with turbine blades, 32 g of zinc cyanurate particles A and 8 g of cyanuric acid powder (manufactured by Nissan Chemical Co., Ltd.) were added to change the (zinc oxide) / (cyanuric acid) conversion molar ratio of zinc cyanurate particles A to 1.5, thereby preparing a mixed slurry (SiO2 concentration 10 mass%, zinc cyanurate concentration 10 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads having a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 11, which was used as a coating additive 11. Furthermore, after the coating additive 11 was left to stand at room temperature for 12 hours, no sedimentation layer was observed by visual inspection, and it was confirmed that a good dispersion state was maintained.

[0434] The solid content (silicon dioxide + zinc cyanurate) concentration of the obtained coating additive 11 was 20% by mass, and the average particle size measured by laser diffraction method was 78 nm.

[0435] 42.7 g of pure water, 0.5 g of 28% NH 3 , 29.5 g of the coating additive 11 and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 11 .

[0436] The obtained coating composition 11 had a solid content concentration of 35.5% by mass, a pH value of 9.0, and a B-type viscosity of 20 mPa·s.

[0437] [Example 12]

[0438] 99 g of aqueous silica sol and 261 g of pure water were placed in a 500 ml polypropylene container, and while stirring with a stirrer equipped with turbine blades, 26.8 g of zinc cyanurate particles A and 13.2 g of zinc oxide (two types of zinc oxides manufactured by Sakai Chemical Co., Ltd.) were added to change the (zinc oxide) / (cyanuric acid) conversion molar ratio of zinc cyanurate particles A to 4.5, thereby preparing a mixed slurry (SiO2 concentration 10 mass%, zinc cyanurate concentration 10 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads having a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 12, which was used as a coating additive 12. Furthermore, after the coating additive 12 was left to stand at room temperature for 12 hours, no sedimentation layer was observed visually, and it was confirmed that a good dispersion state was maintained.

[0439] The solid content (silicon dioxide + zinc cyanurate) concentration of the obtained coating additive 12 was 20% by mass, and the average particle size measured by laser diffraction method was 157 nm.

[0440] 42.7 g of pure water, 0.5 g of 28% NH 3 , 29.5 g of the coating additive 12 and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 12 .

[0441] The obtained coating composition 12 had a solid content concentration of 33.8% by mass, a pH value of 9.1, and a B-type viscosity of 21 mPa·s.

[0442] [Example 13]

[0443] 99 g of aqueous silica sol and 261 g of pure water were placed in a 500 ml polypropylene container, and 40 g of zinc cyanurate particles B were added while stirring with a stirrer equipped with turbine blades to prepare a mixed slurry (SiO2 concentration 10.0 mass%, zinc cyanurate concentration 10.0 mass%). Next, 150 g of the mixed slurry and 180 g of glass beads with a diameter of 0.7-1.0 mm were placed in a 250 ml polypropylene container, and the container was placed on a rotating table of a ball mill set at a rotation speed of 165 rpm, and wet pulverized for 30 hours to obtain a dispersion 13, which was used as a coating additive 13. Furthermore, after the coating additive 13 was left to stand at room temperature for 12 hours, no sedimentation layer was observed by visual observation, and it was confirmed that a good dispersion state was maintained.

[0444] The solid content (silicon dioxide + zinc cyanurate) concentration of the obtained coating additive 13 was 20% by mass, and the average particle size measured by laser diffraction method was 134 nm.

[0445] 42.7 g of pure water, 0.5 g of 28% NH 3 , 29.5 g of the coating additive 1 and 99.6 g of acrylic resin emulsion (trade name VONCOAT 40-418EF) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 1 .

[0446] The obtained coating composition 13 had a solid content concentration of 33.8% by mass, a pH value of 9.1, and a B-type viscosity of 19 mPa·s.

[0447] [Comparative Example 3]

[0448] 85.4 g of pure water and 114.6 g of an acrylic resin emulsion (trade name 40-418EF) were added to a 250 ml polypropylene container, and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a comparative coating composition 3.

[0449] The obtained comparative coating composition 3 had a solid content concentration of 31.8% by mass, a pH value of 9.6, and a B-type viscosity of 17 ma·s.

[0450] [Example 14]

[0451] 32.2 g of pure water, 29.3 g of the coating additive 1 and 110.6 g of acrylic-styrene resin emulsion A (trade name VONCOAT CG-8680) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 14.

[0452] The obtained coating composition 14 had a solid content concentration of 35.5% by mass, a pH value of 7.4, and a B-type viscosity of 50 mPa·s.

[0453] [Example 15]

[0454] 28.4 g of pure water, 29.3 g of the coating additive 1 and 114.5 g of acrylic-styrene resin emulsion B (trade name Movinyl DM-60) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 15.

[0455] The obtained coating composition 15 had a solid content concentration of 35.5% by mass, a pH value of 7.9, and a B-type viscosity of 25 mPa·s.

[0456] [Example 16]

[0457] 29.3 g of the coating additive 1 and 158 g of an acrylic (polysiloxane composite) resin emulsion (trade name: Ceranate WHW-822) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with a stirrer to obtain a coating composition 16.

[0458] The obtained coating composition 16 had a solid content concentration of 32.7% by mass, a pH value of 7.9, and a B-type viscosity of 31 mPa·s.

[0459] [Example 17]

[0460] 25.8 g of pure water, 29.3 g of the coating additive 1 and 117.2 g of an acrylic-silicone resin emulsion (trade name: Movinyl LDM7523) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a coating composition 17.

[0461] The obtained coating composition 17 had a solid content concentration of 35.5% by mass, a pH value of 7.7, and a B-type viscosity of 20 mPa·s.

[0462] [Example 18]

[0463] 29.3 g of the coating additive 1 and 154.5 g of polyurethane resin emulsion A (trade name: HYDRAN HW-171) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a coating composition 18.

[0464] The obtained coating composition 18 had a solid content concentration of 33.3% by mass, a pH value of 8.4, and a B-type viscosity of 16 mPa·s.

[0465] [Example 19]

[0466] 3.7 g of pure water, 29.3 g of the coating additive 1 and 139.3 g of polyurethane resin emulsion B (trade name NeoRez R-967) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 19.

[0467] The obtained coating composition 19 had a solid content concentration of 35.5% by mass, a pH value of 8.4, and a B-type viscosity of 19 mPa·s.

[0468] [Example 20]

[0469] 2.3 g of pure water, 29.3 g of the coating additive 1 and 140.7 g of epoxy resin emulsion (trade name: EPICLONH-502-42W) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a coating composition 20.

[0470] The obtained coating composition 20 had a solid content concentration of 35.5% by mass, a pH value of 9.2, and a B-type viscosity of 197 mPa·s.

[0471] [Example 21]

[0472] 29.3 g of the coating additive 1 and 149.5 g of an epoxy-ester resin emulsion (trade name: WATERSOL EFD-5530) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a coating composition 21.

[0473] The obtained coating composition 21 had a solid content concentration of 34.2% by mass, a pH value of 8.8, and a B-type viscosity of 32 mPa·s.

[0474] [Example 22]

[0475] 50.7 g of pure water, 29.3 g of the coating additive 1 and 92.2 g of an alkyd resin emulsion (trade name WATERSOLS-118) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a coating composition 22.

[0476] The obtained coating composition 22 had a solid content concentration of 35.5% by mass, a pH value of 8.8, and a B-type viscosity of 678 mPa·s.

[0477] [Example 23]

[0478] 32.2 g of pure water, 29.3 g of the coating additive 1 and 110.6 g of acetic acid-acrylic resin emulsion (trade name VONCOAT CF-2800) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain coating composition 23.

[0479] The obtained coating composition 23 had a solid content concentration of 35.5% by mass, a pH value of 5.6, and a B-type viscosity of 65 mPa·s.

[0480] [Example 24]

[0481] 33.4 g of pure water, 29.3 g of the coating additive 1 and 109.5 g of a vinyl acetate resin emulsion (trade name POLYSOL S-65) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a coating composition 24.

[0482] The obtained coating composition 24 had a solid content concentration of 35.5% by mass, a pH value of 7.2, and a B-type viscosity of 14 mPa·s.

[0483] [Example 25]

[0484] 26.5 g of pure water, 21.3 g of the coating additive 1 and 130.0 g of a vinyl chloride resin emulsion (trade name: Vinyblan VE-701) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a coating composition 25.

[0485] The obtained coating composition 25 had a solid content concentration of 25.0% by mass, a pH value of 7.8, and a B-type viscosity of 8.0 mPa·s.

[0486] [Example 26]

[0487] 32.3 g of pure water, 29.3 g of the coating additive 1 and 110.6 g of an olefin resin emulsion (trade name PE-381) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a coating composition 26.

[0488] The obtained coating composition 26 had a solid content concentration of 35.5% by mass, a pH value of 7.8, and a B-type viscosity of 58 mPa·s.

[0489] [Example 27]

[0490] 24.7 g of pure water, 29.3 g of the coating additive 1 and 118.2 g of a fluorine-based resin emulsion (trade name SIFCLEAR F-104) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a coating composition 27.

[0491] The obtained coating composition 27 had a solid content concentration of 35.5% by mass, a pH value of 8.2, and a B-type viscosity of 6.0 mPa·s.

[0492] [Example 28]

[0493] 17.8 g of pure water, 20.1 g of the coating additive 1 and 130.0 g of an ester resin emulsion (trade name: Elitel KA-3556) were added to a 250 ml polypropylene container and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a coating composition 28.

[0494] The obtained coating composition 28 had a solid content concentration of 25.0% by mass, a pH value of 8.3, and a B-type viscosity of 29 mPa·s.

[0495] [Comparative Example 5]

[0496] 128.3 g of pure water and 71.7 g of an acrylic resin emulsion (trade name 40-418EF) were added to a 250 ml polypropylene container, and stirred for 1 hour using a stirrer equipped with turbine blades to obtain a comparative coating composition 5.

[0497] The obtained comparative coating composition 5 had a solid content concentration of 19.9% ​​by mass, a pH value of 9.0, and a B-type viscosity of 11 mPa·s.

[0498] [Comparative Example 6]

[0499] Comparative coating composition 1 prepared in the same manner as in Comparative Example 1 was diluted with pure water so that the solid content concentration became 22% by mass, thereby obtaining comparative coating composition 6 having a solid content concentration of 22.0% by mass.

[0500] The obtained comparative coating composition 6 had a solid content concentration of 22.0% by mass, a pH value of 8.9, and a B-type viscosity of 15 mPa·s.

[0501] [Comparative Example 7]

[0502] Comparative coating composition 1 prepared in the same manner as in Comparative Example 2 was diluted with pure water so that the solid content concentration became 22% by mass, thereby obtaining comparative coating composition 7 having a solid content concentration of 22.0% by mass.

[0503] The obtained comparative coating composition 7 had a solid content concentration of 22.0% by mass, a pH value of 8.9, and a B-type viscosity of 18 mPa·s.

[0504] [Example 29]

[0505] Coating composition 15 prepared in the same manner as in Example 15 was diluted with pure water to a solid content concentration of 22 mass %, thereby obtaining coating composition 29 having a solid content concentration of 22.0 mass %, a pH of 7.9, and a B-type viscosity of 25 mPa·s.

[0506] [Example 30]

[0507] Coating composition 16 prepared in the same manner as in Example 16 was diluted with pure water so as to have a solid content concentration of 22 mass %, thereby obtaining coating composition 30 having a solid content concentration of 22.0 mass %, a pH of 7.9, and a B-type viscosity of 31 mPa·s.

[0508] [Example 31]

[0509] Coating composition 18 prepared in the same manner as in Example 18 was diluted with pure water to a solid content concentration of 22 mass %, thereby obtaining coating composition 31 having a solid content concentration of 22.0 mass %, a pH of 8.4, and a B-type viscosity of 16 mPa·s.

[0510] [Example 32]

[0511] Coating composition 20 prepared in the same manner as in Example 20 was diluted with pure water to a solid content concentration of 22 mass %, thereby obtaining coating composition 32 having a solid content concentration of 22.0 mass %, a pH of 9.2, and a B-type viscosity of 197 mPa·s.

[0512] [Example 33]

[0513] Coating composition 22 prepared in the same manner as in Example 22 was diluted with pure water to a solid content concentration of 22 mass %, thereby obtaining coating composition 33 having a solid content concentration of 22.0 mass %, a pH of 8.8, and a B-type viscosity of 678 mPa·s.

[0514] [Example 34]

[0515] Coating composition 23 prepared in the same manner as in Example 23 was diluted with pure water to a solid content concentration of 22 mass %, thereby obtaining coating composition 34 having a solid content concentration of 22.0 mass %, a pH of 6.3, and a B-type viscosity of 30 mPa·s.

[0516] [Example 35]

[0517] Coating composition 24 prepared in the same manner as in Example 24 was diluted with pure water to a solid content concentration of 22 mass %, thereby obtaining coating composition 35 having a solid content concentration of 22.0 mass %, a pH of 7.4, and a B-type viscosity of 11 mPa·s.

[0518] [Example 36]

[0519] Coating composition 26 prepared in the same manner as in Example 26 was diluted with pure water so as to have a solid content concentration of 22 mass %, thereby obtaining coating composition 36 having a solid content concentration of 22.0 mass %, a pH of 7.5, and a B-type viscosity of 46 mPa·s.

[0520] [Example 37]

[0521] Coating composition 27 prepared in the same manner as in Example 27 was diluted with pure water to a solid content concentration of 22 mass %, thereby obtaining coating composition 37 having a solid content concentration of 22.0 mass %, a pH of 7.9, and a B-type viscosity of 5 mPa·s.

[0522] Using Examples 1 to 3, coating compositions 1 to 3 of Examples 5 to 28, coating compositions 5 to 28, comparative coating compositions 1 to 4 of Comparative Examples 1 to 4, and reference coating compositions 1 to 2 of Reference Examples 1 to 2, coating on aluminum plates and evaluation of coating films were carried out in the order described below.

[0523] In addition, using Example 4, coating composition 4 of Examples 29 to 37, coating composition 29 to coating composition 37, comparative coating compositions 5 to 7 of Comparative Examples 5 to 7, and reference coating composition 3 of Reference Example 3, coating on a PET film and evaluation of the coating film were carried out in the order described below.

[0524] [Examples 38 to 46]

[0525] Using the coating compositions 1, 15, 16, 18, 20, 23, 24, 26, and 27 of Examples 1, 15, 16, 18, 20, 23, 24, 26, and 27, coating on a Cu plate and evaluation of the coating film were carried out in the following order.

[0526] [Comparative Examples 8 to 10]

[0527] Using the comparative coating compositions 3, 1, and 2 of Comparative Examples 3, 1, and 2, coating on a Cu plate and evaluation of the coating film were carried out in the following procedures.

[0528] [Examples 47 to 53]

[0529] Using the coating compositions 1, 16, 18, 20, 22, 26, and 27 of Examples 1, 16, 18, 20, 22, 26, and 27, coating on SUS plates and evaluation of the coating films were carried out in the following procedures.

[0530] [Comparative Examples 11 to 13]

[0531] Using the comparative coating compositions 3, 1, and 2 of Comparative Examples 3, 1, and 2, coating on a SUS plate and evaluation of the coating film were carried out in the following procedure.

[0532] [Examples 54 to 63]

[0533] Using the coating compositions 1, 15, 16, 18, 20, 22 to 24, 26, and 27 of Examples 1, 15, 16, 18, 20, 22 to 24, 26, and 27, coating on mild steel plates and evaluation of the coating films were carried out in the following procedures.

[0534] [Comparative Examples 14 and 15]

[0535] Using the comparative coating compositions 1 and 2 of Comparative Examples 1 and 2, coating on a mild steel plate and evaluation of the coating film were carried out in the following procedures.

[0536] [Examples 64 to 73]

[0537] Using the coating compositions 1, 15, 16, 18, 20, 22 to 24, 26, and 27 of Examples 1, 15, 16, 18, 20, 22 to 24, 26, and 27, coating on galvanized steel sheets and evaluation of the coating films were carried out in the order described below.

[0538] [Comparative Examples 16 and 17]

[0539] Using the comparative coating compositions 1 and 2 of Comparative Examples 1 and 2, coating on a galvanized steel sheet and evaluation of the coating film were carried out in the following procedures.

[0540] [Examples 74 to 82]

[0541] Using the coating compositions 1, 15, 18, 20, 22 to 24, 26, and 27 of Examples 1, 15, 18, 20, 22 to 24, 26, and 27, coating on cedar boards and evaluation of the coating films were carried out in the following procedures.

[0542] [Comparative Examples 18 to 20]

[0543] Using the comparative coating compositions 3, 1, and 2 of Comparative Examples 3, 1, and 2, coating on a cedar board and evaluation of the coating film were carried out in the following procedures.

[0544] (9) A coated aluminum plate was prepared as follows.

[0545] An aluminum plate (manufactured by Koh Co., Ltd., JIS type A1050P) having a plate thickness of 0.5 mm and a size of 70 mm in width x 150 mm in length was used.

[0546] (Coating method)

[0547] The coating compositions 1 to 3, coating compositions 5 to 28, comparative coating compositions 1 to 4, and reference coating compositions 1 to 2 were applied to the surface of the aluminum plate by bar coating at a speed of 2 m / min, and fired in an electric furnace set at 230° C. for 30 seconds to obtain an aluminum plate with a coating film. The specific method of bar coating is as follows.

[0548] Bar coating: Each coating composition was dropped onto an aluminum plate and coated using an RDS.24 bar coater to a wet coating film thickness of 61 μm.

[0549] (10) A film substrate (PET) to be coated was prepared as follows.

[0550] A PET film (manufactured by Toyobo Co., Ltd., trade name: Cosmo Shine A4100) having a thickness of 100 μm and a size of 297 mm in width×420 mm in length and having been subjected to an easy-joining treatment was used.

[0551] (Coating method)

[0552] Coating composition 4, coating compositions 29 to 37, comparative coating compositions 5 to 7, and reference coating composition 3 were applied to the easy-to-bond surface of the PET film by bar coating at a speed of 2 m / min, and dried on a hot plate set at 60° C. for 5 minutes to obtain a PET film with a coating. The specific method of bar coating is as follows.

[0553] Bar coating: Each coating composition was dropped onto a PET film and coated using a No. 2 bar coater to a wet coating film thickness of 4.6 μm.

[0554] (11) The coated Cu plate was prepared as follows.

[0555] A Cu plate (manufactured by Koh Co., Ltd., JIS type C1220P) having a plate thickness of 0.5 mm and a size of 100 mm in width×365 mm in length was used.

[0556] (Coating method)

[0557] Coating compositions 1, 15, 16, 18, 20, 23, 24, 26, 27, and comparative coating compositions 1 to 3 were applied to the surface of a Cu plate at a speed of 2 m / min by bar coating, and fired in an electric furnace set at 230° C. for 30 seconds to obtain a Cu substrate with a coating film. The specific method of bar coating is as follows.

[0558] Bar coating: Each coating composition was dropped onto a copper plate and coated using an RDS.24 bar coater to a wet coating film thickness of 61 μm.

[0559] (12) A coated SUS plate was prepared as follows.

[0560] A SUS plate (manufactured by Koh Co., Ltd., JIS type SUS430) having a plate thickness of 0.5 mm and a size of 100 mm in width×300 mm in length was used.

[0561] (Coating method)

[0562] Coating compositions 1, 16, 18, 20, 22, 26, 27, and comparative coating compositions 1 to 3 were applied to the surface of the SUS plate at a speed of 2 m / min by bar coating, and fired in an electric furnace set at 230° C. for 30 seconds to obtain SUS plates with coating films. The specific method of bar coating is as follows.

[0563] Bar coating: Each coating composition was dropped onto a SUS plate and coated using an RDS.24 bar coater to a wet coating film thickness of 61 μm.

[0564] (13) A coated mild steel plate was prepared as follows.

[0565] A mild steel plate (manufactured by TP Giken Co., Ltd., JIS type SPCC bright steel plate) having a plate thickness of 0.8 mm and a size of 70 mm in width×150 mm in length was used.

[0566] (Coating method)

[0567] Coating compositions 1, 15, 16, 18, 20, 22 to 24, 26, 27 and comparative coating compositions 1 and 2 were applied to the surface of a mild steel plate by bar coating at a speed of 2 m / min, and fired in an electric furnace set at 230° C. for 30 seconds to obtain a mild steel plate with a coating film. The specific method of bar coating is as follows.

[0568] Bar coating: Each coating composition was dropped onto a mild steel plate and coated using an RDS.24 bar coater to a wet coating film thickness of 61 μm.

[0569] (14) The galvanized steel sheet to be coated was prepared as follows.

[0570] A galvanized steel sheet (manufactured by Standard TestPiece Co., Ltd., JIS type SS400, hot-dip galvanizing (without chemical conversion treatment)) having a sheet thickness of 6 mm and a size of 70 mm in width x 150 mm in length was used.

[0571] (Coating method)

[0572] The coating compositions 1, 15, 16, 18, 20, 22 to 24, 26, 27 and the comparative coating compositions 1 and 2 were applied to the surface of the galvanized steel sheet by bar coating at a speed of 2 m / min, and fired in an electric furnace set at 230° C. for 30 seconds to obtain a galvanized steel sheet with a coating film. The specific method of bar coating is as follows.

[0573] Bar coating: Each coating composition was dropped onto a galvanized steel plate, and coated using an RDS.24 bar coater to a wet coating film thickness of 61 μm.

[0574] (15) The wood to be coated was prepared as follows.

[0575] A cedar board having a thickness of 5 mm and a size of 100 mm in width x 150 mm in length (manufactured by Standard Test Piece Co., Ltd., red and white board, planed on four sides) was used.

[0576] (Painting method)

[0577] The coating compositions 1, 15, 18, 20, 22, 23, 24, 26, 27 and comparative coating compositions 1 to 3 were applied by brush coating to a coating amount of 30 g / m after drying. 2The first layer was then formed by coating the surface of the fir board substrate in a manner of 100°C and drying at 80°C for 3 minutes. Next, the same coating composition as that used for the first layer was applied in an amount of 70 g / m2 after drying. 2 The coating was applied to the surface of the first layer in a manner of coating, and dried at 80° C. for 10 minutes, thereby obtaining a coated fir board with a two-layer structure.

[0578] (16) Appearance test of coated aluminum plate, coated Cu plate, coated SUS plate, coated mild steel plate, coated galvanized steel plate, coated fir board and coated PET film

[0579] For each coated aluminum plate, coated Cu plate, coated SUS plate, coated mild steel plate, coated galvanized steel plate, coated cedar board and coated PET film, the area of ​​the portion where the coating was formed relative to the area of ​​the aluminum plate, Cu plate, SUS plate, mild steel plate, galvanized steel plate, cedar board or PET film was visually observed and evaluated based on the following evaluation criteria.

[0580] <Evaluation Criteria>

[0581] Good: 90% or more of the coating film formation area was observed.

[0582] Slightly defective: 50% to 89% of the coating film formation area was observed.

[0583] Defective: 10% to 49% of the coating film formation area was observed.

[0584] (17) Pencil hardness test

[0585] With reference to JIS K5600, pencil hardness of each of the coated aluminum plate, coated Cu plate, coated SUS plate, coated mild steel plate, coated galvanized steel plate and coated PET film was measured by the following method.

[0586] Using a hand-pressed pencil scratch hardness tester manufactured by Yasuda Seiki Seisakusho, Ltd., a pencil lead manufactured by Hi-uni Co., Ltd. manufactured by Mitsubishi Pencil Co., Ltd. was pressed against the coating surface and moved to measure the pencil hardness when the coating peeled off.

[0587] Furthermore, it is desired that the pencil hardness is 3B or more when an aluminum substrate is used, the pencil hardness is 5B or more when a copper substrate is used, the pencil hardness is 3B or more when an iron substrate (SUS, mild steel plate, galvanized steel plate) is used, and the pencil hardness is 6B or more when a PET film is used.

[0588] <Judgment Criteria>

[0589] [Soft] 6B, 5B, 3B, 2B, B, HB, F, H, 2H, 3H, 4H, 5H [Hard]

[0590] (18) Fit test using the cross-cut method

[0591] With reference to JIS K5600, for each coated aluminum plate, coated Cu plate, coated SUS plate, coated mild steel plate, coated galvanized steel plate, coated cedar board and coated PET film, the adhesion (closeness) of the coating obtained by the cross-cut method to the substrate (aluminum plate, PET film, CU plate, SUS plate, mild steel plate, galvanized steel plate, cedar board) was evaluated according to the following method.

[0592] 100 grid patterns were cut at 1 mm intervals on the coating surface, and the tape was placed in contact with the grid portion for 20 mm in a manner that covered the grid portion. Then, the tape was grasped at the end and the tape was peeled off in 0.5 to 1.0 seconds so that the tape was pulled off reliably. The presence or absence of peeling of the coating and the number of peelings (the number of grids) were visually confirmed and evaluated according to the following criteria.

[0593] <Judgment Criteria>

[0594] A: The number of unpeeled squares is more than 90

[0595] B: The number of unpeeled checkerboard squares is more than 60 and less than 90

[0596] C: The number of unpeeled checkerboard squares is more than 40 and less than 60

[0597] D: The number of unpeeled checkerboard squares is less than 40

[0598] (19) HAZE assay

[0599] The HAZE measurement of the coated PET film was performed using NDH-5000 manufactured by Nippon Denshoku Industries Co., Ltd. by a measurement method in accordance with JIS K7105.

[0600] The obtained results are summarized in Tables 1 to 7.

[0601]

[0602]

[0603]

[0604]

[0605]

[0606]

[0607]

[0608]

[0609]

[0610]

[0611]

[0612]

[0613]

[0614]

[0615]

[0616]

[0617]

[0618]

[0619] As shown in Table 1 [Table 1-1 to Table 1-4], according to the present invention, a coating film can be formed on the entire aluminum plate substrate, has a hardness of about 3B or more, and has excellent adhesion to the substrate.

[0620] In detail, as shown in [Table 1-1] and [Table 1-2] (Examples 1 to 3, Examples 5 to 10), even when using various silica powders, colloidal alumina, colloidal zirconium dioxide, colloidal titanium dioxide, and tin oxide sol, a coating film can be formed that is formed on the entire aluminum plate substrate and has excellent adhesion to the substrate.

[0621] In addition, as shown in [Table 1-3] (Examples 11 to 13), even when the particle size of the zinc cyanurate particles and the (zinc oxide) / (zinc cyanurate) conversion molar ratio of the zinc cyanurate particles are changed, a coating film can be formed on the entire aluminum plate substrate, with a hardness of 2B or more and excellent adhesion to the substrate.

[0622] In addition, as shown in [Table 1-4] and [Table 1-5] (Examples 14 to 21, 22 to 28), according to the present invention, when using various resin emulsions, a coating film can be formed on the entire aluminum plate substrate and has both hardness and close adhesion to the substrate.

[0623] On the other hand, in the case where no inorganic oxide powder was used, in either Comparative Example 1 in which zinc cyanurate slurry and resin emulsion were mixed, or in Comparative Example 2 in which zinc cyanurate slurry was wet-ground to form a dispersion and then mixed with a resin emulsion, the coating appearance (poor) and adhesion (D) were much worse than those of the examples. In addition, in the case of Comparative Example 3 in which only the resin emulsion was used, although the coating appearance was good, the adhesion was evaluated as D. In addition, in the case where colloidal metal oxide particles and zinc cyanurate were not formed into a dispersion but simply mixed (Comparative Example 4), although the coating appearance was good, the adhesion (C) was poor.

[0624] Furthermore, in Reference Examples 1 and 2, in which the average particle size of the dispersed substance measured by laser diffraction method in the dispersion containing inorganic oxide powder and zinc cyanurate particles was greater than 10,000 nm, the coating appearance (poor) and adhesion (D) were much worse than those of the examples.

[0625] In addition, as shown in Table 2 [Table 2-1 to Table 2-3] (Example 4, Example 29 to Example 33, Example 34 to Example 37), according to the present invention, when various resin emulsions are used, a coating film having a hardness of 2B or more and excellent adhesion to the substrate can be formed on the entire PET substrate. In addition, according to the present invention, a significant increase in the HAZE value is suppressed, so the adhesion to the substrate can be improved without significantly impairing the transparency of the PET substrate.

[0626] On the other hand, in the case of not using inorganic oxide particles, in either the case of Comparative Example 5 in which zinc cyanurate slurry and resin emulsion were mixed, or in the case of Comparative Example 6 in which zinc cyanurate slurry was wet-ground to form a dispersion and then mixed with a resin emulsion, the coating appearance (poor) and the adhesion (D) were much worse than those of the examples. In addition, in the case of Comparative Example 4 in which only the resin emulsion was used, although the coating appearance was good, the adhesion was evaluated as D.

[0627] In addition, in Reference Example 3, in which the average particle size of the dispersoid measured by laser diffraction method in the dispersion containing inorganic oxide powder and zinc cyanurate particles was more than 10,000 nm, the coating appearance (poor) and adhesion (C) were much worse than those of the examples.

[0628] As shown in Table 3 [Table 3-1 to Table 3-2] (Examples 38 to 40, Examples 41 to 46), according to the present invention, a coating film can be formed on the entire Cu plate substrate, has a hardness of 5B or more, and has excellent adhesion to the substrate.

[0629] On the other hand, in Comparative Example 8 in which inorganic oxide particles were not used and only the resin emulsion was used, although the coating appearance was good, the adhesion was evaluated as D. In Comparative Example 9 in which the zinc cyanurate slurry and the resin emulsion were mixed, and in Comparative Example 10 in which the zinc cyanurate slurry was wet-ground to form a dispersion and then mixed with the resin emulsion, the coating appearance (poor) and the adhesion (D (Comparative Example 9), B (Comparative Example 10)) were much worse than those of the examples.

[0630] As shown in Table 4 [Table 4-1 to Table 4-2] (Examples 47 to 49, Examples 50 to 53), according to the present invention, a coating film can be formed on the entire SUS plate substrate, has a hardness of 3B or more, and has excellent adhesion to the substrate.

[0631] On the other hand, in Comparative Example 11 in which inorganic oxide particles were not used and only the resin emulsion was used, although the coating appearance was good, the adhesion was evaluated as D. In Comparative Example 12 in which the zinc cyanurate slurry and the resin emulsion were mixed, and in Comparative Example 13 in which the zinc cyanurate slurry was wet-ground to form a dispersion and the dispersion was mixed with the resin emulsion, the coating appearance (poor) and the adhesion (D) were both much worse than those of the examples.

[0632] As shown in Table 5 [Table 5-1 to Table 5-2] (Examples 54 to 56, Examples 57 to 63), according to the present invention, a coating film can be formed on the entire mild steel plate substrate, has a hardness of 3B or more, and has excellent adhesion to the substrate.

[0633] On the other hand, in Comparative Example 14 in which the zinc cyanurate slurry and the resin emulsion were mixed without using inorganic oxide particles, and Comparative Example 15 in which the zinc cyanurate slurry was wet-ground to form a dispersion and the dispersion was mixed with the resin emulsion, the coating film appearance (poor) and adhesion (D) were much worse than those of the examples.

[0634] As shown in Table 6 [Table 6-1 to Table 6-2] (Examples 64 to 67, Examples 68 to 73), according to the present invention, a coating film can be formed on the entire galvanized steel sheet substrate, with a hardness of HB or above and excellent adhesion to the substrate.

[0635] On the other hand, in Comparative Example 16 in which the zinc cyanurate slurry was mixed with the resin emulsion and in Comparative Example 17 in which the zinc cyanurate slurry was wet-ground to form a dispersion and then mixed with the resin emulsion without using inorganic oxide particles, the coating film appearance (poor) and adhesion (C (Comparative Example 16), B (Comparative Example 17)) were much worse than those of the examples.

[0636] As shown in Table 7 [Table 7-1 to Table 7-2] (Examples 74 to 76, Examples 77 to 82), according to the present invention, a coating film can be formed which is formed on the entire wood and has excellent adhesion to the substrate.

[0637] On the other hand, in the case where inorganic oxide particles were not used, in Comparative Example 18, which was only a resin emulsion, and in Comparative Example 20, in which zinc cyanurate slurry was wet-ground to form a dispersion and the dispersion was mixed with the resin emulsion, although the coating appearance was good, the adhesion (B) was poor. In Comparative Example 19, in which zinc cyanurate slurry was mixed with a resin emulsion, the coating appearance (poor) and the adhesion (C) were much worse than those of the examples.

[0638] Furthermore, Figure 1 This is a graph showing an approximate curve obtained based on the measured value of the Zeta potential (mV) of the inorganic oxide particles relative to the pH value (pH 2 to 10 (horizontal axis)) of the water-dispersed slurry in which the inorganic oxide powder is silica powder (fumed silica A, fumed silica B, silica powder C) or titanium dioxide powder (titanium dioxide powder).

[0639] like Figure 1 As shown, the inorganic oxide particles used in this embodiment: silica powder (fumed silica A, fumed silica B, silica powder C) and titanium dioxide powder (titanium dioxide powder) do not have an isoelectric point at pH 5 to pH 12, and have a Zeta potential of -5mV to -50mV in this pH range.

[0640] As described above, it was confirmed that coating additive 1 (fumed silica A), coating additive 2 (fumed silica B), coating additive 3 (silicon dioxide powder C) and coating additive 4 (titanium dioxide powder) using these powders were all able to obtain a dispersion liquid with excellent dispersibility by using inorganic oxide particles in which no sedimentation layer was visually observed after standing at room temperature for 12 hours, and a good dispersion state was maintained, and that the inorganic oxide particles had no isoelectric point at pH 5 to pH 12 and a Zeta potential of -5 mV to -50 mV in this pH range.

Claims

1. A coating composition comprising a coating additive, a resin, and a slurry of an inorganic oxide powder, wherein the coating additive comprises a dispersion obtained by dispersoid particles dispersed in a liquid medium, wherein the dispersoid particles comprise inorganic oxide particles and zinc cyanurate particles, and the solid content concentration of the slurry is 0.1 to 50% by mass. The dispersoid particles in the dispersion have an average particle size of 80 nm to 5,000 nm when measured by laser diffraction, and a solid content concentration of the dispersoid particles in the dispersion is 0.1 to 50% by mass.

2. The coating composition according to claim 1, wherein the coating surface is at least one selected from the group consisting of an aluminum substrate, an iron substrate, a copper substrate, a gold substrate, a silver substrate, a platinum substrate, a mirror material, a glass substrate, a silicon substrate, wood and a resin molded product. The coating composition according to claim 2 , wherein the resin molded product is a resin film.

4. The coating composition according to claim 1 or 2, wherein the resin is in the form of a resin emulsion, which is in the form of an oil-in-water emulsion or a water-in-oil emulsion, and is a resin emulsion containing one or more resin components selected from the group consisting of acrylic resins, acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, olefin resins, ethylene-vinyl acetate resins, ester resins, epoxy resins, phenolic resins, amide resins, vinyl alcohol resins, fluorine resins, polyurethane resins, melamine resins, phthalic acid resins, silicone resins, alkyd resins and vinyl chloride resins. The coating composition according to claim 4 , wherein the olefin-based resin is a styrene-based resin.

6. The coating composition according to claim 1 or 2, wherein the resin is in the form of a water-soluble polymer or a colloidal dispersion, and is a water-soluble resin or a colloidal dispersion containing one or more resin components selected from acrylic resins, acrylic-styrene resins, acrylic-silicone resins, vinyl acetate resins, olefin resins, ethylene-vinyl acetate resins, ester resins, epoxy resins, phenolic resins, amide resins, vinyl alcohol resins, fluorine resins, polyurethane resins, melamine resins, phthalic acid resins, silicone resins, alkyd resins and vinyl chloride resins. 7 . The coating composition according to claim 6 , wherein the olefin-based resin is a styrene-based resin.

8. The coating composition according to claim 1 or 2, wherein the inorganic oxide particles are oxides of at least one atom selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

9. The coating composition according to claim 8, wherein the inorganic oxide particles are composite oxides or mixed oxides of two or more atoms selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

10. The coating composition according to claim 1 or 2, wherein the inorganic oxide particles are colloidal oxides of at least one atom selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

11. The coating composition according to claim 10, wherein the inorganic oxide particles are colloidal composite oxides or colloidal mixed oxides of two or more atoms selected from Si, Al, Ti, Zr, Fe, Cu, Zn, Li, Na, K, Mg, Ca, Cs, Sr, Ba, B, Ga, Y, Nb, Mo, In, Sn, Sb, Ta, W, Ge, Pb, P, As, Rb, Bi and Ce.

12. The coating composition according to claim 1 or 2, wherein the zinc cyanurate particles have a primary particle major axis of 400 nm to 3,000 nm and a primary particle minor axis of 10 nm to 300 nm, and a ratio of the major axis to the minor axis of 1.3 to 300 when measured using a transmission electron microscope. 13 . The coating composition according to claim 1 , wherein the dispersoid particles in the dispersion liquid include inorganic oxide particles and zinc cyanurate particles at a mass ratio of 1:0.01 to 100, and the solid content concentration of the dispersoid particles in the dispersion liquid is 0.1 to 50% by mass.

14. The coating composition according to claim 1 or 2, wherein the liquid medium is water or an organic solvent.

15. The coating composition according to claim 1 or 2, wherein the ratio of the solid content in the dispersion to the resin is 1:0.1-20 in terms of the mass ratio of the solid content in the dispersion to the resin, and the ratio of the total solid content in the coating composition is 1-70 mass %.

16. The coating composition according to claim 1 or 2, wherein the ratio of the solid content in the dispersion, the resin and the solid content of the slurry of the inorganic oxide powder is 1:0.1~20:0.1~1 in terms of the mass ratio of the solid content in the dispersion, the resin and the solid content of the slurry, and the proportion of the total solid content in the coating composition is 1~70 mass %.

17. A coating film, which is a coating film of the coating composition according to any one of claims 1 to 16, formed on at least one substrate selected from the group consisting of an aluminum substrate, an iron-based substrate, a copper-based substrate, a gold-based substrate, a silver-based substrate, a platinum-based substrate, a mirror material, a glass substrate, a silicon substrate, a wood and a resin molded product. The coating film according to claim 17 , wherein the resin molded product is a resin film. 19 . A coating film, which is a coating film of the coating composition according to claim 1 , and has a film thickness of 0.1 μm to 100 μm. 20 . The coating film according to claim 19 , which is a spin coating film, a bar coating film, a roller coating film or a dip coating film.

21. A method for producing a coating composition, which is the method for producing a coating composition according to any one of claims 1 to 16, comprising the step of mixing a dispersion and a resin using a liquid disperser, wherein the dispersion is obtained by dispersoid particles containing inorganic oxide particles and zinc cyanurate particles being dispersed in a liquid medium.

22. A method for producing a coating composition, which is the method for producing a coating composition according to any one of claims 1 to 16, comprising the step of mixing a dispersion, the resin and a slurry of the inorganic oxide powder using a liquid disperser, wherein the dispersion is obtained by dispersoid particles containing inorganic oxide particles and zinc cyanurate particles dispersed in a liquid medium.

23. The method for producing a coating composition according to claim 21 or 22, wherein the liquid disperser is a stirrer, a colloid mill, a roll mill, a high-pressure jet disperser, an ultrasonic disperser, a container-driven mill, a media stirring mill or a kneader.

24. The method for producing a coating composition according to claim 21 or 22, further comprising a step of mixing the inorganic oxide particles and the zinc cyanurate particles or a mixed liquid of the slurry thereof using a pulverizing device before the step of mixing using the liquid disperser. 25 . The method for producing a coating composition according to claim 24 , wherein the pulverizing device is a ball mill, a bead mill or a sand mill.

26. The method for producing a coating composition according to claim 21 or 22, further comprising, before the mixing step using the liquid disperser, a step of mixing the pre-crushed inorganic oxide powder with the mixed liquid of zinc cyanurate particles or a slurry thereof using a pulverizing device.

Citation Information

Patent Citations

  • Corrosion preventive coating material on metal surface

    JP1979123145A

  • Manufacture of lead cyanurate and zinc cyanurate

    JP1984031779A

  • Basic zinc cyanurate fine particles, and method for producing same

    WO2011162353A1

  • Production method for basic zinc cyanurate powder and production method for rust-preventive pigment composition

    WO2016006585A1

  • Aerogel hybrid microsphere grafted silicon composite coating and preparation method thereof

    CN106700811A