A kind of organic silicon coating adhesive and its preparation method and application

By combining modified methoxy silicone resin with trimethoxy-terminated polydimethylsiloxane, the shortcomings of existing silicone coatings in chemical corrosion resistance and environmental protection are solved, and solvent-free organics are prepared Silicon-coated glue has excellent mechanical properties and environmental protection, and is suitable for many high-demand fields.

CN116285859BActive Publication Date: 2024-11-19GUANGZHOU JOINTAS CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211646407.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-19
Publication Date
2024-11-19
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

The existing silicone coating glue has shortcomings in its chemical corrosion resistance and environmental protection, and requires solvent dilution, resulting in low strength, poor airtightness and inconsistent environmental protection policies.

Method used

Modified methoxy silicone resin combined with trimethoxy end-ended polydimethylsiloxane, combined with a specific content of crosslinking agent, coupling agent and catalyst, and a specific preparation method to prepare moderate viscosity and moderate hardness , solvent-free silicone coating glue with short surface drying time and high mechanical strength.

Benefits of technology

The silicone coated glue has achieved moderate viscosity, moderate hardness, short surface drying time, high mechanical strength, high temperature and humidity resistance, excellent salt spray resistance, and no solvent required, meeting environmental protection policy requirements, suitable for electronic industry and LED Plant lighting, automotive and aerospace fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004006507120000021
    Figure BDA0004006507120000021
  • Figure BDA0004006507120000022
    Figure BDA0004006507120000022
Patent Text Reader

Abstract

The present invention discloses an organosilicon coating adhesive and a preparation method and application thereof, belonging to the field of chemical technology; the organosilicon coating adhesive provided by the present invention comprises the following raw materials in parts by mass: 80-100 parts of base adhesive, 1-5 parts of methyl silicone oil, 30-80 parts of modified methoxy silicone resin, 0.01-0.5 parts of fluorescent indicator, 3-10 parts of cross-linking agent, 0.5-5 parts of coupling agent, and 2-5 parts of catalyst. The organosilicon coating adhesive provided by the present invention has the characteristics of moderate viscosity, moderate hardness, high mechanical strength, high temperature and humidity resistance, excellent salt spray resistance, and excellent insulation, and the preparation method of the organosilicon coating adhesive provided by the present invention is simple, easy to operate, and is conducive to actual production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical technology, and in particular relates to an organic silicon coating adhesive and a preparation method and application thereof. Background Art

[0002] Coating glue is also called three-proof paint, coating glue, electric anti-glue, etc. It is a dense protective material that is coated on circuit boards (PCBs) and electronic components and cured. It can resist the influence of vibration, high temperature and humidity, salt spray, atmospheric corrosion and other environmental factors on circuit boards and electronic components during use, and has functions such as moisture-proof, dust-proof, insulation, and corona protection. Coating glue can be divided into silicone, acrylic resin, polyurethane, modified resin, etc. according to the material. Because silicone coating glue has excellent properties such as high and low temperature resistance, electrical insulation, ozone resistance, radiation resistance, and hydrophobicity, it is widely used in the electronics industry, LED plant lighting, automotive industry, aerospace, military industry and other fields.

[0003] The mainstream silicone coating adhesives on the market are divided into two categories: one is made of α,ω-dihydroxy polydimethylsiloxane, i.e. 107 silica gel, in combination with a crosslinking agent, a catalyst, a functional additive and a mixture, but this type of coating adhesive has low strength and poor air tightness, which can easily lead to insufficient chemical corrosion resistance; the other type is made of phenyl silicone resin as the base material, in combination with a crosslinking agent and a catalyst, but this type of coating material generally has a macromolecular structure and is too viscous, and needs to be diluted with a solvent (benzene solvent) before use, which is inconsistent with current environmental protection policies. For example, patent document 201811109028.3 discloses a methoxy-terminated methylphenyl polysiloxane resin, a silicone coating adhesive, and a preparation method and application. The invention uses diphenyldimethoxysilane, dimethyldimethoxysilane, and methyltrimethoxysilane through hydrolysis polymerization to obtain a methoxy-terminated silicone resin, and uses this as a base material and a white carbon black reinforcing filler to prepare a silicone coating adhesive. The coating adhesive prepared by this method has good strength and air tightness, but its viscosity is too high and needs to be diluted with toluene solvent before use. It has poor environmental protection and is inconsistent with current environmental protection policies. Patent document 201310677004.9 discloses a one-component silicone coating adhesive, which is obtained by stirring and mixing 80-100 parts of hydroxyl-terminated polydimethylsiloxane, 5-10 parts of diluent, 4-8 parts of MQ resin, 5-10 parts of cross-linking agent, 0.5-1.5 parts of tackifier, and 0.5-2 parts of catalyst in a stirring kettle under vacuum. The adhesive film obtained after curing has the characteristics of high and low temperature resistance, aging resistance, flexibility, insulation, moisture resistance, shock resistance, corona resistance, leakage resistance, and good resistance to cold and heat changes. It has better tear resistance and bonding strength than general neutral silicone. However, the coating adhesive needs to be diluted with a solvent, and due to formula restrictions, it has low strength and poor air tightness, which easily leads to insufficient resistance to salt spray and chemical corrosion. Patent document 201610702125.8 discloses a solvent-free silicone coating adhesive and its preparation method, the silicone coating adhesive comprises the following raw materials by weight: 70-100 parts of hydroxyl-terminated polydimethylsiloxane, 10-30 parts of film enhancer, 2-6 parts of cross-linking agent, 0.1-0.8 parts of catalyst, 0.5-1.5 parts of tackifier to form silicone coating adhesive. It has good high and low temperature resistance, insulation, bonding, moisture resistance, shock resistance and corona resistance. The coating adhesive can be solvent-free, but the curing method of the coating adhesive is deketoxime, which is easy to corrode the metal parts in the circuit board and electronic components. The protection performance is insufficient. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a solvent-free silicone coating adhesive with moderate viscosity, moderate hardness, short surface drying time, high mechanical strength, high temperature and humidity resistance, and excellent salt spray resistance, as well as a preparation method and application thereof.

[0005] To achieve the above object, the technical solution adopted by the present invention is: an organic silicone coating adhesive, the organic silicone coating adhesive comprises the following raw materials in parts by weight: 80-100 parts of base adhesive, 1-5 parts of methyl silicone oil, 30-80 parts of modified methoxy silicone resin, 0.01-0.5 parts of fluorescent indicator, 3-10 parts of cross-linking agent, 0.5-5 parts of coupling agent, and 2-5 parts of catalyst;

[0006] The base rubber is trimethoxy-terminated polydimethylsiloxane with a viscosity of 1500-20000 mPa·s. Its structure is shown in Formula I. In Formula I, n>1,

[0007]

[0008] The general structural formula of the modified methoxy silicone resin is shown in Formula II, wherein a+b+c=1, 0.4<a<0.58, 0.2<b<0.42, 0.05<c<0.4, and R is an alkyl group having 1 to 12 carbon atoms.

[0009]

[0010] The organic silicone coating adhesive provided by the present invention utilizes the modified methoxy silicone resin provided by the present invention as a reinforcing silicone resin, which can have excellent compatibility with trimethoxy-terminated polydimethylsilane, and further cooperates with other components with specific contents to achieve good interaction and achieve excellent synergistic effect, thereby making the prepared organic silicone coating adhesive have the characteristics of moderate viscosity, moderate hardness, short surface drying time, high mechanical strength, high temperature and humidity resistance, and excellent salt spray resistance.

[0011] Preferably, the viscosity of the base glue is 7000-15000 mPa·s.

[0012] Preferably, in the formula II, R is methyl.

[0013] The inventors have found that when the viscosity of the base glue is further preferably within the above range and R in Formula II is preferably methyl, the comprehensive performance of the obtained silicone coating glue is more excellent.

[0014] As a preferred embodiment of the organic silicone coating adhesive described in the present invention, the modified methoxy silicone resin includes the following raw materials in parts by weight: 100-150 parts of trifunctional silane, 0.1-1 parts of acidic catalyst, 40-60 parts of first organic solvent, 10-50 parts of small molecule hydroxyl silicone oil, 30-50 parts of second organic solvent, and 0.01-0.5 parts of alkaline catalyst.

[0015] As a preferred embodiment of the organic silicone coating adhesive of the present invention, the trifunctional silane is at least one of methyltrimethoxysilane, propyltrimethoxysilane, hexyltrimethoxysilane, cyclohexyltrimethoxysilane, nonyltrimethoxysilane, decyltrimethoxysilane, and dodecyltrimethoxysilane, the acid catalyst is at least one of hydrochloric acid, trifluoromethanesulfonic acid, and concentrated sulfuric acid, the viscosity of the small molecule hydroxy silicone oil is 10-100mPa·s, the alkaline catalyst is potassium hydroxide or sodium hydroxide, the first organic solvent is at least one of benzene, toluene, or xylene, and the second organic solvent is at least one of benzene, toluene, or xylene.

[0016] As a preferred embodiment of the organic silicone coating adhesive of the present invention, the preparation method of the modified methoxy silicone resin comprises the following steps:

[0017] S1: After the trifunctional silane and the first organic solvent are mixed, an acidic catalyst and deionized water are added dropwise at 0-30° C. for 30-60 min, wherein the molar ratio of the trifunctional silane to the deionized water is 1:(0.9-1.2);

[0018] S2: After the addition is completed, heat to reflux and react for 4-6 hours, then cool to 48-52°C and adjust the system to neutral, filter, collect the filtrate, and concentrate to obtain methoxy silicone resin intermediate A;

[0019] S3: Mix the methoxy silicone resin intermediate A, the second organic solvent, the small molecule hydroxy silicone oil and the alkaline catalyst evenly, heat to 80-110°C, react for 4-8 hours, introduce excess CO2 to neutralize the alkaline catalyst, then filter, collect and concentrate the filtrate to obtain the modified methoxy silicone resin.

[0020] As a preferred embodiment of the organic silicone coating adhesive of the present invention, the viscosity of the methyl silicone oil is 50-500 mPa·s.

[0021] The modified methoxy silicone resin prepared by using the above raw materials and preparation method can ensure good compatibility with trimethoxy-terminated polydimethylsiloxane in the subsequent preparation, thereby achieving excellent reinforcement effect, thereby making the comprehensive performance of the obtained silicone coating adhesive excellent.

[0022] As a preferred embodiment of the organic silicone coating adhesive of the present invention, at least one of (a) to (d) is

[0023] (a) the fluorescent indicator is selected from at least one of 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2-(2-hydroxy-3,5-di-tert-phenyl)-5-chlorobenzotriazole and 2,4,6-tris(2-n-butoxyphenyl)-1,3,5-triazine;

[0024] (b) the crosslinking agent is selected from at least one of methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane and acryltrimethoxysilane;

[0025] (c) the coupling agent is selected from at least one of vinyltrimethoxysilane, vinyltriethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, (3-aminopropyl)trimethoxysilane, γ-aminoethylaminopropyltrimethoxysilane and γ-aminoethylaminopropyltriethoxysilane;

[0026] (d) The catalyst is selected from titanate esters and their complexes.

[0027] Preferably, the catalyst is selected from at least one of tetra-n-butyl titanate, tetraisopropyl titanate, tetraisobutyl titanate, tetraisooctyl titanate, diisopropoxy titanium bis(ethyl acetoacetate), and diisopropoxy titanium bis(acetoacetonate).

[0028] In addition, the present invention also provides a method for preparing an organic silicon coating adhesive, the preparation method comprising the following steps:

[0029] (1) The base rubber, methyl silicone oil, modified methoxy silicone resin and fluorescent indicator are mixed uniformly, and then heated to 100-120° C. under vacuum conditions and stirred and dispersed for 30-60 minutes;

[0030] (2) Cooling to 23-28°C, adding a crosslinking agent and dispersing for 4-6 minutes at normal pressure, and then vacuuming and dispersing for another 5-10 minutes;

[0031] (3) After adding the coupling agent and the catalyst under normal pressure and dispersing at a low speed for 5-10 minutes, the mixture is dispersed at a high speed for 20-30 minutes under vacuum conditions, and then the mixture is discharged to obtain the silicone coating adhesive.

[0032] In addition, the present invention also provides an application of the organosilicon coating adhesive in the electronics industry, LED plant lighting, automobile, aerospace or military fields.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The organic silicone coating adhesive provided by the present invention uses the modified methoxy silicone resin provided by the present invention as a reinforcing silicone resin, which can have excellent compatibility with trimethoxy-terminated polydimethylsiloxane, and further cooperates with other components with specific contents to achieve good interaction and achieve excellent synergistic effect, so that the prepared organic silicone coating adhesive has the characteristics of moderate viscosity, moderate hardness, short surface drying time, high mechanical strength, high temperature and high humidity resistance, excellent salt spray resistance, and excellent insulation. Specifically, the obtained viscosity is below 760-2000mPa·s, the hardness is between 40-60A, the tensile strength is above 3.1MPa, the dielectric strength is above 17KV / mm, and the volume resistivity is above 2.8*10 14 Ω·cm or more, and after 1000h of high temperature and high humidity test and salt spray resistance test, no bubbles are generated and no shedding occurs, that is, it still has good protection performance; therefore, it can be widely used in the electronics industry, LED plant lighting, automobiles, aerospace or military fields; and the preparation method of the organic silicone coating adhesive provided by the present invention is simple, easy to operate, and is conducive to actual production. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is the infrared spectrum of the modified methoxy silicone resin 1 prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0037] The reagents, methods and equipment used in the present invention are all conventional reagents, methods and equipment in the art unless otherwise specified. Unless otherwise specified, the components used in the parallel experiments of the examples of the present invention and the comparative examples are from the same source.

[0038] Base glue 1: n is 480, viscosity is 7000mPa·s, lubricating material, RH-FW7K;

[0039] Base glue 2: n is 660, viscosity is 15000 mPa·s, Chengtian New Materials, FT-150;

[0040] Base glue 3: n is 240, viscosity is 1500mPa·s, Chengtian New Materials, FT-15;

[0041] Base glue 4: n is 720, viscosity is 20000mPa·s, Chengtian New Materials; FT-200;

[0042] Base glue 5: n is 225, viscosity is 1000mPa·s, lubricating material, RH-FW1K;

[0043] Base glue 6: n is 810, viscosity is 28000mPa·s, Chengtian New Materials, FT-300;

[0044] Methyl silicone oil 1: viscosity 100 mPa·s, Jibisheng, MSO-100;

[0045] Methyl silicone oil 2: viscosity 1000 mPa·s, Jibisheng, MSO-1000;

[0046] Small molecule hydroxy silicone oil: viscosity 70mPa·s, Dow Corning, PMX-0156;

[0047] Trifunctional silane: methyltrimethoxysilane, commercially available;

[0048] Fluorescent indicator: 2-(2-hydroxy-5-methylphenyl)benzotriazole, commercially available;

[0049] Cross-linking agent: methyltrimethoxysilane, commercially available;

[0050] Coupling agent: γ-aminoethylaminopropyltriethoxysilane, commercially available;

[0051] Catalyst: tetrabutyl titanate, commercially available.

[0052] Example 1

[0053] The embodiment of the present invention provides a modified methoxy silicone resin 1, the general structural formula of the modified methoxy silicone resin 1 is shown in Formula III, the viscosity is 106 mPa·s,

[0054]

[0055] The preparation method of the modified methoxy silicone resin 1 comprises the following steps:

[0056] S1: After mixing 130 parts of methyltrimethoxysilane and 60 parts of toluene, 1 part of hydrochloric acid (mass concentration is 36%) and 17.4 parts of deionized water are added dropwise at 15±2°C for 45 minutes, wherein the molar ratio of methyltrimethoxysilane to deionized water is 1:1.05;

[0057] S2: After the addition is completed, the temperature is raised to 65°C, refluxed and reacted for 4 hours, then the temperature is lowered to 50°C, sodium bicarbonate is added to adjust the system to neutrality, and the filtrate is collected and concentrated to obtain methoxy silicone resin intermediate A;

[0058] S3: Mix methoxy silicone resin intermediate A, 50 parts of toluene, 35 parts of small molecule hydroxy silicone oil and 0.1 parts of potassium hydroxide evenly, heat to 100°C and react for 4 hours, evaporate the methanol small molecules, then introduce excess CO2 to neutralize the potassium hydroxide, then filter, collect the filtrate and concentrate to obtain modified methoxy silicone resin 1.

[0059] The infrared spectrum of the modified methoxy silicone resin obtained is as follows: Figure 1 As shown, the infrared spectrum found 3400cm -1 The characteristic peak of silanol group disappears, which proves that the small molecule hydroxy silicone oil and methoxy silicone resin intermediate A have been block-connected to form a block-modified methoxy silicone resin compound.

[0060] Example 2

[0061] The embodiment of the present invention provides a modified methoxy silicone resin 2, the general structural formula of the modified methoxy silicone resin 2 is shown in Formula VI, the viscosity is 85 mPa·s,

[0062]

[0063] The preparation method of the modified methoxy silicone resin 2 comprises the following steps:

[0064] S1: After mixing 100 parts of methyltrimethoxysilane and 40 parts of toluene, 0.1 parts of trifluoromethanesulfonic acid and 13.88 parts of deionized water were added dropwise at 15±2°C for 30 minutes, wherein the molar ratio of methyltrimethoxysilane to deionized water was 1:1.05;

[0065] S2: After the addition is completed, the temperature is raised to 70°C, refluxed and reacted for 4 hours, then the temperature is lowered to 50°C, sodium bicarbonate is added to adjust the system to neutrality, and the filtrate is collected and concentrated to obtain methoxy silicone resin intermediate A;

[0066] S3: Mix methoxy silicone resin intermediate A, 30 parts of toluene, 50 parts of small molecular weight hydroxy silicone oil, and 0.05 parts of potassium hydroxide, and heat to 90°C for 6 hours to evaporate methanol small molecules, then introduce excess CO2 to neutralize potassium hydroxide, then filter, collect the filtrate, and concentrate to obtain modified methoxy silicone resin 2;

[0067] Example 3

[0068] The embodiment of the present invention provides a modified methoxy silicone resin 3, the general structural formula of the modified methoxy silicone resin 3 is shown in Formula V, the viscosity is 108 mPa·s,

[0069]

[0070] The preparation method of the modified methoxy silicone resin 3 comprises the following steps:

[0071] S1: After mixing 150 parts of methyltrimethoxysilane and 60 parts of toluene, 0.5 parts of concentrated sulfuric acid and 20.81 parts of deionized water were added dropwise at 15±2°C for 45 minutes, wherein the molar ratio of methyltrimethoxysilane to deionized water was 1:1.05;

[0072] S2: After the addition is completed, the temperature is raised to 60°C, refluxed and reacted for 4 hours, then the temperature is lowered to 50°C, sodium bicarbonate is added to adjust the system to neutrality, and the filtrate is collected and concentrated to obtain methoxy silicone resin intermediate A;

[0073] S3: Mix methoxy silicone resin intermediate A, 50 parts of toluene, 10 parts of small molecule hydroxy silicone oil and 0.5 parts of potassium hydroxide evenly, heat to 100°C and react for 4 hours, evaporate the methanol small molecules, then introduce excess CO2 to neutralize the potassium hydroxide, then filter, collect the filtrate and concentrate to obtain modified methoxy silicone resin 3.

[0074] Comparative Example 1

[0075] The comparative example of the present invention provides a modified methoxy silicone resin 4, the general structural formula of the modified methoxy silicone resin 4 is shown in Formula VI, the viscosity is 75 mPa·s,

[0076]

[0077] The preparation method of the modified methoxy silicone resin 4 comprises the following steps:

[0078] S1: After mixing 130 parts of methyltrimethoxysilane and 60 parts of toluene, 1 part of hydrochloric acid (mass concentration is 36%) and 17.4 parts of deionized water are added dropwise at 15±2°C for 45 minutes, wherein the molar ratio of methyltrimethoxysilane to deionized water is 1:1.05;

[0079] S2: After the addition is completed, the temperature is raised to 65°C, refluxed and reacted for 4 hours, then the temperature is lowered to 50°C, sodium bicarbonate is added to adjust the system to neutrality, and the filtrate is collected and concentrated to obtain modified methoxy silicone resin 4.

[0080] Comparative Example 2

[0081] The comparative example of the present invention provides a modified methoxy silicone resin 5, the general structural formula of the modified methoxy silicone resin 5 is shown in Formula VI, the viscosity is 85 mPa·s,

[0082]

[0083] The preparation method of the modified methoxy silicone resin 5 comprises the following steps:

[0084] S1: After mixing 130 parts of methyltrimethoxysilane and 60 parts of toluene, 1 part of hydrochloric acid (mass concentration is 36%) and 17.4 parts of deionized water are added dropwise at 15±2°C for 45 minutes, wherein the molar ratio of methyltrimethoxysilane to deionized water is 1:1.05;

[0085] S2: After the addition is completed, the temperature is raised to 65°C, refluxed and reacted for 4 hours, then the temperature is lowered to 50°C, sodium bicarbonate is added to adjust the system to neutrality, and the filtrate is collected and concentrated to obtain methoxy silicone resin intermediate A;

[0086] S3: Mix methoxy silicone resin intermediate A, 50 parts of toluene, 80 parts of small molecule hydroxy silicone oil and 0.5 parts of potassium hydroxide evenly, heat to 100°C and react for 4 hours, evaporate the methanol small molecules, then introduce excess CO2 to neutralize the potassium hydroxide, then filter, collect the filtrate and concentrate to obtain modified methoxy silicone resin 5.

[0087] Example 4-12 Comparative Example 3-6

[0088] Examples 4-12 of the present invention and comparative examples 3-6 provide an organosilicon coating adhesive, and the component contents (parts by weight) of the organosilicon coating adhesive are shown in Table 1-2;

[0089] Table 1

[0090]

[0091]

[0092] Table 2

[0093]

[0094] The preparation methods of the organic silicon coating adhesives provided in Examples 4-12 and Comparative Examples 3-8 are as follows:

[0095] (1) The base rubber, methyl silicone oil, modified methoxy silicone resin and fluorescent indicator are mixed uniformly, and then heated to 110° C. under vacuum conditions and stirred and dispersed for 45 minutes;

[0096] (2) Cooling to 25°C, adding a crosslinking agent and dispersing for 5 min at normal pressure, and then vacuuming and dispersing for another 10 min;

[0097] (3) After adding the coupling agent and the catalyst under normal pressure and dispersing at a low speed for 8 minutes, the mixture is dispersed at a high speed for 25 minutes under vacuum conditions, and then discharged to obtain the silicone coating adhesive.

[0098] Effect example

[0099] The effect examples of the present invention verify the performance of the organic silicone coating adhesive prepared in Examples 4-12 and Comparative Examples 3-8, specifically including:

[0100] (1) Viscosity: Tested in accordance with GB / T 10247;

[0101] (2) Surface drying time: Tested in accordance with GB / T 13477.5-2003;

[0102] (3) Hardness: Tested in accordance with GB / T531-1999;

[0103] (4) Tensile strength: Test according to GB / T 528-2009. Pour the coated product into a polytetrafluoroethylene mold and dry it under ventilation at room temperature for 7 days before testing its performance.

[0104] (5) Dielectric strength: Tested in accordance with GB / T 1695;

[0105] (6) Volume resistivity: Tested in accordance with GB / T 1692;

[0106] (7) High temperature and high humidity (double 85): Tested in accordance with GB / T 15905-1995. The test material is PCBA circuit board. After sizing, ventilation and curing for 7 days, the performance can be tested.

[0107] (8) Salt spray resistance: Refer to the neutral salt spray project of GB / T 10125-2012 for testing. The test material is PCBA circuit board. After applying glue and ventilating and curing for 7 days, the performance can be tested.

[0108] The test results are shown in Table 3;

[0109] Table 3

[0110]

[0111]

[0112] It can be seen from Table 3 that when the preparation method of the present invention is adopted, the obtained organic silicone coating adhesive has the characteristics of moderate viscosity, moderate hardness, short surface drying time, high mechanical strength, high temperature and humidity resistance, excellent salt spray resistance, and excellent insulation. Specifically, the obtained viscosity is between 760-2000mPa·s, the surface drying time is between 8-16min, the hardness is between 40-60A, the tensile strength is above 3.1MPa, the dielectric strength is above 17KV / mm, and the volume resistivity is above 2.8*10 14 Ω·cm or above, and no bubbles or shedding occurs after 1000h high temperature and high humidity test and salt spray test, which means it still has good protection performance;

[0113] It can be seen from Example 4, Examples 7-9 and Comparative Examples 7-8 that the viscosity of the base glue will also affect the performance of the product. When the viscosity of the base glue is further preferably 7000-15000 mPa.s, the comprehensive performance of the obtained product is more excellent. Specifically, the surface drying time of the obtained product is less than 13 min, the tensile strength is more than 4.2 MPa, the dielectric strength is more than 20 KV / mm, and the volume resistivity is more than 1.3*1015 Ω·cm or more; when the viscosity of the base glue is too low and the molecular weight is too little (Comparative Example 7), the viscosity is significantly reduced to only 380mPa.s, and the surface drying time is significantly increased to 22min, which is 120% higher than that in Example 4, and the mechanical properties are reduced. Compared with Example 4, the tensile strength is reduced by 40.48%, and the elongation at break is reduced by 59.23%. Due to the small molecular weight, the methoxy content is high under the same conditions, and bubbles are easily generated in the cured film of the coating glue during application. Therefore, the high temperature and humidity resistance and salt spray resistance of the product are reduced; when the viscosity of the base glue is too high and the molecular weight is too large (Comparative Example 8), the cross-linking activity of the coating glue will be reduced, causing its performance to decline, and the viscosity of the base glue is too large, reaching 3200mPa.s, and the surface drying time is significantly increased to 30min, which is 200% higher than that in Example 4, which will seriously affect the construction performance of the coating glue.

[0114] It can be seen from Examples 4-6 and Comparative Examples 3-4 that when the number of components added is within the range given in the present invention, the obtained product has excellent comprehensive performance. When the number of modified methoxy silicone resins added is too small (Comparative Example 3), the obtained product has low mechanical properties, and the tensile strength is only 1.6 MPa, which is 61.9% lower than that of Example 4. The high temperature and humidity resistance and salt spray resistance are weak, and bubbles will be generated at the end of the test; when the number of modified methoxy silicone resins added is too large (Comparative Example 4), the mechanical properties of the obtained product decrease, and the high temperature and humidity resistance and salt spray resistance are also significantly reduced. A large number of bubbles will be generated in the high temperature and humidity experiment, and a small amount of bubbles will be generated in the salt spray resistance experiment accompanied by slight corrosion. This is because the modified methoxy silicone resin is excessive, resulting in the product being unable to combine well with the base glue during the curing process, resulting in poor performance.

[0115] It can be seen from Example 4, Examples 11-12 and Comparative Examples 5-6 that the structure of the modified methoxy silicone resin has a significant effect on the performance of the product. When the structure of the modified methoxy silicone resin provided in Comparative Examples 5-6 is not within the scope of the present invention, the performance of the obtained product shows a significant downward trend. Compared with Example 4, the modified methoxy silicone resin 4 in Comparative Example 5 does not use small molecule hydroxy silicone oil to combine with its block, the modified methoxy silicone resin has poor compatibility with the base glue, and silicone resin is easily generated during the curing process of the coating glue, and the base glue is separated, resulting in performance degradation, which is specifically reflected in the significant reduction in tensile strength and the significant deterioration of high temperature and humidity resistance and salt spray resistance. Among them, the tensile strength is reduced by 80.95% compared with Example 4, and a large number of bubbles are generated in the high temperature and humidity resistance test and the salt spray resistance test; the modified methoxy silicone resin 5 in Comparative Example 6 uses an excessive amount of small molecule hydroxy silicone oil, which ultimately leads to the deterioration of the reinforcement performance of the modified methoxy silicone resin, a significant decrease in mechanical properties, and a significant decrease in high temperature and humidity resistance and salt spray resistance, that is, the comprehensive performance of the product is significantly reduced.

[0116] Finally, it should be noted that the above embodiments are intended to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A silicone coating adhesive, It is characterized in that The organic silicone coating adhesive comprises the following raw materials in parts by weight: 80-100 parts of base adhesive, 1-5 parts of methyl silicone oil, 30-80 parts of modified methoxy silicone resin, 0.01-0.5 parts of fluorescent indicator, 3-10 parts of cross-linking agent, 0.5-5 parts of coupling agent, and 2-5 parts of catalyst; The base rubber is trimethoxy-terminated polydimethylsilane, with a viscosity of 1500-20000 mPa·s, and its structure is shown in Formula I, wherein n>1, Formula I; The modified methoxy silicone resin comprises the following raw materials in parts by mass: 100-150 parts of trifunctional silane, 0.1-1 parts of acidic catalyst, 40-60 parts of first organic solvent, 10-50 parts of small molecule hydroxy silicone oil, 30-50 parts of second organic solvent, and 0.01-0.5 parts of basic catalyst; the viscosity of the small molecule hydroxy silicone oil is 10-100 mPa·s; The preparation method of the modified methoxy silicone resin comprises the following steps: S1: After the trifunctional silane and the first organic solvent are mixed, an acidic catalyst and deionized water are added dropwise at 0-30°C for 30-60 minutes, wherein the molar ratio of the trifunctional silane to the deionized water is 1:(0.9-1.2); S2: After the addition is completed, heat to reflux and react for 4-6 hours, then cool to 48-52°C and adjust the system to neutral, filter, collect the filtrate, and concentrate to obtain methoxy silicone resin intermediate A; S3: Mix the methoxy silicone resin intermediate A, the second organic solvent, the small molecule hydroxy silicone oil and the alkaline catalyst evenly, heat to 80-110°C, react for 4-8 hours, and then introduce excess CO 2 The alkaline catalyst is neutralized, followed by suction filtration, and the filtrate is collected and concentrated to obtain a modified methoxy silicone resin.

2. The organic silicon coating adhesive according to claim 1, It is characterized in that The trifunctional silane is at least one of methyltrimethoxysilane, propyltrimethoxysilane, hexyltrimethoxysilane, cyclohexyltrimethoxysilane, nonyltrimethoxysilane, decyltrimethoxysilane, and dodecyltrimethoxysilane; the acidic catalyst is at least one of hydrochloric acid, trifluoromethanesulfonic acid, and concentrated sulfuric acid; the alkaline catalyst is potassium hydroxide or sodium hydroxide; the first organic solvent is at least one of benzene, toluene, and xylene; and the second organic solvent is at least one of benzene, toluene, and xylene.

3. The organic silicon coating adhesive according to claim 1, It is characterized in that The viscosity of the base glue is 7000-15000 mPa·s.

4. The organic silicon coating adhesive according to claim 1, It is characterized in that The viscosity of the methyl silicone oil is 50-500 mPa·s.

5. The organic silicon coating adhesive according to claim 1, It is characterized in that At least one of (a) to (d), (a) the fluorescent indicator is at least one selected from 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2-(2-hydroxy-3,5-di-tert-phenyl)-5-chlorobenzotriazole and 2,4,6-tris(2-n-butoxyphenyl)-1,3,5-triazine; (b) the crosslinking agent is at least one selected from methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, and acryltrimethoxysilane; (c) the coupling agent is at least one selected from vinyl trimethoxy silane, vinyl triethoxy silane, 3-(methacryloyloxy)propyl trimethoxy silane, 3-(2,3-epoxypropoxy)propyl trimethoxy silane, (3-aminopropyl) trimethoxy silane, γ-aminoethylaminopropyl trimethoxy silane, and γ-aminoethylaminopropyl triethoxy silane; (d) The catalyst is selected from titanate esters and their complexes.

6. A method for preparing the organic silicon coating adhesive according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: (1) Mix the base glue, methyl silicone oil, modified methoxy silicone resin and fluorescent indicator evenly, then heat to 100-120°C under vacuum and stir and disperse for 30-60 minutes; (2) Cooling to 23-28°C, adding a crosslinking agent and dispersing for 4-6 minutes at normal pressure, and then vacuuming and dispersing for another 5-10 minutes; (3) After adding the coupling agent and catalyst under normal pressure and dispersing at a low speed for 5-10 minutes, the mixture is dispersed at a high speed for 20-30 minutes under vacuum conditions, and then discharged to obtain the silicone coating adhesive.

7. Application of the organosilicon coating adhesive as claimed in any one of claims 1 to 5 in the electronics industry, LED plant lighting, automobile, aerospace or military fields.