A production method for producing electromagnetic pure iron DT4 hot-rolled round steel using VD process

Through the VD process and reasonable steelmaking and steel rolling processes, the problem of producing electromagnetic pure iron DT4 hot-rolled round steel in steel plants without RH vacuum equipment is solved, achieving the satisfaction of performance indicators and reduction of equipment requirements, and reducing the cost after rolling. The twisting problem of pure iron.

CN116287939BActive Publication Date: 2024-10-29BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202310236937.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-13
Publication Date
2024-10-29
Estimated Expiration
2043-03-13

AI Technical Summary

Technical Problem

In the existing technology, there is a lack of effective methods for producing electromagnetic pure iron DT4 hot-rolled round steel in steel plants without RH vacuum treatment equipment, resulting in high equipment requirements and low production efficiency.

Method used

The VD process is used to produce electromagnetic pure iron DT4 hot-rolled round steel, including blast furnace molten iron pretreatment, converter top and bottom blowing smelting, LF outside furnace refining, VD vacuum treatment and continuous casting, combined with reasonable steel rolling processes to control chemical composition and performance indicators. , such as tensile strength, elongation and Vickers hardness.

Benefits of technology

It realizes the production of electromagnetic pure iron without RH vacuum decarburization equipment, reduces equipment requirements, reduces the distortion problem of pure iron after rolling, and meets the performance indicators of tensile strength, elongation and hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004122716420000031
    Figure BDA0004122716420000031
  • Figure BDA0004122716420000032
    Figure BDA0004122716420000032
  • Figure BDA0004122716420000041
    Figure BDA0004122716420000041
Patent Text Reader

Abstract

The present invention discloses a production method for producing electromagnetic pure iron DT4 hot-rolled round steel by VD process, comprising: steelmaking process: blast furnace molten iron - molten iron pretreatment - converter top and bottom combined blowing smelting - LF refining outside the furnace - VD vacuum treatment - continuous casting; steel rolling process: billet heating - high-pressure water dephosphorization - Ф850mm billet opening machine - Ф700mm×3+Ф550mm×4 continuous rolling mill group rolling - sawing (sampling) - straightening - stacking (cooling, heat collection) - inspection - grinding - bundling - storage - delivery. The purpose of the present invention is to provide a production method for producing electromagnetic pure iron DT4 hot-rolled round steel by VD process, and its performance indicators meet the following requirements: tensile strength Rel≥265MPa, elongation A≥25%, and Vickers hardness≤195HV.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material metallurgy, and in particular to a production method for producing electromagnetic pure iron DT4 hot-rolled round steel by VD process. Background Art

[0002] Electromagnetic pure iron hot-rolled round steel is a functional material with excellent soft magnetic properties, which is widely used in relays, solenoid valves, DC motors and other fields. Electromagnetic pure iron is used in the largest amount of industrial pure iron, accounting for about 80%. Pure iron has good soft magnetic properties, high saturation magnetic induction intensity (2.16T), low coercive force Hc, high magnetic permeability μ and magnetic induction intensity B, good processability and weldability, simple manufacturing process and low cost. Electromagnetic pure iron is a high-performance and low-cost soft magnetic material that is indispensable for the development of science and technology. It reflects the direction and highest level of electrical steel research and development in the world today from a unique perspective, and will further develop in the direction of ultra-purification and functional diversification.

[0003] At present, most steel mills use RH vacuum treatment to produce electromagnetic pure iron. For some smaller steel mills that do not have RH vacuum treatment equipment, it is not easy to achieve. However, the present invention provides a production preparation method for producing electromagnetic pure iron DT4 hot-rolled round steel using a VD process. Summary of the invention

[0004] The purpose of the present invention is to provide a production method for producing electromagnetic pure iron DT4 hot-rolled round steel by VD process, and its performance indicators meet the following requirements: tensile strength Rel≥265MPa, elongation A≥25%, and Vickers hardness≤195HV.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] The invention discloses a production method for producing electromagnetic pure iron DT4 hot-rolled round steel by VD process, comprising: steelmaking process: blast furnace molten iron - molten iron pretreatment - converter top and bottom combined blowing smelting - LF refining outside the furnace - VD vacuum treatment - continuous casting; steel rolling process: billet heating - high-pressure water dephosphorization - Ф850mm billet opening machine - Ф700mm×3+Ф550mm×4 continuous rolling mill group rolling - sawing (sampling) - straightening - stacking (cooling, heat collection) - inspection - grinding - bundling - warehousing - delivery; wherein:

[0007] Steelmaking process: The composition requirements of blast furnace hot metal are Si≤0.45%, Mn≤0.40%, P≤0.120%, S≤0.030%; pre-treat the blast furnace hot metal for ≥20 minutes to make S≤0.015%;

[0008] Converter smelting: The converter is subjected to oxygen blowing to remove C and Mn. The converter tapping temperature is controlled between 1550-1600℃. The converter end point C≤0.003%, Mn≤0.10%, P≤0.010%;

[0009] VD vacuum treatment: VD adds Al for deoxidation before vacuum treatment, the Al content is between 0.20-0.70%, deep vacuum time ≥15min, vacuum degree ≤0.10KPa, argon blowing time after vacuum treatment ≥10min;

[0010] LF refining: Desulfurization is carried out in LF refining, and slag removal, re-slag making and heating operations are carried out during the process. The refining steel temperature is ≥1560℃;

[0011] Continuous casting: superheat is controlled between 30-40℃; casting machine speed is controlled between 0.6-0.65m / min;

[0012] Steel rolling process: The temperature of the preheating section of the steel rolling heating furnace is controlled at 600-800℃, the temperature of the soaking section is controlled at 1220-1250℃, and the insulation time is ≥3 hours; the starting rolling temperature is controlled at 1150-1200℃, and the final rolling temperature is 900-920℃; the temperature of the hot-rolled round steel entering the straightening machine is between 50-80℃.

[0013] Furthermore, the chemical composition of the round steel is calculated by mass percentage as follows: C≤0.005%, Mn≤0.20%, Si≤0.05%, P≤0.010, S≤0.010, Al: 0.20-0.70%, and the rest is Fe and unavoidable impurities.

[0014] Furthermore, the performance indicators of the round steel meet the following requirements: tensile strength Rel≥265MPa, elongation A≥25%, and Vickers hardness≤195HV.

[0015] Compared with the prior art, the beneficial technical effects of the present invention are:

[0016] The VD production process is used to produce electromagnetic pure iron, which is suitable for steel mills without RH vacuum decarburization equipment and can reduce the requirements of electromagnetic pure iron on production equipment.

[0017] By using a reasonable rolling process, the surface quality problems of rolled electromagnetic pure iron can be reduced and the distortion of pure iron after rolling can be reduced.

[0018] Its performance indicators meet the following requirements: tensile strength Rel≥265MPa, elongation A≥25%, Vickers hardness≤195HV. DETAILED DESCRIPTION

[0019] The present invention is further described below by means of specific examples. The examples are only for the purpose of explanation, and the protection scope of the present invention is not limited to these examples.

[0020] The present invention will be further described below:

[0021] Table 1 and Table 2 show the chemical composition of blast furnace molten iron and the process of molten iron pretreatment, and the chemical composition and tapping temperature of converter steel in various embodiments of the present invention.

[0022] Table 1 Chemical composition of molten iron and molten iron pretreatment process in the embodiment

[0023]

[0024] Table 2 Chemical composition and tapping temperature of converter steel

[0025] Example C% Mn% P% S% Steel tapping temperature ℃ 1 0.0020 0.08 0.09 0.007 1590 2 0.0015 0.06 0.08 0.009 1594

[0026] Table 3 Process parameters of refining and VD treatment

[0027]

[0028]

[0029] Table 4 Chemical composition of DT4 smelting

[0030] Example C% Si% Mn% P% S% Al% 1 0.0045 0.032 0.08 0.009 0.005 0.65 2 0.0040 0.035 0.09 0.008 0.003 0.63

[0031] Table 5 Heating and rolling process parameters of DT4 electromagnetic industrial pure iron

[0032]

[0033] Table 6 Mechanical properties test results of DT4 hot-rolled round steel

[0034] Example Tensile strength MPa Elongation % Vickers hardness HV 1 283 37 163 2 281 38 161

[0035] It can be seen from the above table that a VD process production method for producing electromagnetic pure iron DT4 hot-rolled round steel can achieve the requirements of technical indicators through reasonable steelmaking and rolling processes.

[0036] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A production method for producing electromagnetic pure iron DT4 hot-rolled round steel by VD process, characterized in that: include: Steelmaking process: blast furnace hot metal - hot metal pretreatment - converter top and bottom blowing smelting - LF refining outside the furnace - VD vacuum treatment - continuous casting; steel rolling process: billet heating - high-pressure water dephosphorization - Ф850mm billet opening machine - Ф700mm×3+Ф550mm×4 continuous rolling mill group rolling - sawing - straightening - stacking - inspection - grinding - bundling - warehousing - delivery; Among them: Steelmaking process: The composition requirements of blast furnace iron water are Si≤0.45%, Mn≤0.40%, P≤0.120%, S≤0.030%; pre-treat the blast furnace iron water for ≥20 minutes to make S≤0.015%; Converter smelting: The converter is subjected to oxygen blowing to remove C and Mn. The converter tapping temperature is controlled between 1550-1600℃. The converter end point C≤0.003%, Mn≤0.10%, P≤0.010%; VD vacuum treatment: VD adds Al for deoxidation before vacuum treatment, the Al content is between 0.20-0.70%, deep vacuum time is ≥15min, vacuum degree is ≤0.10KPa, and argon blowing time is ≥10min after vacuum treatment; LF refining: Desulfurization is carried out in LF refining, and slag removal, re-slag making and temperature raising operations are carried out during the process. The refining tapping temperature is ≥1560℃; Continuous casting: superheat is controlled between 30-40℃; casting machine speed is controlled between 0.6-0.65m / min; Steel rolling process: The temperature of the preheating section of the steel rolling heating furnace is controlled at 600-800℃, the temperature of the soaking section is controlled at 1220-1250℃, and the holding time is ≥3 hours; the starting rolling temperature is controlled at 1150-1200℃, and the final rolling temperature is 900-920℃; the temperature of the hot-rolled round steel entering the straightening machine is between 50-80℃; The chemical composition of the round steel is calculated by mass percentage as follows: C≤0.005%, Mn≤0.20%, Si≤0.05%, P≤0.010, S≤0.010, Al: 0.20-0.70%, and the rest is Fe and unavoidable impurities; The performance indicators of the round steel meet the following requirements: tensile strength Rel≥265MPa, elongation A≥25%, and Vickers hardness≤195HV.

Citation Information

Patent Citations

  • Method and apparatus for processing magnetite

    AU2019312556A1

  • Rare earth containing H profile steel with high strength and high toughness and production method thereof

    CN103266279A

  • Method for manufacturing electromagnetic pure iron

    CN103789609A

  • Smelting method for producing electromagnetic pure iron

    CN107779544A

  • Preparation method of high-hardenability hot-rolled round steel for engineering machinery

    CN113652604A