A high-strength, corrosion-resistant chain steel for mining and preparation method thereof

By optimizing the chemical composition and process flow of mining chain steel, the failure problem of mining chain steel in the corrosion environment is solved, high-strength, corrosion resistance and low-cost production are achieved, and production efficiency and market competitiveness are improved.

CN116288003BActive Publication Date: 2024-11-19JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310235349.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-13
Publication Date
2024-11-19
Estimated Expiration
2043-03-13

AI Technical Summary

Technical Problem

Existing mining chain steels are prone to corrosion and failure in humid and corrosive coal mine environments, and the production process is high, making it difficult to optimize costs.

Method used

By optimizing the chemical composition and process flow, C: 0.21-0.24%, Si: 0.15-0.35%, Mn: 1.25-1.40%, Cr: 0.50-0.70%, Mo: 0.55-0.65%, Ni: 1.05-1.15 % and V: 0.15-0.25% high-strength, corrosion-resistant chain steel, and adopts electric furnace smelting, LF refining, VD vacuum degassing, continuous casting, slow cooling, rolling and cooling control processes to eliminate the annealing process, improve production efficiency and Antioxidant properties.

Benefits of technology

It realizes high strength, corrosion resistance and low-cost production of mining chain steel, shortens the production process, improves market competitiveness, and enhances the corrosion resistance of the chain, and has excellent welding performance and dimensional accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288003B_ABST
    Figure CN116288003B_ABST
Patent Text Reader

Abstract

The invention relates to a high-strength and corrosion-resistant chain steel for mining. The chemical composition of the chain steel is calculated by mass percentage as follows: C: 0.21-0.24%, Si: 0.15-0.35%, Mn: 1.25-1.40%, P: ≤0.010%, S: ≤0.010%, Cr: 0.50-0.70%, Mo: 0.55-0.65%, Ni: 1.05-1.15%, V: 0.15-0.25%, and the balance is Fe and inevitable impurity elements. The whole process flow is: batching → electric furnace smelting → LF refining → VD vacuum degassing → continuous casting → slow cooling in a slow cooling pit → cold charging into a furnace for heating → high-pressure water descaling → billet rolling → slow cooling in a pit → cold charging into a furnace for heating → rolling forming (controlled rolling and controlled cooling) → stack cooling → straightening → finishing and warehousing. The diameter of the chain steel is 20-100mm, the yield strength is ≥1080MPa, the tensile strength is ≥1220MPa, the shrinkage is ≥48%, the elongation is ≥10%, the Charpy impact energy at room temperature is ≥60J, and the hardness in the delivery state is 240-260HB.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of special steel smelting, and specifically relates to a high-strength, corrosion-resistant chain steel for mining and a preparation method thereof. Background Art

[0002] Mining chain steel is used to manufacture mining chains. Chains are key bearing parts on scraper conveyors in coal mines. Chains work in a complex environment. Most coal mine environments are humid and corrosive. Corrosion failure is one of the main failure modes of mining chains. Therefore, the material is not only required to have high strength and toughness, but also corrosion resistance. By analyzing chains that have failed due to corrosion, most of the corrosion is manifested as oxidation on the surface of the chain. See the attached Figure 1 Therefore, the corrosion failure of the chain can be solved by improving the oxidation resistance of mining chain steel. In addition, with the increasing market competition pressure, all links in the coal mining process are pursuing cost optimization, and from the perspective of raw materials, costs also need to be reduced. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a high-strength, corrosion-resistant chain steel for mining and a preparation method thereof in response to the above-mentioned prior art, thereby optimizing the production process of the mining chain steel, achieving cost optimization, and making the steel more corrosion-resistant.

[0004] The technical solution adopted by the present invention to solve the above problems is: a high-strength, corrosion-resistant chain steel for mining, the chemical composition of the chain steel is C: 0.21-0.24%, Si: 0.15-0.35%, Mn: 1.25-1.40%, P: ≤0.010%, S: ≤0.010%, Cr: 0.50-0.70%, Mo: 0.55-0.65%, Ni: 1.05-1.15%, V: 0.15-0.25%, and the balance is Fe and unavoidable impurity elements.

[0005] The diameter of the chain steel is in the range of 20 to 100 mm.

[0006] The chemical composition of the high-strength, corrosion-resistant chain steel for mining of the present invention is determined as follows:

[0007] C: It is an element necessary to ensure the strength of steel, but too high C content is not good for the ductility and toughness of steel and significantly increases the carbon equivalent of the material, which is not good for the welding performance of steel. In order to ensure the plasticity, toughness, cutting and welding properties of chain steel, the carbon content should not be too high. In order to ensure the performance stability of the chain after heat treatment, the fluctuation of carbon content should not be too large. The present invention controls the carbon content to 0.21-0.24%.

[0008] Si: It is a deoxidizing element in steel and improves the strength of steel in the form of solid solution strengthening. When the Si content is less than 0.10%, the deoxidation effect is poor. When the Si content is higher, the brittleness of the steel is increased and the weldability of flash welding and the performance of the weld are reduced. The present invention controls the silicon content to 0.15-0.35%.

[0009] Mn: It is an element that improves the hardenability of steel and plays a role in solid solution strengthening to compensate for the strength loss caused by the reduction of C content in steel. Too high Mn content will increase its carbon equivalent and thus damage the welding performance. The Mn content of the present invention is controlled to be 1.25-1.40%.

[0010] Ni: To ensure the weldability of the material, the C and Mn contents of the chain steel are controlled to be relatively low, but in order to ensure hardenability, it is necessary to increase the alloy Ni. Due to the existence of open-pit mines, the low-temperature impact performance of the chain needs to be guaranteed. The present invention controls its content to 1.05-1.15%.

[0011] Cr: It is a medium carbide-forming element. When heated, Cr dissolved in austenite strongly improves hardenability. Part of Cr in steel replaces iron to form alloy cementite, improving stability; part of Cr is dissolved in ferrite, playing a solid solution strengthening role, improving the strength and hardness of ferrite. The present invention controls its content to 0.50-0.70%.

[0012] Mo: It exists in the solid solution and carbide of steel, has a solid solution strengthening effect, can improve the hardenability and tempering stability of steel, and can also refine the grains and improve the inhomogeneity of carbides, thereby improving the strength and toughness of steel. Mo is also a precious metal, and too high a content will increase the cost. In the present invention, the content of Mo is controlled at 0.55-0.65%.

[0013] S and P are harmful impurity elements in steel, which are easy to form defects such as segregation and inclusion. As impurity elements, they will have an adverse effect on the toughness of steel (especially the toughness of the core) and the toughness of the flash welding heat-affected zone, and their content should be reduced as much as possible. The present invention controls P: ≤ 0.010%, S: ≤ 0.010%.

[0014] V: It is an element that makes V (C, N) precipitate, which can significantly improve the strength of steel in the form of dispersed precipitation. The addition of V can improve the anti-tempering stability of the chain, but if the addition amount is too high, the toughness and welding performance of the steel will be reduced. The present invention controls its content to 0.15-0.25%.

[0015] The technical solution of the present invention to solve another technical problem is a method for manufacturing the above-mentioned high-strength, corrosion-resistant chain steel for mining. The entire process flow is: batching → electric furnace smelting → LF refining → VD vacuum degassing → continuous casting → slow cooling in slow cooling pit → cold charging into furnace heating → high-pressure water descaling → billet rolling → slow cooling in pit → cold charging into furnace heating → rolling and forming (controlled rolling and controlled cooling) → stacking cooling → straightening → finishing and warehousing.

[0016] The specific process steps are as follows:

[0017] First, the smelting raw materials are successively smelted in an electric furnace, LF refined, VD degassed and continuously cast to obtain a 300*340mm steel sheet that meets the chemical composition requirements. 2 In order to prevent P from returning to the subsequent process and ensure the P requirements of the finished product, the electric furnace must adopt the slag removal process to tap the steel, and the P content must be controlled below 0.008%;

[0018] The ingot is put into the slow cooling pit at high temperature. The temperature of the ingot must not be lower than 600℃. The slow cooling time must be more than 64 hours before it is taken out of the pit. Then the ingot is cold loaded into the heating furnace and heated at 1250-1300℃. It is kept warm for 4-5 hours before it is taken out of the furnace.

[0019] After descaling by high-pressure water, the billet is rolled into a size of 230*230mm. 2 After rolling, the intermediate billet is put into the pit for slow cooling, and the slow cooling time is more than 48 hours; the intermediate billet is cold loaded into the furnace for heating, the heating temperature is 1250-1300℃, and it is kept warm for 3-4 hours before being taken out of the furnace;

[0020] After the billet comes out of the heating furnace, it is dephosphorized with high-pressure water and rolled using a high-precision Kocks rolling mill. The final rolling temperature is 900-1000℃, and a controlled rolling and controlled cooling process is used. An insulation cover is added to the rolling line to strictly control the cooling rate of the material. The surface temperature drop of the material is ≤15℃ / minute, and the temperature of the material leaving the insulation cover is ≤300℃ to prevent the formation of martensite structure and reduce the proportion of bainite structure. Finally, "ferrite + pearlite + a small amount of bainite structure" is obtained, so that the hardness of the material is controlled within the range of 240-260HB, which is convenient for customers to unload materials, improves the organizational state before welding, is conducive to ring weaving, reduces high temperature resistance during welding, and improves the welding performance of the material.

[0021] Compared with the prior art, the advantages of the present invention are:

[0022] 1) Traditional mining chain steel needs to be annealed after rolling to meet customer material requirements. The present invention uses a controlled rolling and controlled cooling process to control the hardness of the hot-rolled material within the range of 240-260HB, eliminates the annealing process, shortens the production process of raw materials, improves production efficiency, and reduces material costs, thereby greatly increasing the market competitiveness of mining chain steel products.

[0023] 2) Based on the traditional mining chain steel, the present invention optimizes the chemical composition and increases the amount of Cr, Ni, Mo and V alloys, which greatly improves the oxidation resistance of the material itself, thereby enhancing the corrosion resistance of the chain.

[0024] 3) The chain steel of the present invention has a diameter of 20 to 100 mm, a yield strength of ≥1080 MPa, a tensile strength of ≥1220 MPa, a shrinkage of ≥48%, an elongation of ≥10%, a Charpy impact energy of ≥60 J at room temperature, and a hardness of 240-260 HB in the delivered state. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Corrosion failure diagram of mining chain prepared by traditional process. DETAILED DESCRIPTION

[0026] The present invention will be further described below with reference to examples.

[0027] Example 1

[0028] The diameter of the high-strength, corrosion-resistant chain steel for mining involved in this embodiment is 26 mm, and its chemical composition is as follows by mass percentage: C: 0.22%, Si: 0.18%, Mn: 1.32%, P: 0.008%, S: 0.005%, Cr: 0.59%, Mo: 0.61%, Ni: 1.12%, V: 0.18%, and the remainder is Fe and unavoidable impurity elements.

[0029] The manufacturing process of the chain steel is as follows: the smelting raw materials are configured according to the chemical composition of the above chain steel finished product, and the smelting is carried out in sequence through electric furnace smelting, LF refining, VD degassing and continuous casting to obtain a chain steel with a specification of 300*340mm that meets the chemical composition requirements. 2 The casting billet needs to adopt the slag removal process for electric furnace steel production, and the P content is 0.006%; the casting billet is put into the slow cooling pit at high temperature, the off-line temperature is 650℃, the slow cooling time is 70 hours, and then it is taken out of the pit; then the casting billet is cold loaded into the heating furnace for heating, the heating temperature is 1280℃, and it is kept warm for 4.5 hours before being taken out of the furnace; after descaling with high-pressure water, the billet is rolled, and the size of the billet rolled is 230*230mm 2 After rolling, the intermediate billet is put into the pit for slow cooling, and the slow cooling time is 52 hours; the intermediate billet is cold loaded into the furnace for heating, the heating temperature is 1290℃, and it is kept warm for 3.4 hours before being taken out of the furnace. The controlled rolling and controlled cooling process is used, and the high-precision Kocks rolling mill is used for rolling. The cooling rate of the material is strictly controlled. The final hardness control measured value of the material is 251HB.

[0030] The chain steel produced by the above manufacturing process has high strength, corrosion resistance and excellent flash welding performance. The dimensional accuracy sampling is shown in Table 1, and the mechanical properties and hardness values ​​are shown in Table 2.

[0031] Example 2

[0032] The diameter of the high-strength, corrosion-resistant chain steel for mining involved in this embodiment is 48 mm, and its chemical composition is as follows by mass percentage: C: 0.23%, Si: 0.20%, Mn: 1.34%, P: 0.009%, S: 0.003%, Cr: 0.61%, Mo: 0.62%, Ni: 1.14%, V: 0.22%, and the remainder is Fe and unavoidable impurity elements.

[0033] The manufacturing process of the chain steel is as follows: the smelting raw materials are configured according to the chemical composition of the above chain steel finished product, and the smelting is carried out in sequence through electric furnace smelting, LF refining, VD degassing and continuous casting to obtain a chain steel with a specification of 300*340mm that meets the chemical composition requirements. 2 The casting billet needs to adopt the slag removal process for electric furnace steel production, and the P content is 0.005%; the casting billet is put into the slow cooling pit at high temperature, the off-line temperature is 645℃, the slow cooling time is 68 hours, and then it is taken out of the pit; then the casting billet is cold loaded into the heating furnace for heating, the heating temperature is 1285℃, and it is kept warm for 4.6 hours before being taken out of the furnace; after descaling with high-pressure water, the billet is rolled, and the size of the billet rolled is 230*230mm 2 After rolling, the intermediate billet is put into the pit for slow cooling, and the slow cooling time is 55 hours; the intermediate billet is cold loaded into the furnace for heating, the heating temperature is 1280℃, and it is kept warm for 3.4 hours before being taken out of the furnace. The controlled rolling and controlled cooling process is used, and the high-precision Kocks rolling mill is used for rolling. The cooling rate of the material is strictly controlled. The final hardness control measured value of the material is 245HB.

[0034] The chain steel produced by the above manufacturing process has high strength, corrosion resistance and excellent flash welding performance. The dimensional accuracy sampling is shown in Table 1, and the mechanical properties and hardness values ​​are shown in Table 2.

[0035] Table 1 Random inspection of chain steel sizes produced in various embodiments (20 pieces)

[0036]

[0037]

[0038] Table 2 Mechanical properties of chain steel produced in each embodiment

[0039]

[0040] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing high-strength, corrosion-resistant chain steel for mining, characterized in that: The chemical composition of the chain steel is C: 0.21-0.24%, Si: 0.15-0.35%, Mn: 1.25-1.40%, P: ≤0.010%, S: ≤0.010%, Cr: 0.50-0.70%, Mo: 0.55-0.65%, Ni: 1.05-1.15%, V: 0.15-0.25%, and the balance is Fe and inevitable impurity elements; the whole process flow is: batching → electric furnace smelting → LF refining → VD vacuum degassing → continuous casting → slow cooling in a slow cooling pit → cold charging into a furnace for heating → high-pressure water descaling → billet rolling → slow cooling in a slow cooling pit → cold charging into a furnace for heating → rolling and forming → stack cooling → straightening → finishing and warehousing; the method mainly comprises the following steps: 1) First, the smelting raw materials are successively smelted in an electric furnace, LF refined, VD degassed and continuously cast to obtain a product that meets the chemical composition requirements and has a specification of 300*340mm. 2 of the casting billet; 2) Put the ingot into the slow cooling pit at high temperature. The temperature of the ingot must not be lower than 600℃. The slow cooling time must be more than 64 hours before leaving the pit. 3) Then the ingot is cold loaded into the heating furnace for heating at a temperature of 1250-1300°C and kept at this temperature for 4-5 hours before being taken out of the furnace; 4) After descaling with high-pressure water, the billet is rolled to a size of 230*230mm 2 ; Adopt controlled rolling and controlled cooling process, add heat preservation cover on the rolling line to control the cooling speed of the material, the temperature drop of the material surface is ≤15℃ / minute, and the temperature of the material leaving the heat preservation cover is ≤300℃; 5) After rolling, the intermediate billet is put into the pit for slow cooling, and the slow cooling time is greater than 48 hours; 6) The intermediate billet is cold loaded into the furnace for heating at a temperature of 1250-1300°C and kept warm for 3-4 hours before being taken out of the furnace; 7) After the billet comes out of the heating furnace, it is descaled with high-pressure water and rolled using a high-precision Kocks rolling mill with a final rolling temperature of 900-1000℃.

2. The method for preparing a high-strength, corrosion-resistant chain steel for mining according to claim 1, characterized in that: The diameter of the chain steel is 20-100 mm.

3. The method for preparing a high-strength, corrosion-resistant chain steel for mining according to claim 1, characterized in that: The chain steel has a yield strength of ≥1080MPa, a tensile strength of ≥1220MPa, a shrinkage of ≥48%, an elongation of ≥10%, a Charpy impact energy of ≥60J at room temperature, and a hardness of 240-260HB in the delivery state.

4. The method for preparing a high-strength, corrosion-resistant chain steel for mining according to claim 1, characterized in that: The chain steel has a structure of ferrite+pearlite+a small amount of bainite.

5. The method for preparing a high-strength, corrosion-resistant chain steel for mining according to claim 1, characterized in that: During the smelting process, the electric furnace steel is tapped using the slag removal process, and the P content is controlled below 0.008%.