A modified attapulgite-based material and its preparation method and application
Modified attapulgite-based materials are prepared by grinding and acidic modification of attapulgite, and loading sulfur, which solves the problems of poor adsorption effect and high cost in electroplating wastewater treatment, and achieves efficient silver ion adsorption and resource recovery. .
Patent Information
- Application Number
- CN202310122146.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-16
AI Technical Summary
In the existing technology, the adsorbents used to treat electroplating wastewater have problems such as poor effectiveness, short service life, and high cost. Especially for the treatment of silver-containing wastewater, the exchange resin is expensive and non-renewable, and the adsorbent material has a short service life.
By grinding and acidifying attapulgite, and loading sulfur on its surface, a modified attapulgite-based material is prepared, which enhances its adsorption capacity and efficiency for silver ions, reduces production costs, and facilitates recycling through magnetization properties.
It significantly improves the adsorption effect and efficiency of silver ions on modified attapulgite-based materials, reduces usage costs, expands the treatment ideas for silver-containing wastewater, and achieves efficient resource recovery.
Smart Images

Figure BDA0004080322940000041 
Figure BDA0004080322940000042 
Figure BDA0004080322940000051
Abstract
Description
Technical Field
[0001] The invention relates to the field of electroplating wastewater treatment materials, and in particular to a attapulgite-based material modified by sulfur loading acidity, and a preparation method and application thereof. Background Art
[0002] With the rapid development of society, heavy-duty industries represented by the electronic information industry generate a large amount of industrial wastewater every year. Electroplating wastewater is a typical heavy metal-contaminated wastewater. At present, electroplating wastewater has become one of the three major pollution sources in the world. Its discharge without meeting the standards will pollute rivers, lakes, and seas, infiltrate into the soil, and destroy crops, endanger aquatic life and human and animal health. At the same time, electroplating wastewater also has certain resource attributes. Among them, silver-containing wastewater is one of the most harmful heavy metal wastewaters. It has a wide range of sources, complex components, different properties, great environmental hazards, fast water diffusion, high biological toxicity, and is easy to accumulate in organisms. In addition, silver is a widely used valuable metal. Direct discharge not only pollutes the environment but also wastes silver resources. Therefore, conducting research on resource treatment and deep purification of silver-containing wastewater has the dual significance of environmental protection and resource security.
[0003] Silver is widely present in industrial production fields such as electroplating and metallurgy. The silver-containing wastewater generated is mainly divided into three types: fixing wastewater, electroplating wastewater, and experimental and analytical wastewater. Heavy metal pollution, especially the treatment of highly toxic and highly stable heavy metal wastewater, has attracted more and more attention from all walks of life and scientific researchers, and the discharge of silver-containing wastewater has also been strictly controlled. According to the latest national "Electronic Industry Water Pollution Emission Standard" (GB 39731-2020), from July 1, 2021, the concentration of silver in wastewater discharged by pollutant discharge units into environmental water bodies shall not exceed 0.3 mg / L.
[0004] At present, the commonly used methods for treating silver-containing electroplating wastewater are: ion exchange method, chemical precipitation method, electrolysis method, adsorption method, etc. Each method has its own advantages and disadvantages. For example, the chemical precipitation method is simple to operate, low in cost, and suitable for high-concentration silver-containing wastewater, but there are problems such as large amount of slag and secondary pollution; the ion exchange method is suitable for treating medium and low-concentration silver-containing wastewater, but the exchange resin capacity is limited and it is easy to be contaminated; the advantages of the adsorption method are mainly strong selectivity, high sensitivity, short response time, and large adsorption capacity, but there are problems such as short service life of the adsorption material, difficulty in recycling the adsorbed ions, and high cost. Summary of the invention
[0005] The invention provides a modified attapulgite-based material and a preparation method and application thereof, which are used to solve the technical problems of poor adsorption effect, short service life and high use cost existing in the adsorbent for treating electroplating wastewater.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A method for preparing a modified attapulgite-based material comprises the following steps:
[0008] (1) The surface of attapulgite is modified by grinding, and the ground attapulgite is mixed with an acid and heated for a set reaction time to obtain acid-modified attapulgite.
[0009] (2) The acid-modified attapulgite and the sulfiding agent are uniformly mixed in a solvent and then heated to 60-90° C. for reaction for 1-2 hours. After the reaction is completed, the solid matter is separated to obtain the modified attapulgite-based material.
[0010] The design idea of the above technical scheme is that in the prior art, silver-containing wastewater is mainly recycled and treated by ion exchange resin, but ion exchange resin is expensive and non-renewable compared with attapulgite. The present invention utilizes the physicochemical properties of attapulgite and its special layered chain structure, prepares a modified material with attapulgite as raw material, and uses it as a treatment material for silver-containing electroplating wastewater for the first time, thereby improving the adsorption of the material, reducing its production and use costs, and expanding the current treatment ideas for silver-containing wastewater. At the same time, the present invention also designs and optimizes the preparation method according to the adsorption effect of attapulgite-based materials. First, The attapulgite is modified by grinding, and the continuity of grinding is used to increase the specific surface area of the attapulgite. Then, the number of pores in the attapulgite is increased and the specific surface area is further increased through acid modification. At the same time, the acid modification can also achieve the purpose of removing impurities (such as carbonates) and unblocking the pores. Then, sulfur loading is carried out on this basis to make the attapulgite contain more active sulfur sites, thereby enhancing the material's adsorption capacity for silver ions, and utilizing the sustained release effect of the sulfur loaded on the material to improve the material's adsorption efficiency for silver ions, thereby greatly improving the adsorption effect and efficiency of the modified attapulgite-based material for silver ions.
[0011] As a further preferred embodiment of the above technical solution, the sulfiding agent is a soluble sulfide salt or a sulfur-containing mineral; the mass ratio of the sulfiding agent to the acid-modified attapulgite is (2-5):1. The main basis for the addition of the sulfiding agent is the mass ratio of attapulgite to the sulfiding agent. The higher the sulfiding agent is loaded on the attapulgite, the stronger its adsorption capacity for silver ions is. However, an excessively large addition ratio of the sulfiding agent will lead to a decrease in the loading effect and an increase in the cost of the agent. According to the inventor's experiments and research, when the mass ratio of attapulgite to the sulfiding agent (g) is 1:2-1:5, the sulfur loading effect is better, and both the production cost and the loading effect can be taken into account.
[0012] As a further preferred embodiment of the above technical solution, the sulfiding agent includes at least one of potassium sulfide, sodium sulfide, ammonium sulfide, pyrite, chalcopyrite and molybdenite. The sulfidation modification of attapulgite mainly increases the sulfur active sites on the surface of attapulgite. This preferred solution selects the above sulfiding agent with good solubility or sulfide mineral with fine particle size as the preferred material type, which can effectively improve the loading amount of sulfidation and enhance the adsorption capacity of the material for silver ions.
[0013] As a further preferred embodiment of the above technical solution, the reaction temperature of the ground attapulgite and the acid in step (1) is 25-50°C, and the reaction time is 1-2h. The reaction temperature is generally room temperature. Heating can accelerate the reaction rate and thus reduce the reaction time, but heating will also increase energy consumption and production costs. The reaction temperature range of this preferred solution can take into account both the reaction rate and production costs; the acid modification of attapulgite is mainly to remove impurities on its surface and dredge the pores, so the longer the reaction time is, the better. On the contrary, too long a reaction time will also destroy the structure of the attapulgite and lead to a weakening of the adsorption performance. Therefore, the reaction time of this preferred solution avoids the problem of a decrease in the material adsorption capacity due to too long a reaction time while ensuring the degree of the acid modification reaction.
[0014] As a further preferred embodiment of the above technical solution, the acid includes at least one of hydrochloric acid and nitric acid; the concentration of the acid is 4 mol / L, and the liquid-to-solid ratio of the acid to the attapulgite after grinding is (15-25 mL): 1 g.
[0015] As a further preferred embodiment of the above technical solution, the particle size of the attapulgite after surface modification by grinding in step (1) is 200-400 meshes.
[0016] As a further preferred embodiment of the above technical solution, after the reaction of the acid-modified attapulgite and the sulfiding agent in step (2) is completed, the separated solid is prepared into a solution, and an iron salt solution is added dropwise under stirring to react, and the reaction system temperature is maintained at 60 to 90°C, the pH is 4 to 10, and the reaction time is 1 to 2 hours, so as to obtain the modified attapulgite-based material. This preferred solution adds a magnetic material to the solid so that the modified attapulgite-based material finally obtained has a magnetic property, which facilitates the recovery of the material after use and reduces the cost of the material.
[0017] Based on the same technical concept, the present invention also provides a modified attapulgite-based material, which is prepared by the preparation method of the above technical solution.
[0018] Based on the same technical concept, the present invention also provides an application of the above-mentioned modified attapulgite-based material, wherein the modified attapulgite-based material is used to adsorb silver ions in silver-containing electroplating wastewater, comprising the following operations: adding the modified attapulgite-based material to the silver-containing electroplating wastewater for adsorption, filtering and separating after the adsorption is completed and drying the solid, adding the dried modified attapulgite-based material to a thiosulfate solution for desorption, the reaction time is 40 to 60 minutes, and after the reaction is completed, a precious liquid containing silver metal complex ions is separated and obtained, and the precious liquid is electrolyzed to achieve silver recovery.
[0019] As a further preferred embodiment of the above technical solution, the concentration of the thiosulfate solution is 1 mol / L, and the solid-liquid ratio of the dried modified attapulgite-based material to the thiosulfate solution is 1 g: (15-20) mL.
[0020] As a further preferred embodiment of the above technical solution, when the modified attapulgite-based material is used to adsorb silver ions in silver-containing electroplating wastewater, the added concentration of the modified attapulgite-based material in the silver-containing electroplating wastewater is 0.1 to 0.5 g / L.
[0021] Compared with the prior art, the advantages of the present invention are:
[0022] The modified attapulgite-based material prepared by the present invention applies attapulgite to the treatment of silver-containing electroplating wastewater for the first time, expands the treatment ideas of silver-containing wastewater, and greatly improves the treatment effect and efficiency of the modified attapulgite-based material on silver-containing wastewater through the design of the preparation process, reduces its recovery difficulty and use cost, and increases the practicality of its application; the preparation method of the present invention has a simple process flow, easily available raw materials, and low production cost, which is conducive to large-scale industrial production. DETAILED DESCRIPTION
[0023] The present invention is further described in detail below in conjunction with specific embodiments.
[0024] Embodiment 1:
[0025] The modified attapulgite-based material of this embodiment is prepared by the following steps:
[0026] (1) The attapulgite is ground for surface modification, and the particle size of the ground attapulgite is 200 mesh; the ground attapulgite is mixed with 4 mol / L hydrochloric acid at a liquid-solid ratio of 15 mL:1 g, and then heated to 25° C. for reaction for 2 h, and then washed with deionized water until neutral, and dried to obtain acid-modified attapulgite.
[0027] (2) The acid-modified attapulgite and sodium sulfide were mixed in deionized water at a mass ratio of 2:1, and the stirring speed was maintained at 150 r / min. The mixture was heated to 60° C. and reacted for 2 h. After the reaction was completed, a solid was separated and obtained.
[0028] (3) The solid material in step (2) is prepared into a solution, and an iron salt solution and sodium hydroxide are added dropwise under stirring to react, the reaction system temperature is maintained at 60° C., the pH is 4-10, and the reaction time is 2 h. After the reaction is completed, the solution is allowed to stand for separation and washed with deionized water until neutral, thereby obtaining the modified attapulgite-based material of this embodiment.
[0029] The modified attapulgite-based material of this embodiment is used to treat the silver-containing electroplating wastewater. The specific operation is to add the modified attapulgite-based material of this embodiment to the silver-containing electroplating wastewater for adsorption, filter and separate after adsorption, and dry the solid, and add the dried modified attapulgite-based material to the thiosulfate solution for desorption. The concentration of the thiosulfate solution is 1 mol / L, the solid-liquid ratio of the modified attapulgite-based material to the thiosulfate solution is 1g:15mL, and the reaction time is 40min. After the reaction is completed, the precious liquid containing silver metal complex ions is separated and the precious liquid is electrolyzed to achieve silver recovery. Among them, the addition amount of the modified attapulgite-based material added to the silver-containing electroplating wastewater in this embodiment is 0.1g / L, 0.2g / L, and 0.5g / L (divided into three groups for comparative analysis), the adsorption reaction temperature is 25°C, the pH is 5.6, and the adsorption time is 5min, 10min, 20min, and 30min, respectively. The final treatment effect is shown in Table 1.
[0030] Table 1: Treatment effect of the modified attapulgite-based material of Example 1 on silver-containing electroplating wastewater at different addition amounts and adsorption times
[0031]
[0032] It can be seen from Table 1 that when the amount of modified attapulgite-based material, solution pH, reaction temperature and stock solution concentration of this embodiment are constant, the silver removal rate continues to increase with the increase of adsorption time, and the longer the adsorption time, the smaller the increase in removal rate, indicating that the optimal adsorption time is about 20 to 30 minutes; when the adsorption time, solution pH, reaction temperature and stock solution concentration are constant, with the increase of the amount of modified attapulgite-based magnetized material of this embodiment, the removal rate of silver ions continues to increase, and its removal efficiency can reach more than 96%.
[0033] This example further studies the effect of silver-containing electroplating wastewater with different silver ion contents on the adsorption effect of the modified attapulgite-based material of this example. The results are shown in Tables 2 and 3, wherein Table 2 shows the treatment results of silver-containing electroplating wastewater with an initial silver ion concentration of 27 mg / L, and Table 3 shows the treatment results of silver-containing electroplating wastewater with an initial silver ion concentration of 13.5 mg / L (the reaction conditions of both are consistent with Table 1).
[0034] Table 2: Treatment effect of the modified attapulgite-based material of Example 1 on silver-containing electroplating wastewater (silver ion concentration of 27 mg / L)
[0035]
[0036]
[0037] Table 3: Treatment effect of the modified attapulgite-based material of Example 1 on silver-containing electroplating wastewater (silver ion concentration of 13.5 mg / L)
[0038]
[0039] It can be seen from Table 2 and Table 3 that the modified attapulgite-based material of this embodiment has a good treatment effect on silver-containing electroplating wastewater with different initial silver ion concentrations.
[0040] Embodiment 2:
[0041] The modified attapulgite-based material of this embodiment is prepared by the following steps:
[0042] (1) The attapulgite is ground for surface modification, and the particle size of the ground attapulgite is 100 mesh; the ground attapulgite is mixed with 4 mol / L nitric acid at a liquid-solid ratio of 25 mL:1 g, heated to 50° C. for reaction for 1 h, washed with deionized water until neutral, and dried to obtain acid-modified attapulgite.
[0043] (2) The acid-modified attapulgite and pyrite were mixed in deionized water at a mass ratio of 5:1, and the stirring speed was maintained at 150 r / min. The mixture was heated to 90° C. for 1 h. After the reaction was completed, a solid was separated and obtained.
[0044] (3) The solid material in step (2) is prepared into a solution, and an iron salt solution and sodium hydroxide are added dropwise under stirring to react, the reaction system temperature is maintained at 90° C., the pH is 4-10, and the reaction time is 1 h. After the reaction is completed, the solution is allowed to stand for separation and washed with deionized water until neutral, thereby obtaining the modified attapulgite-based material of this embodiment.
[0045] The modified attapulgite-based material of this embodiment is used to treat the silver-containing electroplating wastewater. The specific operation is to add the modified attapulgite-based material of this embodiment to the silver-containing electroplating wastewater for adsorption, filter and separate after the adsorption, and dry the solid, and add the dried modified attapulgite-based material to a thiosulfate solution for desorption. The concentration of the thiosulfate solution is 1 mol / L, the solid-liquid ratio of the modified attapulgite-based material to the thiosulfate solution is 1 g:20 mL, and the reaction time is 60 min. After the reaction is completed, a precious liquid containing silver metal complex ions is separated and electrolyzed to achieve silver recovery.
[0046] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. For those skilled in the art, improvements and changes obtained without departing from the technical concept of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. An application of a modified attapulgite-based material, characterized in that: The modified attapulgite-based material is used to adsorb and recover silver ions in silver-containing electroplating wastewater, comprising the following operations: adding the modified attapulgite-based material to the silver-containing electroplating wastewater for adsorption, filtering and separating after the adsorption is completed and drying the solid, adding the dried modified attapulgite-based material to a thiosulfate solution for desorption, the reaction time is 40 to 60 minutes, separating and obtaining a precious liquid containing silver metal complex ions after the reaction is completed, and electrolyzing the precious liquid to achieve silver recovery; The modified attapulgite-based material is prepared by the following preparation method: (1) grinding the attapulgite for surface modification, mixing the ground attapulgite with an acid and heating the mixture for a set reaction time to obtain acid-modified attapulgite; (2) The acid-modified attapulgite and the sulfiding agent are mixed evenly in a solvent and then heated to 60-90° C. for reaction for 1-2 hours. After the reaction is completed, the solid matter is separated to obtain the modified attapulgite-based material; the sulfiding agent is a soluble sulfide salt or a sulfur-containing mineral.
2. The use of the modified attapulgite-based material according to claim 1, characterized in that: The mass ratio of the vulcanizing agent to the acid-modified attapulgite is (2-5):
1.
3. The use of the modified attapulgite-based material according to claim 2, characterized in that: The sulfiding agent includes at least one of potassium sulfide, sodium sulfide, ammonium sulfide, pyrite, chalcopyrite and molybdenite.
4. The use of the modified attapulgite-based material according to claim 1, characterized in that: In step (1), the reaction temperature of the ground attapulgite and the acid is 25-50° C., and the reaction time is 1-2 hours.
5. The use of the modified attapulgite-based material according to claim 1, characterized in that: The acid includes at least one of hydrochloric acid and nitric acid; the concentration of the acid is 4 mol / L, and the liquid-solid ratio of the acid to the attapulgite after grinding is (15-25 mL): 1 g.
6. The use of the modified attapulgite-based material according to claim 1, characterized in that: The particle size of the attapulgite after surface modification by grinding in step (1) is 200-400 meshes.
7. The use of the modified attapulgite-based material according to any one of claims 1 to 6, characterized in that: After the reaction of the acid-modified attapulgite and the sulfiding agent in step (2) is completed, the separated solid is configured into a solution, and an iron salt solution is added dropwise under stirring to react, the reaction system temperature is maintained at 60-90°C, the pH is 4-10, and the reaction time is 1-2h. After the reaction is completed, the modified attapulgite-based material is obtained.
8. The use of the modified attapulgite-based material according to any one of claims 1 to 6, characterized in that: When the modified attapulgite-based material is used to adsorb silver ions in silver-containing electroplating wastewater, the added concentration of the modified attapulgite-based material in the silver-containing electroplating wastewater is 0.1-0.5 g / L.
Citation Information
Patent Citations
Composite reagent for deep removal of heavy metals in wastewater and preparation method thereof
CN103482750A
Hydrothermal method for preparing creamy white attapulgite
CN104261421A
Silver ammonia wastewater processing method
CN109205842A
Method for recovering precious metal complexing ion from thiosulfate leachate by using sulfide ore
CN109652658A
Preparation method of supported molybdenum disulfide silver ion adsorbent
CN111589417A