A cationized sugarcane loaded nanosilver composite material and its preparation method and application
By reducing silver ions to nanoparticles using eutectic solvents and cationically modified sugarcane, the problems of high pollution and energy consumption in the preparation of silver nanoparticles are solved, and efficient dye adsorption and catalytic effects are achieved.
Patent Information
- Application Number
- CN202310224296.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art requires additional reducing agents and stabilizers when preparing silver nanoparticles, resulting in high environmental pollution and energy consumption, and silver nanoparticles are prone to agglomeration, affecting the experimental effect.
The sugarcane was pretreated by eutectic solvent synthesized by tetraethylammonium hydroxide and 1,3-dimethylurea, and the cationic agent 2,3-epoxypropyltrimethylammonium chloride was added for cationic modification. , the lignin reducing properties in sugar cane are used to reduce silver ions to silver nanoparticles to form cationized sugar cane-loaded nanosilver composite material.
Achieve green, pollution-free and low energy consumption silver nanoparticles preparation, inhibit the agglomeration of silver nanoparticles, improve the adsorption and catalytic properties of dyes, especially when removing Congo red and methyl orange in dye wastewater High efficiency.
Smart Images

Figure CN116328733B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material synthesis, and in particular relates to a cationized sugarcane-loaded nano-silver composite material and a preparation method and application thereof. Background Art
[0002] In recent years, as people's environmental awareness increases, it is of great significance to improve the efficient utilization of biomass and the treatment methods of dye wastewater. Among them, the role of precious metal nanoparticles in the chemical reduction and decolorization of dyes has gradually attracted widespread attention from experts and scholars. In particular, silver nanoparticles (abbreviated as nanosilver) as a new functional material has gradually attracted people's attention. Because of its unique properties of nanomaterials, it has been widely used in many fields such as antibacterial, catalysts, medicine and new energy.
[0003] The most widely used method for reducing silver nanoparticles is the chemical method, which requires the additional addition of reducing agents and stabilizers such as hydrazine, hydrazine hydrate, ascorbic acid and other chemical reagents, which are harmful to the human body and the environment. In addition, the prepared silver nanoparticles are prone to interconnection and form larger particle clusters from multiple particles during separation, processing and storage, which affects the experimental results. Therefore, it is crucial to select a carrier skeleton that has both reducing properties and a rich network structure to reduce silver ions to silver nanoparticles without agglomeration.
[0004] Biological methods for in-situ generation of precious metal nanoparticles using certain reducing components in plants have received increasing attention. Sugarcane, as a three-dimensional porous material, is rich in the reducing component lignin. The natural channels inside sugarcane and the nanopores on the channels can serve as a natural reaction platform and a skeleton for loading silver nanoparticles. They contain functional groups of various reducing lignin components, such as phenol and methoxyl groups, which can reduce silver ions to silver nanoparticles under certain conditions. In-situ reduction and fixation of silver nanoparticles can effectively alleviate the agglomeration effect of silver nanoparticles. However, the fiber bundles on the sugarcane cell wall are tightly entangled, and the exposed available reducing lignin groups are limited, which is not conducive to the reduction of silver nanoparticles. Therefore, it is necessary to pretreat the sugarcane raw material. However, conventional pretreatment methods such as mechanical treatment require large energy consumption and enzyme treatment methods have low treatment efficiency, which have many shortcomings.
[0005] Deep eutectic solvents (DESs) are easy to prepare, low in toxicity and biodegradable, and can be used as green solvents or reactants for sugarcane pretreatment. In addition, DES can be recycled and reused, which helps to reduce production costs. Structurally, DES consists of at least one hydrogen bond donor (HBD) and one hydrogen bond acceptor (HBA), has strong hydrogen bonds and a low melting point, and the low eutectic solvent synthesized from tetraethylammonium hydroxide and 1,3-dimethylurea can be mixed into a colorless and transparent liquid at room temperature. Patent Publication No. CN115160591A discloses a method for quickly and efficiently deconstructing lignocellulose using an alkaline low eutectic solvent, wherein the alkaline low eutectic solvent is a binary system composed of a mixture of a hydrogen bond acceptor, a hydrogen bond donor and an alkaline auxiliary agent, benzyltrimethylammonium chloride and a polyol, and an additional alkaline auxiliary agent is sodium sulfide to deconstruct lignin. Although this method can successfully dissociate lignocellulose, it requires additional alkaline auxiliary agents to achieve the reaction conditions, which is easy to pollute the environment.
[0006] In order to give functionality to sugarcane pretreated with DES, a cationic agent is added in the presence of DES so that the cationic groups are grafted onto the hydroxyl sites of cellulose, which has better electrostatic attraction to anionic dyes. 2,3-Epoxypropyltrimethylammonium chloride has high cationization efficiency and commercial value. According to scientific research on cellulose cationization, the modification process is an etherification reaction. Using 2,3-Epoxypropyltrimethylammonium chloride as a modifier, the adsorption capacity of the material or the adsorption performance of pollutants with different charge properties is changed. At the same time, quaternary ammonium salts have lower cytotoxicity and are considered to be a promising modified material.
[0007] Therefore, it is necessary to find a green modified biomass in situ reduction method for silver nanoparticles that does not require additional reaction reagents, has a simple preparation process, mild reaction conditions and low energy consumption. Summary of the invention
[0008] In view of the above problems, the present invention provides a cationized sugarcane-loaded nano-silver composite material and its preparation method and application. The silver ions are reduced to silver nanoparticles and fixed on the surface of the cationized sugarcane three-dimensional network by utilizing the reducing property of lignin in the cation-modified sugarcane, thereby obtaining a cationized sugarcane-loaded nano-silver composite material. The material of the present invention has good adsorption and catalytic properties and can be used for the adsorption and removal of organic dyes. Moreover, the preparation process of the material is green and pollution-free, with mild reaction conditions and low energy consumption.
[0009] The present invention is achieved through the following technical solutions:
[0010] A cationized sugarcane-loaded nano-silver composite material is prepared by pretreating sugarcane with a low eutectic solvent synthesized from tetraethylammonium hydroxide and 1,3-dimethylurea, then adding a cationic agent 2,3-epoxypropyltrimethylammonium chloride for cation modification, using the obtained cationized sugarcane as a carrier, utilizing the reducing property of the lignin component in the sugarcane to reduce silver ions into silver nanoparticles and fix them on the surface of the carrier, thereby obtaining the cationized sugarcane-loaded nano-silver composite material.
[0011] In the cationized sugar cane loaded nano-silver composite material of the present invention, the surface potential of the cationized sugar cane is 20.7-33.2 mV, and the diameter distribution of the silver nano-particles is 50-1000 nm.
[0012] A method for preparing the cationized sugarcane-loaded nanosilver composite material as described above comprises the following steps:
[0013] (1) Pretreatment of sugarcane: peeling and cutting sugarcane into pieces, immersing the pieces in hot water and freeze-drying the pieces to remove sugar, and uniformly mixing the sugarcane with a low eutectic solvent prepared from tetraethylammonium hydroxide and 1,3-dimethylurea to obtain pretreated sugarcane;
[0014] (2) Cationic modification of sugarcane: Add cationic agent 2,3-epoxypropyltrimethylammonium chloride to the pretreated sugarcane and react in an air shaker. After the reaction, wash to neutrality and freeze-dry to obtain cationized sugarcane.
[0015] (3) Reduction of silver nanoparticles: The cationized sugar cane was immersed in a silver nitrate solution, placed in a vacuum drying oven to fully immerse the cationized sugar cane, and then placed in an oil bath for reaction. After the reaction was completed, the solution was washed and freeze-dried to obtain a cationized sugar cane-loaded nanosilver composite material.
[0016] As a preferred technical solution, in step (1), the mass ratio of the desugared sugarcane to the low eutectic solvent is 1:10 to 60.
[0017] As a preferred technical solution, in step (1), the molar ratio of tetraethylammonium hydroxide to 1,3-dimethylurea is 1:2-3; and the concentration of tetraethylammonium hydroxide is 30-35 wt%.
[0018] As a preferred technical solution, in step (2), the mass ratio of the desugared sugarcane to 2,3-epoxypropyltrimethylammonium chloride is 1:5-20; and the concentration of the 2,3-epoxypropyltrimethylammonium chloride is 80-85wt%.
[0019] As a preferred technical solution, in step (2), the reaction temperature is 20-25°C, the reaction time is 6-10 hours, and the freeze-drying time is 20-24 hours.
[0020] In step (2) of the present invention, the reaction formula for the reaction between the chemical components in the pretreated sugarcane and the cationic agent 2,3-epoxypropyltrimethylammonium chloride is:
[0021]
[0022] Wherein, R is cellulose, hemicellulose or lignin.
[0023] As a preferred technical solution, in step (3), the plastomeric ratio of the cationized sugarcane to the silver nitrate solution is 1 g:100-500 mL; and the concentration of the silver nitrate solution is 0.002-0.02 mol / L.
[0024] As a preferred technical solution, in step (3), the reaction temperature is 80-90°C, the reaction time is 6-10 hours, and the freeze-drying time is 24-34 hours.
[0025] An application of the cationic sugarcane-loaded nanosilver composite material as described above in the adsorption-catalytic removal of Congo red and methyl orange from dye wastewater.
[0026] Reaction principle of the present invention:
[0027] (1) During the pretreatment of sugarcane, tetraethylammonium hydroxide has a strong alkalinity and synthesizes a low eutectic solvent with 1,3-dimethylurea at room temperature. Tetraethylammonium hydroxide and 1,3-dimethylurea act synergistically as hydrogen bond donors and hydrogen bond acceptors, respectively, mainly acting on the sugarcane cell wall and fibrillating it, weakening the hydrogen bond interaction between lignin components. After treatment with an alkaline low eutectic solvent, the hydrogen bond force between cellulose, hemicellulose and lignin is weakened, and the hydroxyl groups are broken. In addition, the low eutectic solvent has a good swelling ability, deconstructing the natural porous matrix of sugarcane, causing the fibers to swell, loosening the cell wall structure, forming loose and porous gaps, increasing the reaction area, and exposing more reducing groups such as carbonyl, aldehyde and phenolic hydroxyl groups of lignin, which are used to reduce and fix silver nanoparticles and increase reaction sites.
[0028] (2) In the process of sugarcane modification, 2,3-epoxypropyltrimethylammonium chloride is a cationic agent. Under alkaline conditions, a ring-opening reaction occurs, and quaternary ammonium functional groups are introduced to functionalize cellulose. As shown in the above reaction formula, the pretreated sugarcane undergoes a ring-opening reaction with the cationic agent 2,3-epoxypropyltrimethylammonium chloride, and is grafted with the hydroxyl groups in the chemical components of the sugarcane, so that the positively charged quaternary ammonium groups are successfully loaded on the sugarcane, and the surface charge of the sugarcane changes from negative to positive, enhancing the electrostatic attraction of the composite material to anionic dyes such as Congo red and methyl orange, and enhancing the adsorption performance. At the same time, the cationic agent controls the excessive growth of silver nanoparticles on the active groups of lignin, inhibits the agglomeration effect of silver due to the nano size, and makes the composite material have better adsorption performance.
[0029] (3) In the reduction process of silver nanoparticles, cationic sugarcane is used as a carrier, and the reducing property of the lignin component in the sugarcane is utilized to directly reduce the silver ions into silver nanoparticles and fix them on the surface of the carrier, thereby synthesizing a cationic sugarcane-loaded nanosilver composite material.
[0030] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0031] 1. The present invention uses tetraethylammonium hydroxide and 1,3-dimethylurea to synthesize a green and safe low eutectic solvent to pretreat sugarcane, then adds a cationic agent 2,3-epoxypropyltrimethylammonium chloride for cation modification, uses the obtained cationized sugarcane as a carrier, utilizes the reducibility of the lignin component in the sugarcane, reduces silver ions into silver nanoparticles and fixes them on the surface of the carrier, and obtains a cationized sugarcane-loaded nanosilver composite material. The material synthesized by the present invention can effectively improve the absorption of visible light, enhance light shielding performance, have good adsorption performance and catalytic performance, and can effectively adsorb and catalytically remove Congo red and methyl orange in dye wastewater.
[0032] 2. In the present invention, when pre-treating sugarcane, a low eutectic solvent is synthesized from hydrogen bond donor tetraethylammonium hydroxide and hydrogen bond acceptor 1,3-dimethylurea, which mainly acts on the sugarcane cell wall and microfibrillates it, dissociates the cellulose chemical components without destroying the cell structure, and exposes more reducing groups such as carbonyl, aldehyde and phenolic hydroxyl groups of lignin, deconstructs the natural porous matrix of sugarcane, causes expansion between fibers, loosens the cell wall structure, forms loose and porous gaps, increases the reaction area, improves the adsorption capacity, and subsequently reduces and fixes the silver nanoparticles to increase the reaction sites. The process is simple to operate and saves energy.
[0033] 3. In the cationization process of the present invention, the sugarcane treated with the low eutectic solvent undergoes a ring-opening reaction with the cationic agent 2,3-epoxypropyltrimethylammonium chloride, and is grafted with the hydroxyl groups in the chemical components of the sugarcane, so that the positively charged quaternary ammonium salt groups are successfully loaded on the sugarcane, and anionic dyes are adsorbed through electrostatic interactions to form an adsorption-catalytic synergistic effect. At the same time, the cationic agent controls the excessive growth of silver nanoparticles on the active groups of lignin, inhibits the agglomeration effect of silver due to its nano size, and makes the composite material have better adsorption performance.
[0034] 4. In the reduction process of silver nanoparticles, the present invention uses cationized sugarcane as a carrier, utilizes the reducing property of cationized sugarcane, directly reduces silver ions into silver nanoparticles and fixes them on the surface of the carrier, and the cationized sugarcane loads the nanosilver composite material. This process does not require the addition of an additional reducing agent, and compared with the traditional method of reducing silver nanoparticles, the reaction conditions are more environmentally friendly.
[0035] 5. The cationized sugarcane-loaded nanosilver composite material synthesized by the present invention can effectively improve the absorption of visible light, and can effectively adsorb and catalyze the removal of Congo red and methyl orange in dye wastewater. The adsorption removal rate of Congo red is as high as 97.78%, and the catalytic degradation efficiency of methyl orange is 94.48%. It has good economic value and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the SEM image of the sugarcane after desugaring in Example 1.
[0037] Figure 2 This is a SEM image of sugarcane treated with a deep eutectic solvent in Example 1.
[0038] Figure 3 This is the SEM image of the cationized sugarcane-loaded nanosilver composite material prepared in Example 1.
[0039] Figure 4 This is a diagram showing the size measurement of silver nanoparticles in the cationized sugarcane-loaded nanosilver composite material prepared in Example 1.
[0040] Figure 5 The XRD diagrams of the cationized sugarcane-loaded nano-silver composite materials prepared in Examples 1-4 and the non-cationized sugarcane-loaded nano-silver composite materials prepared in the blank control group.
[0041] Figure 6 The zeta potential diagrams of the cationized sugar canes prepared in Examples 1-4 and the non-cationized sugar canes prepared in the blank group.
[0042] Figure 7Solid UV images of the cationized sugarcane-loaded nanosilver composite material prepared in Examples 1-4 and the non-cationized sugarcane-loaded nanosilver composite material prepared in the blank control group.
[0043] Figure 8 This is a diagram showing the adsorption effect of the cationized sugarcane-loaded nanosilver composite material prepared in Example 1-4 on Congo red.
[0044] Fig. 9 This is a diagram showing the catalytic removal effect of methyl orange by the cationic sugarcane-loaded nanosilver composite material prepared in Example 4. DETAILED DESCRIPTION
[0045] The present invention is further described in detail below by way of examples. These examples are only used to illustrate the present invention and do not limit the protection scope of the present invention.
[0046] Example 1
[0047] Preparation of cationized sugarcane loaded nanosilver composite materials:
[0048] (1) Pretreatment of sugarcane: peel the sugarcane and cut it into discs with a diameter of 10 to 20 mm and a width of 4 to 6 mm. Place it in 500 mL of deionized water and heat it at 80°C. Change the water every 12 hours. After 24 hours, remove the sucrose component in the sugarcane cells and freeze-dry it for 24 hours. Then take 0.2 g of the sugarcane after sugar removal, add 0.02 mol of tetraethylammonium hydroxide (8.414 g) and 0.04 mol of 1,3-dimethylurea (3.524 g) for pretreatment, and mix well to obtain pretreated sugarcane;
[0049] (2) Cationic modification of sugarcane: 1.0 g of cationic agent 2,3-epoxypropyltrimethylammonium chloride was prepared into a solution with a mass fraction of 85% with deionized water, and added to the pretreated sugarcane mixture for cationic modification. The mixture was reacted at a temperature of 25°C and a speed of 180 rpm under mechanical stirring for 8 h. After the reaction, 500 mL of deionized water was added to terminate the reaction. The reacted sugarcane mixture was separated by vacuum filtration, and the reacted sugarcane solid was collected and added with deionized water. The washing solution was repeatedly washed until it was neutral, and freeze-dried for 24 h to obtain cationized sugarcane.
[0050] (3) Reduction of silver nanoparticles: 0.1 g of cationized sugarcane was placed in 50 mL of 20 mM silver nitrate solution and placed in a vacuum drying oven under vacuum conditions for 1 h to allow the sugarcane to be fully immersed. The sugarcane was then placed in an oil bath at 80 °C for 8 h. The color of the sugarcane gradually turned into black-brown, indicating that the silver nanoparticles were successfully reduced. After the reaction was completed, the sample was washed with a large amount of deionized water and freeze-dried for 24 h to obtain a cationized sugarcane-loaded nanosilver composite material.
[0051] Example 2
[0052] (1) Pretreatment of sugarcane: peel the sugarcane and cut it into discs with a diameter of 10 to 20 mm and a width of 4 to 6 mm. Place it in 500 mL of deionized water and heat it at 80°C. Change the water every 12 hours. After 24 hours, remove the sucrose component in the sugarcane cells and freeze-dry it for 24 hours. Then take 0.2 g of the sugarcane after sugar removal, add 0.02 mol of tetraethylammonium hydroxide (8.414 g) and 0.04 mol of 1,3-dimethylurea (3.524 g) for pretreatment, and mix well to obtain pretreated sugarcane;
[0053] (2) Cationic modification of sugarcane: 2.0 g of cationic agent 2,3-epoxypropyltrimethylammonium chloride was prepared into a solution with a mass fraction of 85% with deionized water, and added to the pretreated sugarcane mixture for cationic modification. The mixture was reacted at a temperature of 25°C and a speed of 180 rpm for 8 h. After the reaction, 500 mL of deionized water was added to terminate the reaction. The reacted sugarcane mixture was separated by vacuum filtration, and the reacted sugarcane solid was collected and added with deionized water. The washings were repeatedly washed until the washings were neutral, and freeze-dried for 24 h to obtain cationized sugarcane.
[0054] (3) Reduction of silver nanoparticles: 0.1 g of cationized sugarcane was placed in 50 mL of 20 mM silver nitrate solution and placed in a vacuum drying oven under vacuum conditions for 1 h to allow the sugarcane to be fully immersed. The sugarcane was then placed in an oil bath at 80 °C for 8 h. The color of the sugarcane gradually turned into black-brown, indicating that the silver nanoparticles were successfully reduced. After the reaction was completed, the sample was washed with a large amount of deionized water and freeze-dried for 24 h to obtain a cationized sugarcane-loaded nanosilver composite material.
[0055] Example 3
[0056] (1) Pretreatment of sugarcane: peel the sugarcane and cut it into discs with a diameter of 10 to 20 mm and a width of 4 to 6 mm. Place it in 500 mL of deionized water and heat it at 80°C. Change the water every 12 hours. After 24 hours, remove the sucrose component in the sugarcane cells and freeze-dry it for 24 hours. Then take 0.2 g of the sugarcane after sugar removal, add 0.02 mol of tetraethylammonium hydroxide (8.414 g) and 0.04 mol of 1,3-dimethylurea (3.524 g) for pretreatment, and mix well to obtain pretreated sugarcane;
[0057] (2) Cationic modification of sugarcane: 3.0 g of cationic agent 2,3-epoxypropyltrimethylammonium chloride was prepared into a solution with a mass fraction of 85% with deionized water, and added to the pretreated sugarcane mixture for cationic modification. The mixture was reacted at a temperature of 25°C and a speed of 180 rpm for 8 h. After the reaction, 500 mL of deionized water was added to terminate the reaction. The reacted sugarcane mixture was separated by vacuum filtration, and the reacted sugarcane solid was collected and added with deionized water. The washing solution was repeatedly washed until it was neutral, and freeze-dried for 24 h to obtain cationized sugarcane.
[0058] (3) Reduction of silver nanoparticles: 0.1 g of cationized sugarcane was placed in 50 mL of 20 mM silver nitrate solution and placed in a vacuum drying oven under vacuum conditions for 1 h to allow the sugarcane to be fully immersed. The sugarcane was then placed in an oil bath at 80 °C for 8 h. The color of the sugarcane gradually turned into black-brown, indicating that the silver nanoparticles were successfully reduced. After the reaction was completed, the sample was washed with a large amount of deionized water and freeze-dried for 24 h to obtain a cationized sugarcane-loaded nanosilver composite material.
[0059] Example 4
[0060] (1) Pretreatment of sugarcane: peel the sugarcane and cut it into discs with a diameter of 10 to 20 mm and a width of 4 to 6 mm. Place it in 500 mL of deionized water and heat it at 80°C. Change the water every 12 hours. After 24 hours, remove the sucrose component in the sugarcane cells and freeze-dry it for 24 hours. Then take 0.2 g of the sugarcane after sugar removal, add 0.02 mol of tetraethylammonium hydroxide (8.414 g) and 0.04 mol of 1,3-dimethylurea (3.524 g) for pretreatment, and mix well to obtain pretreated sugarcane;
[0061] (2) Cationic modification of sugarcane: 4.0 g of cationic agent 2,3-epoxypropyltrimethylammonium chloride was prepared into a solution with a mass fraction of 85% with deionized water, and added to the pretreated sugarcane mixture for cationic modification. The mixture was reacted for 8 h under mechanical stirring conditions of 25 °C and 180 rpm. After the reaction, 500 mL of deionized water was added to terminate the reaction. The reacted sugarcane mixture was separated by vacuum filtration, and the reacted sugarcane solid was collected and added with deionized water. The solution was repeatedly washed until the washing solution was neutral, and freeze-dried for 24 h to obtain cationized sugarcane.
[0062] (3) Reduction of silver nanoparticles: 0.1 g of cationized sugarcane was placed in 50 mL of 20 mM silver nitrate solution and placed in a vacuum drying oven under vacuum conditions for 1 h to allow the sugarcane to be fully immersed. The sugarcane was then placed in an oil bath at 80 °C for 8 h. The color of the sugarcane gradually turned into black-brown, indicating that the silver nanoparticles were successfully reduced. After the reaction was completed, the sample was washed with a large amount of deionized water and freeze-dried for 24 h to obtain a cationized sugarcane-loaded nanosilver composite material.
[0063] Blank control group
[0064] (1) Pretreatment of sugarcane: peel the sugarcane and cut it into discs with a diameter of 10 to 20 mm and a width of 4 to 6 mm. Place it in 500 mL of deionized water and heat it at 80°C. Change the water every 12 hours. After 24 hours, remove the sucrose component in the sugarcane cells and freeze-dry it for 24 hours. Then take 0.2 g of the sugarcane after sugar removal, add 0.02 mol of tetraethylammonium hydroxide (8.414 g) and 0.04 mol of 1,3-dimethylurea (3.524 g) for pretreatment, and mix well to obtain pretreated sugarcane;
[0065] (2) Cationic modification control group: No cationic agent 2,3-epoxypropyltrimethylammonium chloride was added to the pretreated sugarcane, and the sugarcane was directly freeze-dried for 24 h to obtain non-cationized sugarcane;
[0066] (3) Reduction of silver nanoparticles: 0.1 g of non-cationized sugarcane was placed in 50 mL of 20 mM silver nitrate solution and placed in a vacuum drying oven under vacuum conditions for 1 h to allow the sugarcane to be fully immersed. The sugarcane was then placed in an oil bath at 80 °C for 8 h. The color of the sugarcane gradually turned black-brown, indicating that the silver nanoparticles were successfully reduced. After the reaction was completed, the sample was washed with a large amount of deionized water and freeze-dried for 24 h to obtain a non-cationized sugarcane-loaded nanosilver composite material.
[0067] 1. Material Characterization and Analysis
[0068] (I) SEM analysis
[0069] The morphology of the sugarcane after desugaring, the sugarcane treated with a deep eutectic solvent, the cationized sugarcane loaded with nanosilver composite material and the size measurement of the silver nanoparticles in Example 1 were characterized by field emission scanning electron microscopy (SEM). The characterization results are shown in FIG. Figure 1-4 As shown, Figure 1 This is a SEM image of sugarcane after sugar removal in Example 1. Figure 2 is a SEM image of sugarcane treated with a deep eutectic solvent in Example 1, Figure 3 This is a SEM image of the cationized sugarcane-loaded nanosilver composite material prepared in Example 1. Figure 4 This is a diagram showing the size measurement of silver nanoparticles in the cationized sugarcane-loaded nanosilver composite material prepared in Example 1.
[0070] from Figure 1 It can be seen that the internal channels of the untreated sugarcane plant cells are flat and smooth, which is suitable for serving as a reaction platform. Figure 2It can be seen that after being treated with a low eutectic solvent, microfibrillation appeared on the surface of the sugarcane, the basic morphology of the sugarcane cell wall was not destroyed, wrinkles and slight component separation appeared, and the reaction contact area was increased. This shows that in this reaction system, the low eutectic solvent has a significant effect on the treatment of sugarcane. Figure 3 It can be seen that after the cationized sugarcane is immersed in the silver nitrate solution, silver nanoparticles are obviously reduced in situ and distributed on the surface of the sugarcane and inside the channels. Figure 4 It can be seen that the size distribution of the reduced silver nanoparticles is mainly between 50 and 1000 nm.
[0071] (ii) XRD analysis
[0072] The cationized sugarcane-loaded nano-silver composite materials prepared in Examples 1-4 and the non-cationized sugarcane-loaded nano-silver composite materials prepared in the blank control group were characterized by XRD analysis. The characterization results are as follows: Figure 5 As shown, Figure 5 The XRD diagrams of the cationized sugarcane-loaded nano-silver composite materials prepared in Examples 1-4 and the non-cationized sugarcane-loaded nano-silver composite materials prepared in the blank control group. Figure 5 In the table, Blank represents the non-cationized sugarcane-loaded nanosilver composite material prepared in the blank control group, and 1:5, 1:10, 1:15, and 1:20 represent the cationized sugarcane-loaded nanosilver composite materials prepared by reacting desugared sugarcane with a cationic agent 2,3-epoxypropyltrimethylammonium chloride in different mass ratios in Examples 1-4, respectively.
[0073] Depend on Figure 5 It can be seen that the XRD crystal diffraction peaks are at 38°, 44°, 64.3°, 77.5° and 81.4°, corresponding to the characteristic peaks of (111), (200), (220), (311) and (222) of the AgJCPDS04-0783 card number, respectively, confirming the successful reduction to AgNPs inside and on the surface of sugarcane, further proving the successful reduction of silver nanoparticles.
[0074] (III) Zeta potential analysis
[0075] Zeta potential analysis was performed on the cationized sugar canes obtained in Examples 1-4 and the non-cationized sugar canes obtained in the blank control group using a Zeta potential analyzer. The analysis results are as follows: Figure 6 As shown, Figure 6 The zeta potential diagrams of the cationized sugar canes prepared in Examples 1-4 and the non-cationized sugar canes prepared in the blank group. Figure 6In the figure, blank represents the non-cationized sugar cane prepared in the blank control group, and 1:5, 1:10, 1:15, and 1:20 represent the cationized sugar cane prepared by reacting desugared sugar cane with a cationic agent 2,3-epoxypropyltrimethylammonium chloride in different mass ratios in Examples 1-4, respectively.
[0076] Depend on Figure 6 It can be seen that the surface charge of the uncationized sugarcane obtained by not adding the cationic agent 2,3-epoxypropyltrimethylammonium chloride in the blank control group is negative, while the surface charge of the cationized sugarcane obtained by adding different amounts of cationic agents in Examples 1-4 changes from negative to positive. In Example 4, when the mass ratio of sugarcane to the cationic agent is 1:20, the charge is the highest, reaching 33.2mV, which further illustrates that the cationic modification of sugarcane by 2,3-epoxypropyltrimethylammonium chloride is successful, and the quaternary ammonium salt group reacts successfully with sugarcane.
[0077] (IV) Solid UV Analysis
[0078] Solid UV test analysis was performed on the sugarcane after desugaring, the sugarcane treated with a low eutectic solvent, the sugarcane after desugaring directly loaded with silver nanoparticles, and the cationized sugarcane loaded with nanosilver composites prepared in Examples 1-4. The test results are as follows: Figure 7 shown. Figure 7 In the table, Blank represents the desugared sugarcane in the blank control group, Blank-Ag represents the desugared sugarcane in the blank control group directly loaded with silver nanoparticles, DES represents the sugarcane treated with a low eutectic solvent in the blank control group, and DES-Ag-1:5, DES-Ag-1:10, DES-Ag-1:15, and DES-Ag-1:20 represent cationized sugarcane loaded with nanosilver composite materials prepared by reacting desugared sugarcane with different mass ratios and a cationic agent 2,3-epoxypropyltrimethylammonium chloride in Examples 1-4, respectively.
[0079] Depend on Figure 7 It can be seen that the composite materials of Examples 1-4 have an absorption peak of silver nanoparticles at a wavelength of 418nm, proving that lignin has successfully reduced silver. In addition, after the sugarcane in Examples 1-4 is treated with a low eutectic solvent and then cationized, the visible light absorption is significantly improved after loading silver nanoparticles, proving that after the sugarcane is modified, the loading amount of silver nanoparticles is increased, and the composite material is enhanced to effectively absorb visible light, proving that the treated material has a certain light shielding performance.
[0080] 2. Material adsorption performance analysis
[0081] (I) Adsorption and removal of Congo red dye
[0082] Weigh 50 mg of the non-cationized sugarcane-loaded nanosilver composite material prepared in the blank control group and the cationized sugarcane-loaded nanosilver composite material prepared in Examples 1-4 respectively in a beaker, add 100 mL of a 30 mg / L Congo red solution, place on a magnetic stirrer and stir at 300 r / min to allow the sugarcane to fully contact the dye, take samples of 3 to 4 mL at regular intervals after the reaction, place in a centrifuge and centrifuge at 5000 r / min, take the supernatant and put it in a cuvette to measure the absorbance under ultraviolet spectrophotometry at a wavelength range of 400 to 600 nm, and the test results are as follows: Figure 8 As shown, Figure 8 This is a diagram showing the adsorption effect of the cationized sugarcane-loaded nanosilver composite material prepared in Example 1-4 on Congo red. Figure 8 In the figure, 0 represents the non-cationized sugarcane loaded with nanosilver composite material prepared in the blank control group, and 1:5, 1:10, 1:15, and 1:20 represent the cationized sugarcane prepared by reacting desugared sugarcane with a cationic agent 2,3-epoxypropyltrimethylammonium chloride in different mass ratios in Examples 1-4, respectively.
[0083] Depend on Figure 8 It can be seen that the adsorption performance of cationic sugarcane reducing nanoparticles was explored using 30 mg / L Congo red solution. The adsorption performance changed with the addition amount of the cationic agent.
[0084] In Example 4, when the amount of the cationic agent added was 4 g, that is, when the mass ratio of sugarcane to the cationic agent was 1:20, the adsorption removal rate of Congo red was the highest, which was 97.78%, as shown in Table 1.
[0085] Table 1 Study on the adsorption performance of materials
[0086]
[0087]
[0088] (II) Catalytic degradation of methyl orange dye
[0089] 50 mg of the sugarcane after desugaring in the blank control group, the sugarcane treated with a low eutectic solvent, and the 1:20 cationized sugarcane-loaded nanosilver composite material with the best adsorption performance obtained in Example 4 were weighed into a beaker, 40 mL of a 30 mg / L methyl orange and 50 mM sodium hydride mixture was added, and the mixture was stirred on a magnetic stirrer to allow the sugarcane to fully contact the dye. After the reaction, 3 to 4 mL of samples were taken at regular intervals, and the mixture was centrifuged at 5000 r / min in a centrifuge. The supernatant was taken and placed in a cuvette to measure the absorbance under ultraviolet spectrophotometry at a wavelength range of 300 to 600 nm. The test results are as follows: Fig. 9 As shown, Fig. 9This is a diagram showing the catalytic removal effect of methyl orange by the cationic sugarcane-loaded nanosilver composite material prepared in Example 4. Fig. 9 In the table, blank represents the sugarcane after desugaring in the blank control group, DES represents the sugarcane treated with a low eutectic solvent in the blank control group, and DES-Ag represents the cationized sugarcane-loaded nanosilver composite material prepared in Example 4.
[0090] Depend on Fig. 9 It can be seen that in the presence of the cationic sugarcane-loaded nanosilver composite material as a catalyst, sodium borohydride as a reducing agent, the degradation rate of methyl orange solution reached 94.48% within ten minutes. However, the material without silver nanoparticles has no adsorption capacity for methyl orange. Therefore, it can be proved that the cationic sugarcane-loaded nanosilver composite material has good catalytic performance.
Claims
1. A cationized sugarcane-loaded nanosilver composite material, It is characterized in that Sugarcane is pretreated with a low eutectic solvent synthesized from tetraethylammonium hydroxide and 1,3-dimethylurea, and then a cationic agent 2,3-epoxypropyltrimethylammonium chloride is added for cation modification. The cationized sugarcane obtained is used as a carrier, and the reducing property of the lignin component in the sugarcane is utilized to reduce silver ions into silver nanoparticles and fix them on the surface of the carrier, thereby obtaining a cationized sugarcane-loaded nanosilver composite material. The preparation method of the cationized sugarcane-loaded nanosilver composite material comprises the following steps: (1) Pretreatment of sugar cane: peeling and cutting sugar cane into pieces, immersing the pieces in hot water and freeze-drying the pieces to remove sugar, and uniformly mixing the sugar cane after removal of sugar with a low eutectic solvent synthesized from tetraethylammonium hydroxide and 1,3-dimethylurea to obtain pretreated sugar cane; the mass ratio of the sugar cane after removal of sugar to the low eutectic solvent is 1:10 to 60; the molar ratio of the tetraethylammonium hydroxide to 1,3-dimethylurea is 1:2 to 3; (2) Cationic modification of sugarcane: adding a cationic agent 2,3-epoxypropyltrimethylammonium chloride to the pretreated sugarcane, reacting the sugarcane in an air shaker, washing the sugarcane until the filtrate is neutral, and freeze-drying the filtrate to obtain cationic sugarcane; the mass ratio of the 2,3-epoxypropyltrimethylammonium chloride to the sugarcane after desugaring is 5 to 20:1; (3) Reduction of silver nanoparticles: immerse the cationized sugar cane in a silver nitrate solution, place it in a vacuum drying oven to allow the cationized sugar cane to fully contact the silver nitrate solution, and then place it in an oil bath for reaction. After the reaction is completed, wash it and freeze-dry it to obtain a cationized sugar cane-loaded nanosilver composite material; the mass ratio of the cationized sugar cane to the silver nitrate solution is 1 g: 100-500 mL.
2. The cationized sugarcane-loaded nanosilver composite material according to claim 1, It is characterized in that The surface potential of the cationized sugar cane is 20.7-33.2 mV, and the diameter distribution of the silver nanoparticles is 50-1000 nm.
3. A method for preparing the cationized sugarcane-loaded nanosilver composite material as claimed in claim 1 or 2, It is characterized in that The following steps are involved: (1) Pretreatment of sugar cane: peeling and cutting sugar cane into pieces, immersing the pieces in hot water and freeze-drying the pieces to remove sugar, and uniformly mixing the sugar cane after removal of sugar with a low eutectic solvent synthesized from tetraethylammonium hydroxide and 1,3-dimethylurea to obtain pretreated sugar cane; the mass ratio of the sugar cane after removal of sugar to the low eutectic solvent is 1:10 to 60; the molar ratio of the tetraethylammonium hydroxide to 1,3-dimethylurea is 1:2 to 3; (2) Cationic modification of sugarcane: adding a cationic agent 2,3-epoxypropyltrimethylammonium chloride to the pretreated sugarcane, reacting the sugarcane in an air shaker, washing the sugarcane until the filtrate is neutral, and freeze-drying the filtrate to obtain cationic sugarcane; the mass ratio of the 2,3-epoxypropyltrimethylammonium chloride to the sugarcane after desugaring is 5 to 20:1; (3) Reduction of silver nanoparticles: immerse the cationized sugar cane in a silver nitrate solution, place it in a vacuum drying oven to allow the cationized sugar cane to fully contact the silver nitrate solution, and then place it in an oil bath for reaction. After the reaction is completed, wash it and freeze-dry it to obtain a cationized sugar cane-loaded nanosilver composite material; the mass ratio of the cationized sugar cane to the silver nitrate solution is 1 g: 100-500 mL.
4. The method for preparing the cationized sugarcane-loaded nanosilver composite material according to claim 3, It is characterized in that In step (2), the reaction temperature is 20-25° C. and the reaction time is 6-10 h.
5. The method for preparing the cationized sugarcane-loaded nanosilver composite material according to claim 3, It is characterized in that In step (3), the reaction temperature is 80-90° C. and the reaction time is 6-10 h.
6. Use of the cationized sugarcane-supported nanosilver composite material as claimed in claim 1 or 2 in the adsorption-catalytic removal of Congo red and methyl orange from dye wastewater.
Citation Information
Patent Citations
Method for quickly and efficiently deconstructing lignocellulose by using alkaline eutectic solvent
CN115160591A
Method for preparing silver / carbon nano composite body
CN101480604A
Preparation method of carboxylmethyl-CHTAC (3-chloro-2-hydroxypropyl trimethyl ammonium chloride) quaternary ammonium bagasse xylan used for drug carrier
CN104610461A
Nano-composite and preparation method and application thereof