A coal tar steam reforming hydrogen production catalyst and preparation method thereof

By developing defect sites on Al2O3 and adding CaO, a Ni-Ca-Al catalyst was prepared, which solved the problems of low efficiency and high cost of existing catalysts, achieved high-efficiency hydrogen production and low CO2 yield, and was suitable for industrial applications.

CN116328772BActive Publication Date: 2024-10-29YUNNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310312126.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-29
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Existing catalysts have low efficiency and high cost in the coal tar steam reforming process, making it difficult to effectively remove tar, and too many hydroxyl groups in the traditional Al2O3 carrier limit the application of the catalyst.

Method used

Using Ni-Ca-Al catalyst, by developing defect sites on Al2O3 and adding CaO, combined with nickel nitrate and citric acid, the activated Al2O3 is prepared as a carrier to improve the activity and stability of the catalyst.

Benefits of technology

It achieves high catalytic activity and high H2 selectivity, significantly reduces CO2 production rate, has a simple process and low cost, and is suitable for industrial-scale production. The catalyst maintains high hydrogen production rate during at least 8 reuses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116328772B_ABST
    Figure CN116328772B_ABST
Patent Text Reader

Abstract

The present invention provides a coal tar steam reforming hydrogen production catalyst and a preparation method thereof, belonging to the field of catalyst technology. In the method described in the present invention, Al2O3 is calcined in a 700-900°C tubular furnace, placed in a 1-3 mol / L nitric acid solution, stirred at room temperature for 0-2h, and washed with deionized water until neutral, and the obtained Al2O3 is dried and calcined in a nitrogen atmosphere at 700-900°C to obtain activated Al2O3; a precursor of calcium is calcined at 800-900°C using a muffle furnace to obtain CaO; CaO and activated Al2O3 are mixed with nickel nitrate and citric acid solution, fully stirred and mixed, and then heated in an 80°C water bath until the solvent is completely evaporated, dried overnight at 105°C, and then calcined in a nitrogen atmosphere at 700-900°C for 2h to obtain a Ni‑Ca‑Al catalyst. The catalyst preparation process provided by the present invention is simple, low in cost, and easy to mass produce, and the prepared catalyst has a high H2 yield and a low CO2 yield for coal tar steam reforming.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, in particular to a coal tar steam reforming hydrogen production catalyst and a preparation method thereof. Background Art

[0002] Gasification is an attractive technology for achieving energy utilization of coal and biomass due to its wide applicability and environmental friendliness compared to landfill and incineration. However, tar is produced along with the gasification products, and the viscous mixture mainly contains heavy hydrocarbons and aromatic compounds, which can lead to reduced efficiency and downstream blockage. In order to achieve the elimination of tar, various methods such as physical separation, thermal cracking and steam catalytic reforming have been proposed. Among them, steam catalytic reforming has attracted widespread attention due to its ability to efficiently convert tar into useful hydrogen-rich syngas.

[0003] Obviously, the key factor of steam catalytic reforming is the catalyst, and the core is the catalytic reforming step. This process uses the catalyst to deeply convert the gas, liquid and solid phases in the reaction process, thereby improving the gas homogeneity and oil quality. Therefore, the introduction of the catalyst is the key to promoting the production of H2. High-quality catalysts should have the following characteristics: (1) active phase or active phase components; (2) catalyst carrier; (3) additives to improve activity and stability. In steam gasification, the preparation of catalysts mainly considers: (1) high catalytic activity; (2) high H2 selectivity; (3) good stability, recyclable or easy to regenerate, and can be reused; (4) easy to prepare and low cost.

[0004] The active components of noble metal catalysts are precious metals such as platinum, palladium, and rhodium. They have high tar cracking activity and inhibitory effects on carbon deposition, which have been widely studied. However, the limited availability and high cost of noble metal catalysts greatly limit their industrial application potential in tar removal. In contrast, nickel-based catalysts have the advantages of low cost, wide applicability, and excellent CC / CH bond catalytic cleavage and dehydrogenation ability, which makes nickel-based catalysts widely used. Usually, nickel particles need to be loaded on a stable support (Al2O3, SiO2, TiO2, ZrO2), which can reduce nickel agglomeration and promote the uniform distribution of nickel species. Al2O3 is often used as a catalyst support due to its high specific surface area, high porosity and low price. However, traditional Al2O3 contains too many hydroxyl groups, which cannot effectively provide defect sites for the anchoring of Ni catalysts, limiting the commercial application of catalysts. Therefore, it is necessary to develop customized defect sites on Al2O3 through a hydroxyl exposure strategy. In addition, CaO is often used as a catalyst promoter, which can promote the dispersion of the catalyst and significantly improve the catalyst's anti-carbon deposition ability. To this end, the present invention develops a Ni-Ca-Al catalyst for preparing hydrogen by steam reforming of coal tar. Summary of the invention

[0005] The purpose of the present invention is to provide a coal tar steam reforming hydrogen production catalyst and a preparation method thereof, so as to realize the full energy conversion of coal tar; the reforming catalyst of the present invention has high catalytic activity and high H2 selectivity, and can significantly reduce the CO2 yield; the manufacturing method of the present invention has a simple process, low price, and is easy to be mass-produced in industrial applications.

[0006] The present invention is implemented by the following technical solution.

[0007] A coal tar steam reforming hydrogen production catalyst, the catalyst of the invention is a Ni-Ca-Al catalyst.

[0008] The preparation method of the catalyst of the present invention comprises the following steps: calcining Al2O3 in a tube furnace, placing in a nitric acid solution, stirring at room temperature, washing with deionized water until neutral, drying the obtained Al2O3, and calcining in a nitrogen atmosphere to obtain activated Al2O3;

[0009] CaO and activated Al2O3 are mixed with nickel nitrate and citric acid solution, stirred and mixed evenly, then heated in a water bath until the solvent is completely evaporated, dried overnight, and then calcined in a nitrogen atmosphere to obtain a Ni-Ca-Al catalyst.

[0010] Furthermore, the Al2O3 of the present invention is calcined in a tube furnace, placed in a nitric acid solution, stirred at room temperature, and washed with deionized water until neutral, and the obtained Al2O3 is dried and calcined in a nitrogen atmosphere to obtain activated Al2O3;

[0011] CaO is obtained by calcining the calcium precursor in a muffle furnace;

[0012] CaO and activated Al2O3 are mixed with nickel nitrate and citric acid solution, stirred and mixed evenly, then heated in a water bath until the solvent is completely evaporated, dried overnight, and then calcined in a nitrogen atmosphere to obtain a Ni-Ca-Al catalyst.

[0013] Further, the present invention comprises the following steps:

[0014] (1) Thermal activation of Al2O3: calcining Al2O3 in a tube furnace at 700-900°C for 1-3h;

[0015] (2) Chemical activation of Al2O3: 30-50 g / L of the Al2O3 obtained in step (1) is placed in a 1-3 mol / L nitric acid solution, stirred at room temperature for 0-2 h, and washed with deionized water until neutral. The obtained Al2O3 is dried and calcined in a nitrogen atmosphere at 700-900°C to obtain activated Al2O3;

[0016] (3) calcining the calcium precursor in a muffle furnace at 800-900°C to obtain CaO;

[0017] (4) Loading of active components: nickel nitrate and citric acid are mixed and dissolved in deionized water to prepare a solution, and then the activated Al2O3 obtained in step (2) and the CaO obtained in step (3) are added;

[0018] The nickel nitrate contains 2-9% of Al2O3 by weight of elemental Ni, 1-3% of Ca by weight of Al2O3, and 0.1-0.3 g of citric acid. The mixture is stirred and mixed evenly, and then heated in a water bath at 80°C until the solvent is completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 700-900°C for 2 hours to obtain a Ni-Ca-Al catalyst.

[0019] Further, the present invention comprises the following steps:

[0020] (1) Thermal activation of Al2O3: Al2O3 was calcined in a tube furnace at 850°C for 1 h;

[0021] (2) Chemical activation of Al2O3: 40 g / L of the Al2O3 obtained in step (1) was placed in a 2 mol / L nitric acid solution, stirred at room temperature for 1.5 h, and washed with deionized water until neutral. The obtained Al2O3 was dried and calcined in a nitrogen atmosphere at 850°C to obtain activated Al2O3;

[0022] (3) calcining calcium acetate at 900°C in a muffle furnace to obtain CaO;

[0023] (4) Loading of active components: nickel nitrate and citric acid are mixed and dissolved in deionized water to prepare a solution, and then the activated Al2O3 obtained in step (2) and the CaO obtained in step (3) are added, wherein the proportion of elemental Ni in the nickel nitrate to Al2O3 is 7%, the proportion of Ca in Al2O3 is 2%, and the amount of citric acid is 0.3 g. The mixture is stirred and mixed thoroughly, and then heated in a water bath at 80°C until the solvent is completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 850°C for 2 hours to obtain a Ni-Ca-Al catalyst.

[0024] Further, the present invention comprises the following steps:

[0025] (1) Thermal activation of Al2O3: Al2O3 was calcined in a tube furnace at 850°C for 1 h;

[0026] (2) Chemical activation of Al2O3: 40 g / L of the Al2O3 obtained in step (1) was placed in a 2 mol / L nitric acid solution, stirred at room temperature for 1.5 h, and washed with deionized water until neutral. The obtained Al2O3 was dried and calcined in a nitrogen atmosphere at 850°C to obtain activated Al2O3;

[0027] (3) calcining calcium acetate at 900°C in a muffle furnace to obtain CaO;

[0028] (4) Loading of active components: nickel nitrate and citric acid are mixed and dissolved in deionized water to prepare a solution, and then the activated Al2O3 obtained in step (2) and the CaO obtained in step (3) are added, wherein the proportion of elemental Ni in the nickel nitrate to Al2O3 is 7%, the proportion of Ca in Al2O3 is 1%, and the amount of citric acid is 0.3 g. The mixture is stirred and mixed thoroughly, and then heated in a water bath at 80°C until the solvent is completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 850°C for 2 hours to obtain a Ni-Ca-Al catalyst.

[0029] Further, the present invention comprises the following steps:

[0030] (1) Thermal activation of Al2O3: Al2O3 was calcined in a tube furnace at 850°C for 1 h;

[0031] (2) Chemical activation of Al2O3: 40 g / L of the Al2O3 obtained in step (1) was placed in a 2 mol / L nitric acid solution, stirred at room temperature for 1.5 h, and washed with deionized water until neutral. The obtained Al2O3 was dried and calcined in a nitrogen atmosphere at 850°C to obtain activated Al2O3;

[0032] (3) Loading of active components: nickel nitrate and citric acid are mixed and dissolved in deionized water to prepare a solution, wherein the proportion of elemental Ni to Al2O3 in the nickel nitrate is 7% and the proportion of citric acid is 0.3 g. The mixture is stirred thoroughly to be uniform, and then heated in a water bath at 80°C until the solvent is completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 850°C for 2 hours to obtain a Ni-Ca-Al catalyst.

[0033] Furthermore, the particle size of Al2O3 in the present invention is 60-80 mesh; the heating rate of the tubular furnace is 10-40°C / min; and the rate of the nitrogen atmosphere is 40-60mL / min.

[0034] Furthermore, the heating rate of the muffle furnace of the present invention is 10-20° C. / min; the calcium precursor is selected from at least one of calcium acetate, calcium carbonate, calcium nitrate and calcium chloride.

[0035] Furthermore, the precursor of calcium in the present invention is calcium acetate.

[0036] The invention has the beneficial effects that the catalyst for coal tar steam reforming reaction provided by the invention is prepared by using Al2O3, a calcium precursor, nickel nitrate and citric acid as main raw materials, and in the preparation process, nickel nitrate, citric acid, CaO and activated Al2O3 are mixed in deionized water in a certain proportion, and then dried and calcined after being fully stirred to obtain a Ni-Ca-Al catalyst. The catalyst has the characteristics of simple preparation process, low price, easy large-scale production, etc.

[0037] The catalyst for coal tar steam reforming reaction provided by the present invention uses NiO as an active component and Al2O3 after chemical activation as a carrier. Since the activated Al2O3 contains abundant oxygen vacancies, active sites are provided for the anchoring of NiO, and the synergistic effect of NiO and the Al2O3 carrier is increased. In addition, the addition of Ca can further promote the formation of oxygen vacancies, improve the dispersibility of NiO, and significantly improve the activity and stability of the catalyst. The catalyst does not need to be treated in any way and can still maintain a high hydrogen yield in at least 8 repeated uses.

[0038] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a flow chart of the Ni-Ca-Al catalyst prepared in the present invention.

[0040] Figure 2 LT-ERP diagram of the effects of thermal activation and chemical activation of Al2O3 in the present invention.

[0041] Figure 3 This is the XRD pattern of the Ni-Ca-Al catalyst prepared in Example 1 of the present invention.

[0042] Figure 4 The stability of the coal tar steam reforming performance of the Ni-Ca-Al catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0043] In order to enable those skilled in the art to better understand the present invention, the present invention is further described in detail below in conjunction with specific embodiments and comparative examples, but the protection scope of the present invention is not limited to the contents described.

[0044] Embodiment 1:

[0045] Preparation of the catalyst in this example:

[0046] (1) Thermal activation of Al2O3: Al2O3 was calcined in a tube furnace at 850°C for 1 h;

[0047] (2) Chemical activation of Al2O3: 40 g / L of the Al2O3 obtained in step (1) was placed in a 2 mol / L nitric acid solution, stirred at room temperature for 1.5 h, and washed with deionized water until neutral. The obtained Al2O3 was dried and calcined in a nitrogen atmosphere at 850°C to obtain activated Al2O3;

[0048] (3) calcining calcium acetate at 900°C in a muffle furnace to obtain CaO;

[0049] (4) Loading of active components: nickel nitrate and citric acid are mixed and dissolved in deionized water to prepare a solution, and then the activated Al2O3 obtained in step (2) and the CaO obtained in step (3) are added, wherein the proportion of elemental Ni in the nickel nitrate to Al2O3 is 7%, the proportion of Ca in Al2O3 is 2%, and the amount of citric acid is 0.3 g. The mixture is stirred and mixed thoroughly, and then heated in a water bath at 80°C until the solvent is completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 850°C for 2 h to obtain the catalyst of this embodiment.

[0050] The experimental conditions for coal tar steam reforming in this example are:

[0051] Weigh 6g of the prepared catalyst and place it in the reforming section (the second section). Select medium and low temperature coal tar from a coal chemical enterprise in Yunnan Province as the raw material and place it in the pyrolysis section (the first section). Then introduce N2 (50mL / min) to purge for 15min to remove the impurity gas in the reaction tube. Then heat the reforming section to 800℃ at a heating rate of 30℃ / min. After the temperature stabilizes, start heating the pyrolysis section to 800℃ at a heating rate of 20℃ / min. When the temperature reaches 110℃, use a continuous injection pump to inject water at a rate of 0.2mL / min. The pyrolysis section is kept warm for 2h and then the reaction is stopped. The gas products are analyzed by gas chromatography.

[0052] The coal tar steam reforming gas product yield (mL / g) is determined as:

[0053]

[0054] Y i ——Production rate of each gas (unit: mL / g);

[0055] Xi——Volume percentage of each gas measured by GC;

[0056] V total ——Volume of collected gas (mL);

[0057] m——mass of coal tar (g).

[0058] The tar conversion rate is determined as (Xc ):

[0059]

[0060] C out ——Total carbon content of the product;

[0061] C in ——Carbon content of tar.

[0062] The performance of the catalyst in this example:

[0063] The coal tar steam reforming catalyst prepared according to the method of this embodiment has a hydrogen yield of 3421.44 mL / g for coal tar.

[0064] Embodiment 2:

[0065] Preparation of the catalyst in this example:

[0066] (1) Thermal activation of Al2O3: Al2O3 was calcined in a tube furnace at 850°C for 1 h;

[0067] (2) Chemical activation of Al2O3: 40 g / L of the Al2O3 obtained in step (1) was placed in a 2 mol / L nitric acid solution, stirred at room temperature for 1.5 h, and washed with deionized water until neutral. The obtained Al2O3 was dried and calcined in a nitrogen atmosphere at 850°C to obtain activated Al2O3;

[0068] (3) calcining calcium acetate at 900°C in a muffle furnace to obtain CaO;

[0069] (4) Loading of active components: nickel nitrate and citric acid are mixed and dissolved in deionized water to prepare a solution, and then the activated Al2O3 obtained in step (2) and the CaO obtained in step (3) are added, wherein the proportion of elemental Ni in the nickel nitrate to Al2O3 is 7%, the proportion of Ca in Al2O3 is 1%, and the amount of citric acid is 0.3 g. The mixture is stirred and mixed thoroughly, and then heated in a water bath at 80°C until the solvent is completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 850°C for 2 h to obtain the catalyst of this embodiment.

[0070] The experimental conditions for coal tar steam reforming in this example were the same as those in Example 1 for catalyst evaluation.

[0071] The performance of the catalyst in this example:

[0072] The coal tar steam reforming catalyst prepared according to the method of this embodiment has a hydrogen yield of 2945.44 mL / g for coal tar.

[0073] Embodiment 3:

[0074] Preparation of the catalyst in this example:

[0075] (1) Thermal activation of Al2O3: Al2O3 was calcined in a tube furnace at 850°C for 1 h;

[0076] (2) Chemical activation of Al2O3: 40 g / L of the Al2O3 obtained in step (1) was placed in a 2 mol / L nitric acid solution, stirred at room temperature for 1.5 h, and washed with deionized water until neutral. The obtained Al2O3 was dried and calcined in a nitrogen atmosphere at 850°C to obtain activated Al2O3;

[0077] (3) Loading of active components: nickel nitrate and citric acid were mixed and dissolved in deionized water to prepare a solution, wherein the proportion of elemental Ni to Al2O3 in the nickel nitrate was 7% and the proportion of citric acid was 0.3 g. The mixture was stirred thoroughly to mix evenly, and then heated in a water bath at 80°C until the solvent was completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 850°C for 2 h to obtain the catalyst of this embodiment.

[0078] The experimental conditions for coal tar steam reforming in this example were the same as those in Example 1 for catalyst evaluation.

[0079] The performance of the catalyst in this example:

[0080] The coal tar steam reforming catalyst prepared according to the method of this embodiment has a hydrogen yield of 2687.85 mL / g for coal tar.

[0081] Embodiment 4:

[0082] Preparation of the carrier in this example:

[0083] (1) Thermal activation of Al2O3: Al2O3 was calcined in a tube furnace at 850°C for 1 h;

[0084] (2) Chemical activation of Al2O3: 40 g / L of the Al2O3 obtained in step (1) was placed in a 2 mol / L nitric acid solution, stirred at room temperature for 1.5 h, and washed with deionized water until neutral. The obtained Al2O3 was dried and calcined in a nitrogen atmosphere at 850°C to obtain activated Al2O3;

[0085] 6 g of Al2O3 activated in step (2) was weighed and placed in the reforming section (second section). Other experimental conditions for coal tar steam reforming were evaluated under the same conditions as in Example 1.

[0086] The performance of the carrier in this embodiment:

[0087] The hydrogen yield of coal tar by the coal tar steam reforming Al2O3 carrier prepared by the method of this embodiment is 2310.39 mL / g.

[0088] Embodiment 5:

[0089] Preparation of the catalyst in this example:

[0090] (1) Thermal activation of Al2O3: Al2O3 was calcined in a tube furnace at 850°C for 1 h;

[0091] (2) Chemical activation of Al2O3: 40 g / L of the Al2O3 obtained in step (1) was placed in a 2 mol / L nitric acid solution, stirred at room temperature for 1.5 h, and washed with deionized water until neutral. The obtained Al2O3 was dried and calcined in a nitrogen atmosphere at 850°C to obtain activated Al2O3;

[0092] (3) calcining calcium acetate at 900°C in a muffle furnace to obtain CaO;

[0093] (4) Loading of active components: nickel nitrate and citric acid are mixed and dissolved in deionized water to prepare a solution, and then the activated Al2O3 obtained in step (2) and the CaO obtained in step (3) are added, wherein the proportion of elemental Ni in the nickel nitrate to Al2O3 is 2%, the proportion of Ca in Al2O3 is 0.5%, and the amount of citric acid is 0.3 g. The mixture is stirred and mixed thoroughly, and then heated in a water bath at 80°C until the solvent is completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 850°C for 2 h to obtain the catalyst of this embodiment.

[0094] The hydrogen yield of coal tar steam reforming according to the comparative example method is 1165.40 mL / g.

[0095] Embodiment 6:

[0096] Non-catalytic reforming: Weigh medium- and low-temperature coal tar from a coal chemical enterprise in Yunnan Province as raw material and place 2g of coal tar in the pyrolysis section in a fixed bed reactor. Then introduce N2 (50mL / min) for 15min to remove impurity gases in the reaction tube. Then increase the temperature to 800℃ at 20℃ / min. When the temperature reaches 110℃, use a continuous injection pump to inject water at a rate of 0.2mL / min. After keeping warm for 2h, stop the reaction and analyze the gas products using gas chromatography.

[0097] The hydrogen yield of coal tar steam reforming according to the comparative example method is 733.14 mL / g.

[0098] The gas yield evaluation results of Examples 1-6 are shown in Table 1:

[0099] Table 1 Gas yield evaluation results of Examples 1-6

[0100]

[0101] It can be seen from the results in Table 1 that the addition of an appropriate amount of the auxiliary agent CaO helps to improve the effect of coal tar steam reforming hydrogen production. 7% Ni-2% Ca-Al (Example 1) has the best catalytic effect on coal tar steam reforming. Figure 2 It shows that compared with thermally activated Al2O3, chemically activated Al2O3 has abundant oxygen vacancies, which is conducive to the adsorption and activation of water vapor and CO2; Figure 3 This shows that the active phase in Example 1 is NiO; Figure 4 It shows that the 7% Ni-2% Ca-Al catalyst in Example 1 can maintain a high hydrogen yield in at least 8 repeated uses without any treatment; the Ni-Ca-Al catalyst prepared with activated Al2O3 as a carrier in Examples 1-6 has the advantages of high catalytic activity, good stability, simple preparation and low price. It is used for coal tar steam reforming with high H2 yield and low CO2 yield, and has broad prospects in industrial applications, providing an efficient, low-cost practical catalyst for coal tar steam reforming hydrogen production.

[0102] The above are only some specific embodiments of the present invention (since the present invention includes a numerical range, the embodiments cannot be exhaustive, and the protection scope recorded in the present invention includes the numerical range and other technical key points of the present invention). The specific content or common sense known in the scheme is not described in detail here (including but not limited to abbreviations, abbreviations, and units commonly used in the art). It should be pointed out that the above embodiments do not limit the present invention in any way. For those skilled in the art, all technical solutions obtained by equivalent substitution or equivalent transformation fall within the protection scope of the present invention. The scope of protection claimed in this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing a catalyst for producing hydrogen by steam reforming of coal tar, characterized in that: The catalyst is a Ni-Ca-Al catalyst; the preparation method comprises the steps of calcining Al2O3 in a tube furnace, placing in a nitric acid solution, stirring at room temperature, and washing with deionized water until neutral, drying the obtained Al2O3, and calcining in a nitrogen atmosphere to obtain activated Al2O3; CaO is obtained by calcining the calcium precursor in a muffle furnace; CaO and activated Al2O3 are mixed with nickel nitrate and citric acid solution, stirred and mixed thoroughly, then heated in a water bath until the solvent is completely evaporated, dried overnight, and then calcined in a nitrogen atmosphere to obtain a Ni-Ca-Al catalyst; The following steps are involved: (1) Thermal activation of Al2O3: calcine Al2O3 in a tube furnace at 700-900℃ for 1-3h; (2) Chemical activation of Al2O3: 30-50 g / L of the Al2O3 obtained in step (1) is placed in a 1-3 mol / L nitric acid solution, stirred at room temperature for 0-2 h, and washed with deionized water until neutral. The obtained Al2O3 is dried and calcined in a nitrogen atmosphere at 700-900°C to obtain activated Al2O3; (3) calcining a calcium precursor at 800-900° C. in a muffle furnace to obtain CaO; the heating rate of the muffle furnace is 10-20° C. / min; (4) Loading of active components: nickel nitrate and citric acid are mixed and dissolved in deionized water to prepare a solution, and then the activated Al2O3 obtained in step (2) and the CaO obtained in step (3) are added; The nickel nitrate contains 2-9% of Al2O3 by weight of elemental Ni, 1-3% of Ca by weight of Al2O3, and 0.1-0.3 g of citric acid. The mixture is stirred and mixed evenly, and then heated in a water bath at 80°C until the solvent is completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 700-900°C for 2 hours to obtain a Ni-Ca-Al catalyst.

2. The method for preparing a coal tar steam reforming hydrogen production catalyst according to claim 1, characterized in that: The following steps are involved: (1) Thermal activation of Al2O3: calcining Al2O3 in a tube furnace at 850℃ for 1h; (2) Chemical activation of Al2O3: 40 g / L of the Al2O3 obtained in step (1) was placed in a 2 mol / L nitric acid solution, stirred at room temperature for 1.5 h, and washed with deionized water until neutral. The obtained Al2O3 was dried and calcined in a nitrogen atmosphere at 850°C to obtain activated Al2O3; (3) Calcination of calcium acetate at 900°C in a muffle furnace to obtain CaO; (4) Loading of active components: nickel nitrate and citric acid are mixed and dissolved in deionized water to prepare a solution, and then the activated Al2O3 obtained in step (2) and CaO obtained in step (3) are added, wherein the proportion of elemental Ni in the nickel nitrate to Al2O3 is 7%, the proportion of Ca in Al2O3 is 2%, and the amount of citric acid is 0.3 g. The mixture is stirred and mixed thoroughly, and then heated in a water bath at 80°C until the solvent is completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 850°C for 2 h to obtain a Ni-Ca-Al catalyst.

3. The method for preparing a catalyst for producing hydrogen from coal tar steam reforming according to claim 1, characterized in that: The following steps are involved: (1) Thermal activation of Al2O3: calcining Al2O3 in a tube furnace at 850℃ for 1h; (2) Chemical activation of Al2O3: 40 g / L of the Al2O3 obtained in step (1) was placed in a 2 mol / L nitric acid solution, stirred at room temperature for 1.5 h, and washed with deionized water until neutral. The obtained Al2O3 was dried and calcined in a nitrogen atmosphere at 850°C to obtain activated Al2O3; (3) Calcination of calcium acetate at 900°C in a muffle furnace to obtain CaO; (4) Loading of active components: nickel nitrate and citric acid are mixed and dissolved in deionized water to prepare a solution, and then the activated Al2O3 obtained in step (2) and the CaO obtained in step (3) are added, wherein the proportion of elemental Ni in the nickel nitrate to Al2O3 is 7%, the proportion of Ca in Al2O3 is 1%, and the amount of citric acid is 0.3 g. The mixture is stirred and mixed thoroughly, and then heated in a water bath at 80°C until the solvent is completely evaporated, dried at 105°C overnight, and then calcined in a nitrogen atmosphere at 850°C for 2 h to obtain a Ni-Ca-Al catalyst.

4. The method for preparing a coal tar steam reforming hydrogen production catalyst according to claim 1, 2 or 3, characterized in that: The particle size of the Al2O3 is 60-80 mesh; the heating rate of the tubular furnace is 10-40°C / min; and the rate of the nitrogen atmosphere is 40-60mL / min.

5. The method for preparing a catalyst for producing hydrogen from coal tar steam reforming according to claim 1, 2 or 3, characterized in that: The calcium precursor is selected from at least one of calcium acetate, calcium carbonate, calcium nitrate and calcium chloride.

6. The method for preparing a catalyst for producing hydrogen from coal tar steam reforming according to claim 5, characterized in that: The calcium precursor is calcium acetate.