Titanium-containing residue oil hydrodemetallization catalyst and preparation method thereof

CN116328782BActive Publication Date: 2024-10-15PETROCHINA CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202111601988.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-24
Publication Date
2024-10-15
Estimated Expiration
2041-12-24

AI Technical Summary

Technical Problem

Existing hydrodemetallization catalysts have problems such as pore blockage, uneven impurity deposition, high cost, and failure to maximize performance when treating heavy and residual oils. Especially when using acidic peptizers and high roasting temperatures, it is difficult to prepare Bimodal pore structure carrier with high macropore ratio.

Method used

Use hydrated alumina, titanium-containing compounds, adhesives and physical pore expanders to mix, add chemical pore expanders, ammonia and low-carbon alcohol aqueous solutions, and prepare the catalyst through kneading, molding, drying and roasting to avoid the use of acidic peptizers , using ammonia and low-carbon alcohol to promote the hole expansion effect and reduce costs.

Benefits of technology

A catalyst with a bimodal pore structure is prepared, with larger pore volume and pore size, high demetalling activity, and strong metal-accommodating ability. It is suitable for the hydrogenation of inferior heavy and residual oils, and has optimized activity stability and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003433307450000091
    Figure BDA0003433307450000091
  • Figure BDA0003433307450000101
    Figure BDA0003433307450000101
Patent Text Reader

Abstract

The present invention relates to a titanium-containing residual oil hydrodemetallization catalyst and a preparation method thereof. The preparation method comprises the following steps: mixing hydrated alumina, a titanium-containing compound, a binder and a physical pore expander, then adding an aqueous solution containing a chemical pore expander, ammonia and a low-carbon alcohol, kneading, molding, drying and roasting, and then loading an active metal to obtain a catalyst; the binder is synthetic cellulose, the physical pore expander is a water-soluble organic polymer, and the chemical pore expander is a boron-containing compound. The catalyst prepared by the method provided by the present invention has a bimodal pore structure and a large pore volume and pore diameter. The prepared catalyst has high demetallization activity and strong metal tolerant capacity, and is particularly suitable for the hydroprocessing of inferior heavy and residual oils, and is particularly suitable for use as a residual oil hydrodemetallization catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrodemetallization catalysts, and in particular relates to a titanium-containing residual oil hydrodemetallization catalyst and a preparation method thereof. Background Art

[0002] At present, with the increasing deterioration and inferiority of oil resources worldwide, as well as the urgent requirements for upgrading oil quality and increasingly stringent environmental regulations, there is an urgent need to develop clean and efficient heavy oil processing technology. Hydrogenation is the most effective heavy and residual oil raw material processing technology. Through hydrogenation, most of the metal impurities and sulfur are removed, while the residual carbon value is reduced, the quality of heavy oil is improved, and further efficient and clean processing is possible. The technical combination of heavy and residual oil hydrotreatment and heavy oil catalytic cracking can not only maximize the conversion of residual oil with low utilization value and easy to cause environmental pollution, and greatly increase the yield of light oil; it can also obtain clean oil products with high added value and high quality. In a sense, the crude oil has been converted 100%, realizing the desire to squeeze out the crude oil in the oil refining process. This technical combination has become the core technology for sulfur-containing crude oil processing and refining enterprises to improve the economic benefits.

[0003] The deposition of metals such as Na, Ca, Ni, and V in heavy oil on the hydrogenation catalyst will cause permanent poisoning, which is an important factor to be considered in the heavy oil hydrogenation process. Hydrodemetallization (HDM) catalyst is one of the key technologies in the heavy oil hydroprocessing process. Its main function is to remove most of the metal impurities such as Ni and V in the raw material, protect the downstream desulfurization (HDS) and denitrification (HDN) catalysts, and have a certain desulfurization capacity. This type of catalyst needs to have not only good metal removal ability, but also a high metal impurity tolerance capacity. Since most of the metal impurities in the residual oil exist in colloids and asphaltene, which are the largest molecular weight, most complex structure, and strongest polarity in the petroleum components, the diffusion resistance is relatively large. The demetallization agent is restricted by the mass transfer and diffusion efficiency of the carrier, and is prone to pore blockage, the deposition distribution of the impurities removed is seriously uneven, and the metal tolerance capacity is limited. All of the above cause serious waste of the internal space of the catalyst, and the efficiency of the catalyst cannot be maximized. Therefore, such catalysts must have a large pore volume, pore diameter and good pore permeability to facilitate the diffusion, reaction and deposition of macromolecular substances such as asphaltene containing metal impurities in the residual oil raw material. One solution is to use a bimodal pore structure carrier. During the reaction process, macropores with a pore diameter of more than 100nm provide channels for the diffusion of macromolecular reaction substances, promoting the diffusion and deposition of impurities into the internal pores of the catalyst; while pores with a pore diameter of less than 50nm provide reaction surfaces and deposition sites for impurities. The two types of pores work synergistically, so that the catalyst has high demetallization activity and high impurity tolerance.

[0004] CN1103009A discloses a method for preparing a double-pore alumina carrier, which is prepared by mixing two aluminas or their precursors with different pore size distributions with carbon black powder, a surfactant, a peptizing agent and water, and drying and calcining. When carbon black powder is used as a pore-enlarging agent, the pore-enlarging effect is poor and the carrier strength is low. At the same time, the addition of a peptizing agent will reduce the pore volume and pore size of the carrier.

[0005] CN1120971 discloses a method for preparing a bimodal pore structure alumina carrier, wherein two or more pseudo-boehmite dry gels prepared by different raw material routes are uniformly mixed, and then peptized, molded, dried and calcined. However, this method uses an oil-ammonia column method to mold the alumina carrier, which has low production efficiency and high pollution in the production process, and is now rarely used.

[0006] CN1647857A discloses a method for preparing a macroporous alumina carrier, wherein a pseudo-boehmite composition containing an organic pore-enlarging agent is molded and calcined to obtain an alumina carrier having a bimodal pore structure. The method requires first slurrying the physical pore-enlarging agent and the pseudo-boehmite and spray drying, and the preparation process is relatively complicated.

[0007] CN105983443B discloses a method for preparing a bimodal pore structure alumina carrier, which comprises mixing an organic binder, a chemical pore expander and a physical pore expander to form and bake to obtain a macroporous bimodal pore structure alumina carrier. The pore size of the carrier prepared by this method is limited, and the macropore ratio is greatly affected by the amount of the pore expander added. It is impossible to prepare a carrier with a larger pore size and macropore ratio. The carrier baking temperature is high and the production cost is high.

[0008] In the existing alumina carrier and catalyst preparation technology, most of the time, acidic substances such as nitric acid, acetic acid, aluminum nitrate, etc. need to be added as peptizing agents when alumina is formed. The addition of acidic substances will destroy the particle structure of alumina and reduce the pore volume and pore size of the carrier. Using organic binders instead of peptizing acids for carrier forming can increase the pore volume and pore size of the carrier to a certain extent, but the effect is limited. The existing methods simply increase the macropore ratio of the carrier by adding pore expanders. When preparing bimodal pore structure carriers and catalysts with high macropore ratios, they face problems such as increased costs, difficult forming, and reduced strength. Summary of the invention

[0009] The object of the present invention is to provide a method for preparing a titanium-containing residue oil hydrodemetallization catalyst in view of the deficiencies in the prior art.

[0010] Another object of the present invention is to provide a titanium-containing residue oil hydrodemetallization catalyst.

[0011] To achieve the above-mentioned purpose, the present invention provides a method for preparing a titanium-containing residue oil hydrodemetallization catalyst, comprising the following steps: mixing hydrated alumina, a titanium-containing compound, a binder and a physical pore expander, then adding an aqueous solution containing a chemical pore expander, ammonia and a low-carbon alcohol, kneading, molding, drying and roasting, and then loading an active metal to obtain a catalyst; the binder is synthetic cellulose, the physical pore expander is a water-soluble organic polymer, and the chemical pore expander is a boron-containing compound.

[0012] In the preparation method of the titanium-containing residue oil hydrodemetallization catalyst of the present invention, the hydrated aluminum oxide is selected from one or more of gibbsite, boehmite, pseudo-boehmite and amorphous aluminum hydroxide, preferably pseudo-boehmite. They can be commercial products or prepared by any method in the prior art, such as preparing pseudo-boehmite by aluminum sulfate-sodium aluminate method.

[0013] The preparation method of the titanium-containing residue oil hydrodemetallization catalyst of the present invention, the titanium-containing compound is selected from one or more of titanic acid, metatitanic acid and titanium dioxide, the particle size is less than or equal to 1000 mesh, the titanium-containing compound is calculated as titanium dioxide, the hydrated alumina is calculated as alumina, and the amount of the titanium-containing compound added is 0.5-5% of the weight of the hydrated alumina.

[0014] The preparation method of the titanium-containing residual oil hydrodemetallization catalyst of the present invention, the water-soluble organic polymer is selected from one or more of polyethylene glycol, polyacrylamide, polyvinyl alcohol and cross-linked polyvinylpyrrolidone, the hydrated alumina is calculated as alumina, and the amount of the water-soluble organic polymer added is 1-6% of the weight of the hydrated alumina.

[0015] The preparation method of the titanium-containing residue oil hydrodemetallization catalyst of the present invention, the boron-containing compound is selected from one or more of boric acid, metaboric acid, ammonium hydrogen borate, ammonium tetraborate tetrahydrate and ammonium pentaborate tetrahydrate, the boron-containing compound is calculated as elemental boron, the hydrated alumina is calculated as alumina, and the amount of the boron-containing compound added is 0.3-2% of the weight of the hydrated alumina.

[0016] In the preparation method of the titanium-containing residue oil hydrodemetallization catalyst of the present invention, the hydrated aluminum oxide is calculated as aluminum oxide, and the added amount of ammonia is 0.05-0.5% of the weight of the hydrated aluminum oxide.

[0017] The method for preparing the titanium-containing residue oil hydrodemetallization catalyst of the present invention comprises the following steps: the low-carbon alcohol is selected from one or more of methanol, ethanol, ethylene glycol, propanol, isopropanol and glycerol; the hydrated alumina is calculated as alumina, and the amount of the low-carbon alcohol added is 0.5-5% of the weight of the hydrated alumina.

[0018] The method for preparing the titanium-containing residue oil hydrodemetallization catalyst of the present invention, the active metal includes a first active metal and / or a second active metal, the first active metal is molybdenum and / or tungsten, the second active metal is cobalt and / or nickel, and the first active metal accounts for 2-8% of the total weight of the catalyst, and the second active metal accounts for 0.4-2% of the total weight of the catalyst, calculated as oxide.

[0019] The method for preparing the titanium-containing residue oil hydrodemetallization catalyst of the present invention comprises the following steps: the synthetic cellulose is selected from one or more of methyl cellulose, ethyl cellulose, hydroxypropyl methyl cellulose and hydroxyethyl methyl cellulose; the hydrated alumina is calculated as alumina, and the amount of the synthetic cellulose added is 1-5% of the weight of the hydrated alumina.

[0020] The method for preparing the titanium-containing residue oil hydrodemetallization catalyst of the present invention is characterized in that the viscosity of the 2% aqueous solution of the synthetic cellulose is greater than or equal to 50000 mPa·s.

[0021] In the method for preparing the titanium-containing residual oil hydrodemetallization catalyst of the present invention, the particle size of the water-soluble organic polymer is 80 to 400 meshes.

[0022] In the preparation method of the titanium-containing residue oil hydrodemetallization catalyst of the present invention, the active metal is loaded by impregnation. The active metal can be prepared into a stable metal solution by any known method, such as adding a certain concentration of ammonia water to dissolve ammonium heptamolybdate and nickel nitrate under stirring conditions, or dissolving molybdenum trioxide, basic nickel carbonate and phosphoric acid together under heating and stirring conditions, to prepare a stable metal solution.

[0023] In the method for preparing the titanium-containing residue oil hydrodemetallization catalyst of the present invention, the molding process is carried out by using an oil pressure or hydraulic extruder, and the extrusion pressure is 10-30 MPa.

[0024] The method for preparing the titanium-containing residue oil hydrodemetallization catalyst of the present invention has the following characteristics: the calcination temperature is 500-1100° C. and the calcination time is 0.5-4 hours.

[0025] In the method for preparing the titanium-containing residue oil hydrodemetallization catalyst of the present invention, the carrier shape can be changed as needed, such as cylinder, three-leaf clover, four-leaf clover, butterfly and five-tooth ball, etc. During the molding process, an appropriate amount of extrusion aid (such as sesbania powder) and water can be added.

[0026] To achieve the above object, the present invention also provides a catalyst prepared by the above method for preparing the titanium-containing residue oil hydrodemetallization catalyst.

[0027] The catalyst of the present invention has a bimodal pore structure, a pore volume of 0.8-1.6 ml / g, pores with a pore diameter of 20-50 nanometers account for 30-70% of the total pore volume, pores with a pore diameter of more than 100 nanometers account for 20-50% of the total pore volume, pores with a pore diameter of less than 20 nm account for less than 30% of the total pore volume, and a BET specific surface area of ​​80-220 square meters / g.

[0028] Beneficial effects of the present invention:

[0029] Compared with the existing methods, the method provided by the present invention does not use an acidic peptizing agent during the carrier molding process, thereby reducing the damage of the acid to the structure of the hydrated alumina particles; a small amount of ammonia is added. On the one hand, ammonia can effectively promote the composite pore expansion effect of chemical pore expanders and physical pore expanders. For example, ammonia can promote the "gelation" reaction between boric acid and polyvinyl alcohol, effectively increasing the proportion of macropores larger than 100 nm in the carrier, and on the other hand, ammonia can effectively reduce the bonding strength between alumina particles and increase the pore volume and pore size of the carrier; a low-carbon alcohol component is added, and the solubility of the low-carbon alcohol in boric acid or boron-containing compounds and the affinity between the low-carbon alcohol and the physical pore expander are utilized to promote the interaction between the boron-containing chemical pore expander and the physical pore expander, reduce the boron-containing compound component from entering the alumina pore channel, thereby generating more macroporous structures and improving the pore expansion efficiency; the amount of physical pore expander added is relatively low, thereby reducing the preparation cost; the addition of titanium is beneficial to optimizing the dispersion of active metal components, regulating the interaction between active components and the carrier, inhibiting catalyst coking, and improving activity stability.

[0030] The catalyst prepared by the method provided by the present invention has a bimodal pore structure and a large pore volume and pore diameter. The prepared catalyst has high demetallization activity and strong metal tolerance, and is particularly suitable for the hydroprocessing of inferior heavy and residual oils, especially for use as a residual oil hydrodemetallization catalyst. For example, the catalyst prepared according to the method provided by the present invention has a specific surface area of ​​130 square meters / gram, a pore volume of 1.20 ml / gram, characteristic peaks at 21 nanometers and 470 nanometers, pores with a pore diameter of 20-50 nanometers account for 38.8% of the total pore volume, pores with a pore diameter of more than 100 nanometers account for 39.4% of the total pore volume, and pores with a pore diameter of less than 20 nm account for 21.8% of the total pore volume. It contains 0.9% titanium dioxide, 4.3% molybdenum oxide, and 1.5% nickel oxide. Using inferior Middle Eastern residual oil with a metal (Ni+V) content of 103 μg / g as a raw material, under the conditions of a reaction pressure of 16 MPa, a reaction temperature of 380°C, and an air velocity of 1.0 h-1, the demetallization rate reaches 82.2% after 200 hours of reaction, 71.7% after 2000 hours of reaction, and still as high as 66.5% after 4000 hours of reaction. DETAILED DESCRIPTION

[0031] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.

[0032] Example 1

[0033] Weigh 500g of macroporous pseudo-boehmite dry glue powder (dry basis content 71.5wt%) produced by Yantai Henghui Chemical Co., Ltd., add 10.73g of titanium dioxide with a particle size of 2000 mesh, 10.7g of hydroxypropyl methylcellulose with a viscosity of 150,000 mPa·s (referring to the viscosity of 2% aqueous solution), and 14.3g of polyvinyl alcohol powder with a particle size of 120 mesh, and mix them evenly; dissolve 14.3g of boric acid in 607.8g of clean water, add 5g of 20% ammonia water and 10g of ethanol, stir evenly, slowly add to the above materials, knead into a plastic body, and then extrude it into a clover shape with a diameter of 1.6mm on an oil pressure extruder, and control the extrusion pressure to 20MPa. Dry at 120℃ for 2.0 hours, then place in a high-temperature roasting furnace, and keep the temperature at 900℃ for 3 hours to obtain a carrier. Prepare (3.8gMoO 3 +0.8g NiO) / 100mL stable metal impregnation solution, the obtained support was impregnated by saturation impregnation method; the impregnated material was dried at 120°C, and kept at 500°C in a roasting furnace for 3 hours to obtain catalyst A. The catalyst properties are shown in Table 1.

[0034] Example 2

[0035] Weigh 500g of macroporous pseudo-boehmite dry glue powder (dry basis content 71.5wt%) produced by Yantai Henghui Chemical Co., Ltd., add 17.88g of titanium dioxide with a particle size of 1000 mesh, 3.6g of hydroxypropyl methylcellulose with a viscosity of 200,000 mPa·s (referring to the viscosity of 2% aqueous solution), 11.5g of polyvinyl alcohol powder with a particle size of 80 mesh and 10.0g of polyethylene glycol powder with a particle size of 120 mesh, and mix them evenly; dissolve 20.4g of ammonium tetraborate tetrahydrate in 607.8g of clean water, add 0.89g of 20% ammonia water, 10g of ethylene glycol and 7.88g of methanol, stir evenly, slowly add to the above materials, mix and knead into a plastic body, and then extrude into a clover shape with a diameter of 1.6mm on an oil pressure extruder, and control the extrusion pressure to be 10MPa. Then put it into a high-temperature roasting furnace and keep it at a constant temperature of 1100℃ for 0.5 hours to obtain a carrier. The preparation contained (1.4 g MoO 3 +1.4g Co 2 O 3) / 100mL of stable metal impregnation solution, and the obtained support was impregnated by saturation impregnation method; the impregnated material was dried at 120°C, and kept at 500°C in a roasting furnace for 3 hours to obtain catalyst B. The catalyst properties are shown in Table 1.

[0036] Example 3

[0037] Weigh 500g of macroporous pseudo-boehmite dry glue powder (dry basis content 71.5wt%) produced by Yantai Henghui Chemical Co., Ltd., add 1.79g of titanium dioxide with a particle size of 3000 mesh, 17.9g of hydroxyethyl methylcellulose with a viscosity of 100,000 mPa·s (referring to the viscosity of 2% aqueous solution), and 17.9g of polyacrylamide with a particle size of 200 mesh, and mix them evenly; dissolve 5.67g of ammonium hydrogen borate in 607.8g of clean water, add 8.94g of 20% ammonia water and 1.79g of propanol, stir evenly, slowly add to the above materials, knead into a plastic body, and then extrude it into a clover shape with a diameter of 1.6mm on an oil pressure extruder, and control the extrusion pressure to 30MPa. Then put it in a high-temperature roasting furnace and keep it at 500℃ for 4 hours to obtain a carrier. Prepare (5.5g WO 3 +1.8g MoO 3 +0.9gNiO+0.5g Co 2 O 3 ) / 100mL of a stable metal impregnation solution, and the obtained support was impregnated by a saturated impregnation method; the impregnated material was dried at 120°C, and kept at a constant temperature of 500°C in a roasting furnace for 3 hours to obtain Catalyst C. The catalyst properties are shown in Table 1.

[0038] Example 4

[0039] Weigh 500g of macroporous pseudo-boehmite dry rubber powder (dry basis content 71.5wt%) produced by Yantai Henghui Chemical Co., Ltd., add 5.19g of titanic acid with a particle size of 2000 mesh, 6.7g of hydroxypropyl methylcellulose with a viscosity of 150,000 mPa·s (referring to the viscosity of 2% aqueous solution) and 4.0g of methylcellulose with a viscosity of 100,000 mPa·s (referring to the viscosity of 2% aqueous solution), and 3.6g of cross-linked polyvinylpyrrolidone with a particle size of 160 mesh, and mix them evenly; dissolve 29.0g of metaboric acid in 607.8g of clean water, add 7.5g of 20% ammonia water and 8g of isopropanol, stir evenly, slowly add to the above materials, knead into a plastic body, and then extrude it into a clover shape with a diameter of 1.6mm on an oil pressure extruder, and control the extrusion pressure to 18MPa. Then put it in a high-temperature roasting furnace and keep it at 800℃ for 3 hours to obtain a carrier. Prepare (3.3g MoO 3+1.2g NiO) / 100mL stable metal impregnation solution, the obtained support was impregnated by saturated impregnation method; the impregnated material was dried at 120°C, and kept at 500°C in a roasting furnace for 3 hours to obtain catalyst D. The catalyst properties are shown in Table 1.

[0040] Example 5

[0041] Weigh 500g of macroporous pseudo-boehmite dry glue powder (dry basis content 71.5wt%) produced by Yantai Henghui Chemical Co., Ltd., add 8.76g of metatitanic acid with a particle size of 1500 mesh, 10.7g of ethyl cellulose with a viscosity of 150,000 mPa·s (referring to the viscosity of 2% aqueous solution), 5.7g of polyvinyl alcohol powder with a particle size of 400 mesh and 5.0g of polyacrylamide with a particle size of 80 mesh, and mix them evenly; dissolve 20.4g of boric acid and 4.7g of ammonium pentaborate tetrahydrate in 607.8g of clean water, add 6g of 20% ammonia water and 15g of glycerol, stir evenly, slowly add to the above materials, knead into a plastic body, and then extrude into a clover shape with a diameter of 1.6mm on an oil pressure extruder, and control the extrusion pressure to 20MPa. Then put it in a high-temperature roasting furnace and keep it at 950℃ for 2.5 hours to obtain a carrier. Prepare (4.7g MoO 3 +0.3g NiO) / 100mL stable metal impregnation solution, the obtained support was impregnated by saturation impregnation method; the impregnated material was dried at 120°C, and kept at 500°C in a roasting furnace for 3 hours to obtain catalyst E. The catalyst properties are shown in Table 1.

[0042] Comparative Examples 1-3 illustrate the prior art method and the bimodal pore structure alumina supports prepared by the prior art method.

[0043] Comparative Example 1

[0044] In this comparative example, the alumina carrier and catalyst were prepared according to the method described in CN1103009A.

[0045] 34.1g aluminum hydroxide dry rubber powder (alkyl aluminum hydrolysis product containing 75% aluminum oxide) and 39.3g aluminum hydroxide powder prepared by aluminum sulfate method were mixed, and then 4.7g high wear-resistant carbon black, 3.5g surfactant SA-20, 2.1g aluminum nitrate and 66ml water were added and fully rolled and mixed. The mixture was extruded into a clover shape with a diameter of 1.8mm on an extruder, dried at 120℃, and calcined at 600℃ for 4 hours to obtain a carrier. 3 +2.9g NiO) / 100mL stable metal impregnation solution, the obtained support was impregnated by saturated impregnation method; the impregnated material was dried at 120°C, and kept at 500°C in a roasting furnace for 3 hours to obtain catalyst F. The catalyst properties are shown in Table 1.

[0046] Comparative Example 2

[0047] In this comparative example, the alumina carrier and catalyst were prepared according to the method described in CN1647857A.

[0048] Aluminum hydroxide was used to react with aluminum hydroxide to prepare NaAlO with a concentration of 200 g aluminum oxide / liter. 2 Solution, add this solution and aluminum sulfate solution with a concentration of 90g aluminum oxide / liter in parallel to a 2-liter gelling tank, put 1.5 liters of water in advance in the tank, the flow rate of sodium aluminate is 1.1 liters / hour, adjust the flow rate of aluminum sulfate solution to make the gelling pH value 8, the gelling temperature is 50°C, and the slurry generated by gelling is collected in an aging tank. Sodium carbonate is added to the aging tank after collection to adjust the pH value to 10, age for 50 minutes, filter and wash to obtain a pseudo-boehmite wet cake. Take 6.5 kg of the wet cake and mix it with 20.5g of sesbania powder, add pulping, and then spray dry at an inlet temperature of 600°C and an outlet temperature of 145°C. The dried composition is extruded on an extruder, dried at 120°C, and calcined at 800°C for 3.5 hours to obtain a carrier. Prepare (10.0g MoO 3 +1.3g NiO) / 100mL stable metal impregnation solution, the obtained support was impregnated by saturation impregnation method; the impregnated material was dried at 120°C, and kept at 500°C in a roasting furnace for 3 hours to obtain catalyst G. The catalyst properties are shown in Table 1.

[0049] Comparative Example 3

[0050] In this comparative example, the alumina carrier and catalyst were prepared according to the method described in CN105983443B.

[0051] Weigh 500g of macroporous pseudo-boehmite dry rubber powder (dry basis content 71.5wt%) produced by Yantai Henghui Chemical Co., Ltd., add 10.7g of hydroxypropyl methylcellulose with a viscosity of 150,000 mPa·s (referring to the viscosity of 2% aqueous solution) and 17.9g of polyvinyl alcohol powder with a particle diameter of 90-150μm, and mix well; dissolve 14.3g of boric acid in 390g of clean water, slowly add to the above materials, knead into a plastic body, and then extrude into a clover shape with a diameter of 1.6mm on a front extrusion single-screw extruder. Dry at 120℃ for 2.0 hours, then place in a roasting furnace and keep constant temperature at 800℃ for 3 hours to obtain a carrier. Prepare (5.0gMoO 3 +1.1gNiO) / 100mL stable metal impregnation solution, the obtained support was impregnated by saturated impregnation method; the impregnated material was dried at 120°C, and kept at 500°C in a roasting furnace for 3 hours to obtain catalyst H. The catalyst properties are shown in Table 1.

[0052] Comparative Example 4

[0053] Weigh 500g of macroporous pseudo-boehmite dry rubber powder (dry basis content 71.5wt%) produced by Yantai Henghui Chemical Co., Ltd., add 10.7g of hydroxypropyl methylcellulose with a viscosity of 150,000 mPa·s (referring to the viscosity of 2% aqueous solution), and mix well; dissolve 58.8g of boric acid in 390g of clean water, slowly add to the above materials, knead into a plastic body, and then extrude into a clover shape with a diameter of 1.6mm on a front extrusion single-screw extruder. Dry at 120℃ for 2.0 hours, then place in a roasting furnace and keep constant temperature at 800℃ for 3 hours to obtain a carrier. Prepare (8.1g MoO 3 +1.7g NiO) / 100mL stable metal impregnation solution, the obtained support was impregnated by saturation impregnation method; the impregnated material was dried at 120°C, and kept at 500°C in a roasting furnace for 3 hours to obtain Catalyst I. The catalyst properties are shown in Table 1.

[0054] Comparative Example 5

[0055] Weigh 500g of macroporous pseudo-boehmite dry rubber powder (dry basis content 71.5wt%) produced by Yantai Henghui Chemical Co., Ltd., add 10.7g of hydroxypropyl methylcellulose with a viscosity of 150,000 mPa·s (referring to the viscosity of a 2% aqueous solution) and 58.8g of polyvinyl alcohol powder with a particle diameter of 90-150μm, and mix them evenly; slowly add 390g of clean water to the above materials, knead them into a plastic body, and then extrude them into a clover shape with a diameter of 1.6mm on a front extrusion single-screw extruder. Dry at 120℃ for 2.0 hours, then place in a roasting furnace and keep it at 800℃ for 3 hours to obtain a carrier. Prepare (7.2g MoO 3 +1.5g NiO) / 100mL stable metal impregnation solution, the obtained support was impregnated by saturated impregnation method; the impregnated material was dried at 120°C, and kept at 500°C in a roasting furnace for 3 hours to obtain catalyst J. The catalyst properties are shown in Table 1.

[0056] Table 1 Physicochemical properties of catalysts

[0057]

[0058] The results in Table 1 show that, compared with the comparative example, the catalyst prepared by the method of the present invention has an obvious bimodal pore structure, and has a large pore volume, a large pore diameter, and a higher proportion of macropores above 100 nm. It can also be seen from the comparison effect of Comparative Example 3 and Example 1 that, by using the method of the present invention, the pore volume and pore diameter of the obtained carrier are larger, the proportion of macropores is higher, and the amount of pore-enlarging agent added can be effectively reduced, which is conducive to reducing production costs.

[0059] The activity stability of the catalyst in Table 1 was evaluated. The evaluation conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0060] Table 2 Catalyst evaluation conditions

[0061] Raw oil properties Middle East Residue <![CDATA[Density (20 °C) / g·cm -3 > 0.99 <![CDATA[(Ni+V),μg.g -1 ]]> 103 Process conditions Reaction temperature, °C 380 Hydrogen partial pressure, MPa 16 <![CDATA[Space velocity, h -1 > 1.0 Hydrogen / Oil Ratio 750

[0062] Table 3 Catalyst metal removal rate (HD (Ni + V))

[0063]

[0064] From the evaluation results in Table 3, it can be seen that the catalyst of the present invention has higher demetallization activity, less activity decrease after long-term operation, good stability, and high impurity tolerance of the catalyst.

[0065] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a titanium-containing residue oil hydrodemetallization catalyst, characterized in that: The method comprises the following steps: mixing hydrated alumina, a titanium-containing compound, a binder and a physical pore-enlarging agent, then adding an aqueous solution containing a chemical pore-enlarging agent, ammonia and a low-carbon alcohol, kneading, molding, drying and calcining, and then loading an active metal to obtain a catalyst; the binder is synthetic cellulose, the physical pore-enlarging agent is an organic polymer, and the chemical pore-enlarging agent is a boron-containing compound; The active metal includes a first active metal and / or a second active metal, the first active metal is molybdenum and / or tungsten, and the second active metal is cobalt and / or nickel; The organic polymer is selected from one or more of polyethylene glycol, polyacrylamide, polyvinyl alcohol and cross-linked polyvinylpyrrolidone.

2. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The hydrated aluminum oxide is selected from one or more of gibbsite, boehmite, pseudo-boehmite and amorphous aluminum hydroxide.

3. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The hydrated alumina is pseudo-boehmite.

4. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The titanium-containing compound is selected from one or more of titanic acid, metatitanic acid and titanium dioxide, with a particle size less than or equal to 1000 meshes, the titanium-containing compound is calculated as titanium dioxide, the hydrated alumina is calculated as alumina, and the amount of the titanium-containing compound added is 0.5-5% of the weight of the hydrated alumina.

5. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The hydrated alumina is calculated as alumina, and the amount of the organic polymer added is 1-6% of the weight of the hydrated alumina.

6. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The boron-containing compound is selected from one or more of boric acid, metaboric acid, ammonium hydrogen borate, ammonium tetraborate tetrahydrate and ammonium pentaborate tetrahydrate. The boron-containing compound is calculated as elemental boron, and the hydrated alumina is calculated as alumina. The amount of the boron-containing compound added is 0.3-2% of the weight of the hydrated alumina.

7. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The hydrated alumina is calculated on the basis of alumina, and the amount of ammonia added is 0.05-0.5% of the weight of the hydrated alumina.

8. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The low-carbon alcohol is selected from one or more of methanol, ethanol, ethylene glycol, propanol, isopropanol and glycerol. The hydrated alumina is calculated as alumina, and the amount of the low-carbon alcohol added is 0.5-5% of the weight of the hydrated alumina.

9. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: Calculated as oxide, the first active metal accounts for 2-8% of the total weight of the catalyst, and the second active metal accounts for 0.4-2% of the total weight of the catalyst.

10. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The synthetic cellulose is selected from one or more of methyl cellulose, ethyl cellulose, hydroxypropyl methyl cellulose and hydroxyethyl methyl cellulose. The hydrated aluminum oxide is calculated as aluminum oxide, and the amount of the synthetic cellulose added is 1-5% of the weight of the hydrated aluminum oxide.

11. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The synthetic cellulose has a 2% aqueous solution viscosity greater than or equal to 50,000 mPa·s.

12. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The particle size of the organic polymer is 80-400 meshes.

13. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The active metal is loaded by impregnation.

14. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The molding process is carried out using a hydraulic extruder with an extrusion pressure of 10-30 MPa.

15. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 14, characterized in that: The hydraulic extruder is an oil pressure extruder.

16. The method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to claim 1, characterized in that: The calcination temperature is 500-1100° C., and the calcination time is 0.5-4 hours.

17. A catalyst prepared by the method for preparing a titanium-containing residue oil hydrodemetallization catalyst according to any one of claims 1 to 16.

18. The catalyst according to claim 17, characterized in that The catalyst has a bimodal pore structure with a pore volume of 0.8-1.6 ml / g. Pores with a diameter of 20-100 nanometers account for 30-70% of the total pore volume, pores with a pore diameter of more than 100 nanometers account for 20-50% of the total pore volume, pores with a pore diameter of less than 20 nm account for less than 30% of the total pore volume, and the BET specific surface area is 80-220 square meters / g.

Citation Information

Patent Citations

  • A dual-peak porous alumina carrier and its preparation method

    CN105983443B

  • Preparing method for aluminium oxide carrier with double-hole

    CN1103009A

  • Macroporous aluminium oxide carrier and its preparing method

    CN1647857A

  • Heavy oil hydrogenating treatment catalyst and preparation method thereof

    CN101433848A

  • Preparation method of boron-modified alumina carrier

    CN102728335A