Titanium silicon molecular sieve and preparation method thereof and method for catalytic oxidation of cycloalkanes

By preparing titanium-silicon molecular sieves with specific parameters and applying them to the catalytic oxidation of naphthenes, the problems of equipment slagging and high energy consumption of cobalt catalysts in the existing technology are solved, and the catalytic oxidation effect of high conversion rate and low energy consumption is achieved.

CN116332198BActive Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202111578457.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-22
Publication Date
2024-10-22
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

The cobalt catalyst used in the existing catalytic oxidation of cyclohexane can easily lead to equipment slagging and the generation of by-products, and the unconverted cyclohexane needs to be separated and recycled, which consumes high energy and the catalytic oxidation performance needs to be improved.

Method used

By preparing titanium-silica molecular sieves with specific parameters and using silanization reagents to treat titanium-silica sol, a titanium-silica molecular sieve with high specific surface area and pore volume is formed, which can be used to catalyze the oxidation of cycloalkanes and improve catalytic activity.

Benefits of technology

The conversion rate of naphthenes reaches over 91%, which improves the catalytic oxidation performance, reduces energy consumption, and simplifies the separation and recovery process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116332198B_ABST
    Figure CN116332198B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of catalytic oxidation of cycloalkanes, and in particular to a titanium silicon molecular sieve and a preparation method thereof and a method for catalytic oxidation of cycloalkanes. The titanium silicon molecular sieve has a pore size of 0.1-2 nm and a specific surface area of ​​440-580 m 2 / g, with a total pore volume of 0.4-0.6cm 3 / g; external surface area 50‑200m 2 / g, micropore volume is 0.13-0.20cm 3 / g; the particle size of the molecular sieve particles is 100-250nm; the molecular sieve crystallinity is ≥50%. The titanium silicalite molecular sieve prepared by treating the titanium silicalite precursor with a specific silanization agent has high catalytic activity when used in the catalytic oxidation of cycloalkanes, and the conversion rate of cycloalkanes can be increased to more than 91%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalytic oxidation of cycloalkanes, and in particular to a titanium silicon molecular sieve and a preparation method thereof, and a method for catalytic oxidation of cycloalkanes. Background Art

[0002] Catalytic oxidation reaction is an important synthesis reaction and is widely used in the fields of petrochemicals and fine chemicals. For example, cyclohexane catalytic oxidation to prepare cyclohexanone and cyclohexanol is the main method for producing cyclohexanol and cyclohexanone in the world. Cyclohexanone is a colorless transparent liquid that is slightly soluble in water and can be miscible with organic solvents such as ethanol and acetone. Cyclohexanol is a colorless transparent oily liquid or white needle-shaped crystals with a camphor-like odor and can be miscible with ethanol, ethyl acetate, and aromatic hydrocarbons. Cyclohexanone and cyclohexanol are mainly used as raw materials for organic synthesis in industry to produce nylon, caprolactam, adipic acid, etc. Cobalt catalysts (soluble cobalt salts) are mainly used for catalytic cyclohexane oxidation in industry, but this process is prone to slagging on equipment and pipeline walls, and produces by-products such as carboxylic acids. A large amount of unconverted cyclohexane needs to be separated and recycled for reaction, which consumes a lot of energy. Therefore, developing a new catalytic oxidation system to obtain high cyclohexane conversion rate and cyclohexanone and cyclohexanol yield is an important research goal.

[0003] Molecular sieve catalysts are heterogeneous catalysts commonly used in the chemical industry. They are not only easy to separate and recycle, but also can obtain specific catalytic activity by introducing different metal atoms into the molecular sieve framework. For example, titanium silicon molecular sieves obtained by inserting titanium atoms into the molecular sieve framework can form a catalytic oxidation system with hydrogen peroxide, which has excellent catalytic effects on many oxidation reactions. This is because the empty orbitals of the framework titanium atoms can receive the lone electron pairs of hydrogen peroxide, thereby forming Ti-OOH catalytic active centers.

[0004] CN108726528A discloses a multi-level porous titanium silicalite molecular sieve, a preparation method thereof and a method for olefin epoxidation. A certain proportion of mesoporous channels can be introduced into the titanium silicalite molecular sieve by treatment with a silanization agent. Although this is beneficial to the mass transfer and diffusion of the reaction molecules, the loss of some active centers at the same time may lead to a decrease in the catalytic oxidation performance of the molecular sieve. Summary of the invention

[0005] The purpose of the present invention is to improve the catalytic oxidation performance of titanium silicate in the catalytic oxidation reaction of cycloalkanes, and to provide titanium silicate and a preparation method thereof and a method for catalytic oxidation of cycloalkanes.

[0006] In order to achieve the above object, the present invention provides a titanium silicon molecular sieve in the first aspect, wherein the pore size of the titanium silicon molecular sieve is 0.1-2nm and the specific surface area is 440-580m 2 / g, with a total pore volume of 0.4-0.6cm 3 / g; external surface area is 50-200m2 / g, micropore volume is 0.13-0.2cm 3 / g; the particle size of the molecular sieve particles is 100-250nm; the crystallinity of the molecular sieve is ≥50%.

[0007] A second aspect of the present invention provides a method for preparing titanium silicon molecular sieve, the method comprising:

[0008] (1) mixing a silicon source, an alkaline template, a titanium source, water and isopropanol to obtain a titanium silicalose sol;

[0009] (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination;

[0010]

[0011] Wherein, i is an integer of 1-6; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group.

[0012] The third aspect of the present invention provides a titanium silicon molecular sieve prepared according to the method described in the second aspect.

[0013] A fourth aspect of the present invention provides a method for catalytic oxidation of cycloalkanes, the method comprising: contacting cycloalkanes and peroxides for reaction in the presence of a catalyst, wherein the catalyst comprises the titanium silicon molecular sieve described in the first aspect or the third aspect.

[0014] Through the above technical scheme, the present invention treats the titanium silicalite precursor with a specific silanization agent, and the titanium silicalite molecular sieve with specific parameters prepared has high catalytic activity when used in the catalytic oxidation reaction of cycloalkanes, and the conversion rate of cycloalkanes can be increased to more than 91%. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is a pore size distribution diagram of the titanium silicon molecular sieve obtained in Example 1 of the present invention;

[0016] Figure 2 is a N2 adsorption-desorption curve diagram of the titanium silicon molecular sieve obtained in Example 1 of the present invention;

[0017] Figure 3 is a TEM image of the titanium silicon molecular sieve obtained in Example 1 of the present invention;

[0018] Figure 4 is the XRD diagram of the titanium silicon molecular sieve obtained in Example 1 of the present invention;

[0019] Figure 5 This is the pore size distribution diagram of the titanium silicon molecular sieve obtained in Comparative Example 1. DETAILED DESCRIPTION

[0020] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0021] As mentioned above, the first aspect of the present invention provides a titanium silicon molecular sieve, wherein the pore size of the titanium silicon molecular sieve is 0.1-2nm, and the specific surface area is 440-580m 2 / g, with a total pore volume of 0.4-0.6cm 3 / g; external surface area is 50-200m 2 / g, micropore volume is 0.13-0.2cm 3 / g; the particle size of the molecular sieve particles is 100-250nm; the crystallinity of the molecular sieve is ≥50%.

[0022] According to the present invention, under preferred conditions, the molar ratio of titanium to silicon in the titanium silicalite is 0.001-0.04:1, preferably 0.005-0.025:1.

[0023] In some preferred embodiments of the present invention, the surface area of ​​the titanium silicalite is 120-200 m 2 / g, preferably 150-200m 2 / g.

[0024] According to the present invention, under preferred conditions, the specific surface area of ​​the titanium silicate molecular sieve is 460-490m 2 / g.

[0025] In the present invention, the external surface area of ​​the titanium silicalite molecular sieve refers to the surface area of ​​the outer surface of the titanium silicalite molecular sieve, which can be obtained by testing using the BET method; the specific surface area of ​​the titanium silicalite molecular sieve refers to the BET specific surface area.

[0026] According to the present invention, under preferred conditions, the particle size of the titanium silicalite molecular sieve is 150-240 nm.

[0027] According to the present invention, under preferred conditions, in the infrared spectrum of the titanium silicalite molecular sieve, the wave number is 960cm -1 The peak area and wave number are 800cm -1 The ratio of the peak areas is 0.4-1.5.

[0028] A second aspect of the present invention provides a method for preparing titanium silicon molecular sieve, the method comprising:

[0029] (1) mixing a silicon source, an alkaline template, a titanium source, water and isopropanol to obtain a titanium silicalose sol;

[0030] (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination;

[0031]

[0032] Wherein, i is an integer of 1-6; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group.

[0033] In the present invention, the C1-C6 alkyl group refers to an alkyl group having 1 to 6 carbon atoms in total, for example, it can be one of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl and n-hexyl.

[0034] In some preferred embodiments of the present invention, i is an integer of 1-5, for example, 1, 2, 3, 4 or 5.

[0035] In some preferred embodiments of the present invention, R1, R2 and R3 are each independently selected from a C1-C3 alkyl group, and the C1-C3 alkyl group may be a methyl group, an ethyl group, a n-propyl group or an isopropyl group. Preferably, R1, R2 and R3 are each independently selected from a methyl group, an ethyl group or an n-propyl group. In the present invention, R1, R2 and R3 may be the same or different. Preferably, R1, R2 and R3 are the same.

[0036] In the present invention, by using the compound represented by formula (I) as a silanization agent, during the hydrothermal crystallization reaction, a titanium silicalite molecular sieve with a fully microporous structure can be formed through the weak intermolecular interaction force between the alkyl chains of the silanization agent, and the titanium silicalite molecular sieve has a high specific surface area and pore volume. When catalyzing the oxidation reaction of cycloalkanes, it is beneficial to the intra-crystal and inter-crystal mass transfer and diffusion of reactant molecules and product molecules, and can basically convert all cycloalkanes into cyclic ketones and cyclic alcohols.

[0037] According to the present invention, if the amount of the silanization agent (the compound shown in formula (I)) is too high, the crystallization performance of the titanium silical sol will deteriorate and the molecular sieve cannot be obtained; if the amount of the silanization agent (the compound shown in formula (I)) is too low, the specific surface area of ​​the obtained titanium silicalite molecular sieve will be reduced, affecting the mass transfer and further affecting its activity in the catalytic oxidation reaction of cycloalkanes; under preferred conditions, in step (1), the silicon source is calculated as SiO2, and the molar ratio of the silicon source to the compound shown in formula (I) is 1:(0.01-0.3), preferably 1:(0.01-0.2); more preferably 1:(0.05-0.2).

[0038] In some preferred embodiments of the present invention, the silicon source is calculated as SiO2, the alkaline template is calculated as N when it contains nitrogen, and the alkaline template is calculated as OH when it does not contain nitrogen. - The molar ratio of the silicon source, the alkaline template and water is 1:(0.05-0.4):(5-40); preferably 1:(0.1-0.3):(5-25).

[0039] According to the present invention, under preferred conditions, the silicon source is selected from at least one of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, tetrabutyl silicate, silica gel, white carbon black and silica sol.

[0040] According to the present invention, under preferred conditions, the alkaline template is selected from at least one of quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines, preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.

[0041] In some preferred embodiments of the present invention, the silicon source is calculated as SiO2, the titanium source is calculated as TiO2, and the molar ratio of the silicon source, the titanium source and isopropanol is 1:(0.001-0.04):(0.1-10), preferably 1:(0.005-0.025):(0.1-5).

[0042] According to the present invention, under preferred conditions, the titanium source is selected from an organic titanium source and / or an inorganic titanium source; further preferably, the titanium source is selected from at least one of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate.

[0043] According to the present invention, under preferred conditions, step (1) further comprises: first stirring and mixing the silicon source, the alkaline template and water to obtain a mixed system; then dropwise adding a mixed solution of the titanium source and isopropanol into the mixed system for a second stirring to obtain a mixed solution.

[0044] In the present invention, the droplet acceleration rate of the mixed solution is preferably 0.01-0.5 mL / min; more preferably 0.1-0.5 mL / min.

[0045] In the present invention, preferably, the first stirring time is 0.1-2h.

[0046] In the present invention, preferably, the second stirring time is 0.5-6h, preferably 0.5-3h.

[0047] In the present invention, preferably, step (1) further comprises: driving out alcohol from the mixed solution; driving out alcohol can remove alcohol generated by hydrolysis of silicon source and titanium source, and in the present invention, preferably, azeotropic distillation is used to remove alcohol generated in the system, and water lost by azeotropic distillation is supplemented during the driving out alcohol process to ensure that the ratio of each substance in the titanium silica sol meets the above requirements; preferably, the conditions for driving out alcohol include: temperature of 30-100°C and time of 2-10h; preferably temperature of 40-90°C and time of 4-10h.

[0048] According to the present invention, in order to make the silanization agent uniformly dispersed in the titanium silica sol, under preferred conditions, step (1) also includes: adding the compound represented by formula (I) to the titanium silica sol and performing a third stirring for 0.1-24 hours, preferably the third stirring time is 0.5-10 hours, and more preferably 1-3 hours.

[0049] In the present invention, by rapidly heating up, the nucleation and growth rates of the molecular sieve at low temperature can be controlled, thereby obtaining molecular sieve particles with smaller sizes. According to the present invention, under preferred conditions, in step (2), the conditions for hydrothermal crystallization include: heating the mixture to 50-200°C within 0.1-1h, and then performing hydrothermal crystallization at 50-200°C for 10-100h; preferably, performing hydrothermal crystallization at a temperature of 100-200°C for 20-80h; further preferably, the heating time is 0.1-0.5h; more preferably, the conditions for hydrothermal crystallization include: a temperature of 120-180°C and a time of 20-80h; under the above preferred conditions, the crystallinity, specific surface area and pore volume of the molecular sieve can be balanced; and a molecular sieve with specific crystallinity, specific surface area and pore volume can be prepared.

[0050] The present invention has no particular limitation on the pressure of hydrothermal crystallization, which may be the autogenous pressure of the crystallization system.

[0051] According to the present invention, under preferred conditions, the method further comprises: washing, filtering and drying the product obtained by hydrothermal crystallization; wherein the washing, filtering and drying processes can be known to those skilled in the art. Exemplarily, the washing temperature can be 20-50°C, the washing solvent can be water, and the amount of the washing solvent is 1-20 times the mass of the crystallized product; the drying conditions can be: the temperature is 40-150°C and the time is 0.5-24h.

[0052] In some preferred embodiments of the present invention, the calcination conditions include: a temperature of 400-800° C. and a time of 1-15 h; preferably a temperature of 500-600° C. and a time of 4-10 h.

[0053] The third aspect of the present invention provides a titanium silicon molecular sieve prepared according to the method described in the second aspect.

[0054] Preferably, the pore size of the titanium silicon molecular sieve is 0.1-2 nm, and the specific surface area is 440-580 m 2 / g, with a total pore volume of 0.4-0.6cm 3 / g; external surface area is 50-200m 2 / g, micropore volume is 0.13-0.2cm 3 / g; the particle size of the molecular sieve particles is 100-250nm; the molecular sieve crystallinity is ≥50%; more preferably, the molar ratio of titanium to silicon in the titanium silicon molecular sieve is 0.001-0.04:1, preferably 0.005-0.025:1; further preferably, in the infrared spectrum of the titanium silicon molecular sieve, the wave number is 960cm -1 The peak area and wave number are 800cm -1 The ratio of the peak areas is 0.4-1.5.

[0055] Further preferably, the titanium silicalite has high activity in catalyzing cyclohexane oxidation reaction, and in the catalytic oxidation reaction of cycloalkanes, the conversion rate of cycloalkanes is increased to more than 90%.

[0056] A fourth aspect of the present invention provides a method for catalytic oxidation of cycloalkanes, the method comprising: contacting cycloalkanes and peroxides for reaction in the presence of a catalyst, wherein the catalyst comprises the titanium silicon molecular sieve described in the first aspect or the third aspect.

[0057] According to the present invention, under preferred conditions, the cycloalkane is selected from C3-C 15 cycloalkane, preferably C4-C8 cycloalkane; more preferably at least one of cyclohexane, cyclopentane and methylcyclohexane, most preferably cyclohexane.

[0058] According to the present invention, under preferred conditions, the peroxide is selected from at least one of tert-butyl hydroperoxide, cyclohexyl hydroperoxide, isopropyl hydroperoxide, cumene hydroperoxide, hydrogen peroxide, sodium percarbonate and sodium perborate.

[0059] In some preferred embodiments of the present invention, the reaction conditions include: the weight ratio of the catalyst to the cycloalkane is 1: (1-20); the molar ratio of the cycloalkane to the peroxide is 1: (0.1-10); further preferably, the reaction conditions also include: temperature of 40-100°C and time of 1-8h.

[0060] In some embodiments of the present invention, the form of the catalyst can be selected according to actual needs. The catalyst can be a molecular sieve supported on a carrier or a molecular sieve powder. In the present invention, it is preferred to directly use the molecular sieve powder as the catalyst.

[0061] According to a particularly preferred embodiment of the present invention, the method for preparing titanium silicon molecular sieve comprises:

[0062] (1) mixing a silicon source, an alkaline template and water in a molar ratio of 1:(0.1-0.3):(5-25), stirring for a first time at room temperature for 0.1-2 hours, then adding a mixed solution of a titanium source and isopropanol dropwise to the mixed system at a rate of 0.1-0.5 mL / min, stirring for a second time for 0.5-3 hours, and obtaining a mixed solution; wherein the molar ratio of the silicon source, the titanium source and isopropanol is 1:(0.005-0.025):(0.1-5);

[0063] Then, the mixed system is subjected to alcohol removal to obtain titanium silicalose; the temperature of the alcohol removal is 40-90° C. and the time is 4-10 hours;

[0064] (2) adding the compound represented by formula (I) to the titanium silicalose, and subjecting the obtained mixture to hydrothermal crystallization and calcination; wherein the molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.2), and the crystallization conditions are: heating the mixture to 150-180° C. within 0.5-1 h, and then subjecting the mixture to hydrothermal crystallization at 150-180° C. for 12-48 h;

[0065]

[0066] Wherein, i is an integer of 1-5; R1, R2 and R3 are the same; R1, R2 and R3 are selected from methyl, ethyl or propyl.

[0067] The present invention will be described in detail below by way of examples. In the following examples, room temperature refers to 25±5°C.

[0068] In the following examples and comparative examples, the X-ray diffraction (XRD) crystal phase diagram of the samples was measured on a Siemens D5005 X-ray diffractometer, with a CuKα source, a tube voltage of 40 kV, a tube current of 40 mA, a scanning speed of 0.5° / min, and a scanning range of 2θ=5°-35°. According to the XRD spectrum, the crystallinity was obtained by fitting using BRUKER's software eva;

[0069] The surface area and specific surface area were obtained by measuring the static N2 adsorption-desorption curve of the sample at liquid nitrogen temperature (77.4K) using Micromeritics' ASAP2405J static nitrogen adsorption instrument and then performing BET fitting on the adsorption curve.

[0070] The pore volume was determined according to the method described in RIPP 151-90 in "Analytical Methods in Petrochemical Industry" compiled by Yang Cuiding et al. (Science Press, first edition, published in September 1990);

[0071] The pore size distribution was calculated according to the BJH formula;

[0072] The particle size was characterized by JEOL JEM-2100 transmission electron microscope (TEM);

[0073] The UV-Vis spectra of the samples were obtained by Agilent Cary 300 UV spectrophotometer with a wavelength interval of 3 nm and a scanning range of 190-800 nm.

[0074] In the following examples, the chemical structural formulas of the silanization agents used are shown in Table 1, and Compound 1, Compound 2 and Compound 3 are all commercially available.

[0075] Table 1

[0076]

[0077]

[0078] Example 1

[0079] (1) tetraethyl silicate, tetrapropylammonium hydroxide and water are first stirred and mixed at room temperature to obtain a mixed system, and during the stirring process, a mixed solution of tetrabutyl titanate and isopropyl alcohol is dropwise added to the mixed system at a rate of 0.2 mL / min, and a second stirring is performed for 0.5 h to obtain a mixed solution; tetraethyl silicate is calculated as SiO2, tetrapropylammonium hydroxide is calculated as N, and tetrabutyl titanate is calculated as TiO2; the molar ratio of tetraethyl silicate, tetrapropylammonium hydroxide and water is 1:0.1:15; the molar ratio of tetraethyl silicate, tetrabutyl titanate and isopropyl alcohol is 1:0.005:3;

[0080] Then, the mixed solution was subjected to alcoholization at 80°C for 6 hours to obtain titanium silicalose;

[0081] (2) adding compound (1) to titanium silicalose, and stirring for a third time at room temperature for 1.5 hours to obtain a mixture, wherein the molar ratio of compound (1) to tetraethyl silicate is 0.1:1;

[0082] (3) heating the mixture to 170° C. for 0.5 h, and performing hydrothermal crystallization at 170° C. for 24 h to obtain a crystallized product; the crystallized product was sequentially rinsed with water, filtered, and dried at 120° C. for 2 h;

[0083] The dried product was calcined at 550°C for 6 hours to obtain titanium silicon molecular sieve;

[0084] The pore size distribution of the titanium silicate molecular sieve obtained in this example is as follows: Figure 1 As shown, the N2 adsorption and desorption curve is as follows Figure 2 shown; from Figure 1 and Figure 2 It can be seen that the titanium silicon molecular sieve obtained in this embodiment only contains micropores with a pore size of about 0.55 nm;

[0085] The TEM image of the titanium silicon molecular sieve obtained in this example is as follows: Figure 3 As shown, from Figure 3 It can be seen that the particle size of the titanium silicon molecular sieve obtained in this embodiment is about 100-150nm;

[0086] The XRD spectrum of the titanium silicon molecular sieve obtained in this example is as follows: Figure 4 As shown, from Figure 4 It can be seen that the titanium silicon molecular sieve obtained in this embodiment has an MFI structure and good crystallization performance;

[0087] The physical properties of the titanium silicate molecular sieve obtained in this example are shown in Table 3.

[0088] Embodiment 2-20

[0089] Titanium silicate molecular sieve was prepared according to the method of Example 1. The proportions and synthesis conditions are shown in Table 2. The physical properties of the prepared molecular sieve are shown in Table 3.

[0090] Comparative Example 1

[0091] Titanium silicon molecular sieve was prepared according to the method of Example 1 of CN106145151B, and the specific method is as follows:

[0092] Tetraethyl silicate, tetrapropylammonium hydroxide, tetrabutyl titanate and deionized water are mixed to obtain a mixture with a molar ratio of SiO2: structure directing agent: TiO2: H2O = 1: 0.2: 0.025: 50. Then, quaternized cellulose and N-phenyl-3-aminopropyltrimethoxysilane are added to the titanium silicate molecular sieve precursor gel mixture at a molar ratio of SiO2 to silanization agent of 1: 0.1 and a weight ratio of SiO2 to natural polymer compound of 1: 0.1. After stirring evenly, the titanium silicate molecular sieve precursor treated with the silanization agent and modified natural polymer compound is transferred to a pressure-resistant stainless steel reactor; heated to 170°C under stirring and crystallized under autogenous pressure for 24 hours. After the stainless steel pressure-resistant reactor is cooled to room temperature, the uncalcined titanium silicate molecular sieve is recovered, dried at 110°C for 6 hours, and then calcined at 550°C for 4 hours to obtain the multi-level porous titanium silicate molecular sieve TS-1. The pore size distribution diagram is as follows Figure 5 The product characteristics are shown in Table 3.

[0093] Comparative Examples 2-6

[0094] Titanium silicate molecular sieve was prepared according to the method of Example 1. The proportion and synthesis conditions are shown in Table 2. The physical property parameters of the prepared molecular sieve are shown in Table 3.

[0095] Comparative Example 7

[0096] Titanium silicate molecular sieve was prepared according to the method of Example 1, except that the silanization agent (Compound 4) was methyltriethoxysilane. The proportion and synthesis conditions thereof are shown in Table 2. The physical properties of the prepared molecular sieve are shown in Table 3.

[0097] Comparative Example 8

[0098] Titanium silicate molecular sieve was prepared according to the method of Example 1, except that the silanization agent (Compound 5) was octyltriethoxysilane. The proportion and synthesis conditions thereof are shown in Table 2. The physical properties of the prepared molecular sieve are shown in Table 3.

[0099] Test Case

[0100] This test example illustrates the reaction effect of the titanium silicon molecular sieve prepared by the example samples provided by the present invention and the comparative example for the preparation of cyclohexanol and cyclohexanone by cyclohexane oxidation reaction. The reagents used in this test example are all commercially available chemically pure reagents. The concentration of each substance after the reaction is quantitatively analyzed using gas chromatography. The instrument used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is an HP-5 capillary chromatographic column and a hydrogen flame ionization detector. The component concentration is quantified using the external standard method. First, the peak area of ​​each component is measured, the component concentration is obtained through the standard working curve, and the selectivity and other indicators of the corresponding product are calculated.

[0101] The cyclohexane conversion, cyclohexanone and cyclohexanol selectivity in the test example were calculated according to the following formulas:

[0102] Cyclohexane conversion rate % = (1-moles of cyclohexane remaining after reaction / moles of cyclohexane added before reaction) × 100%

[0103] Cyclohexanone selectivity % = moles of cyclohexanone after reaction / (moles of cyclohexane added before reaction - moles of cyclohexane remaining after reaction) × 100%

[0104] Cyclohexanol selectivity % = moles of cyclohexanol after reaction / (moles of cyclohexane added before reaction - moles of cyclohexane remaining after reaction) × 100%

[0105] The titanium silicon molecular sieve prepared in the above embodiment and comparative example was taken as a catalyst, and the catalyst, cyclohexane, and solvent methanol were added to a three-necked flask in a mass ratio of 1:20:100, and mixed evenly under magnetic stirring. After the temperature was raised to 70°C by electric heating, an aqueous hydrogen peroxide solution (30% by weight) was added to the above mixture, the molar ratio of cyclohexane to hydrogen peroxide was 1:1, the reaction temperature was maintained at 70°C, the reaction time was 5h, and samples were taken for chromatographic analysis. The reaction results are shown in Table 2.

[0106]

[0107]

[0108]

[0109] It can be seen from the results in Table 3 that the titanium silicalite of the present invention has high activity in catalytic oxidation of cyclohexane. In the catalytic oxidation of cyclohexane, the conversion rate of cyclohexane is as high as 99%, the selectivity of cyclohexanone is as high as 48%, and the selectivity of cyclohexanol is as high as 48%.

[0110] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A titanium silicon molecular sieve, characterized in that: The pore size of the titanium silicate molecular sieve is 0.1-2 nm, and the specific surface area is 440-580 m 2 / g, with a total pore volume of 0.4-0.6cm 3 / g; external surface area is 50-200m 2 / g, micropore volume is 0.13-0.2cm 3 / g; the particle size of the molecular sieve particles is 100-250nm; the crystallinity of the molecular sieve is ≥50%; In the infrared spectrum of the titanium silicate molecular sieve, the wave number is 960cm -1 The peak area and wave number are 800cm -1 The ratio of the peak areas is 0.4-1.

5.

2. The titanium silicon molecular sieve according to claim 1, wherein: The molar ratio of titanium to silicon in the titanium silicalite molecular sieve is 0.001-0.04:

1.

3. The titanium silicon molecular sieve according to claim 2, wherein: The molar ratio of titanium to silicon in the titanium silicalite molecular sieve is 0.005-0.

025.

4. A method for preparing titanium silicon molecular sieve, characterized in that: The method comprises: (1) mixing a silicon source, an alkaline template, a titanium source, water and isopropanol to obtain a titanium silicalose sol; (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination; wherein i is an integer of 1-6; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group; The silicon source is calculated as SiO2, and the molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.3); The silicon source is calculated as SiO2, the alkaline template is calculated as N when it contains nitrogen, and as OH when it does not contain nitrogen. - The titanium source is calculated as TiO2, The molar ratio of the silicon source, the alkaline template and water is 1:(0.05-0.4):(5-40); The molar ratio of the silicon source, the titanium source and isopropanol is 1:(0.001-0.04):(0.1-10); In step (2), the hydrothermal crystallization conditions include: heating the mixture to 50-200° C. within 0.1-1 h, and then crystallizing at 50-200° C. for 10-100 h.

5. The method according to claim 4, wherein: i is an integer from 1 to 5.

6. The method according to claim 4, wherein: R1, R2 and R3 are each independently selected from methyl, ethyl or propyl.

7. The method according to claim 4, wherein: The silicon source is calculated as SiO2, and the molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.2).

8. The method according to any one of claims 4 to 7, wherein: The silicon source is calculated as SiO2, the alkaline template is calculated as N when it contains nitrogen, and as OH when it does not contain nitrogen. - The titanium source is calculated as TiO2, The molar ratio of the silicon source, the alkaline template and water is 1:(0.1-0.3):(5-25); The molar ratio of the silicon source, the titanium source and isopropanol is 1:(0.005-0.025):(0.1-5).

9. The method according to any one of claims 4 to 7, wherein: The silicon source is selected from at least one of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, tetrabutyl silicate, white carbon black and silica sol.

10. The method according to any one of claims 4 to 7, wherein: The alkaline template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.

11. The method according to claim 10, wherein: The alkaline template agent is selected from at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.

12. The method according to any one of claims 4 to 7, wherein: The titanium source is selected from an organic titanium source and / or an inorganic titanium source.

13. The method according to claim 12, wherein: The titanium source is selected from at least one of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate.

14. The method according to any one of claims 4 to 7, wherein: Step (1) also includes: stirring and mixing a silicon source, an alkaline template, and water to obtain a mixed system; and then dropwise adding a mixed solution of a titanium source and isopropanol into the mixed system to obtain a mixed solution.

15. The method according to claim 14, wherein: The droplet acceleration rate of the mixed solution is 0.01-0.5 mL / min.

16. The method according to claim 14, wherein: Step (1) also includes: removing alcohol from the mixed solution.

17. The method according to claim 16, wherein: The conditions for driving out the alcohol include: temperature of 30-100° C. and time of 2-10 h.

18. The method according to claim 17, wherein: The conditions for driving out the alcohol include: temperature of 40-90° C. and time of 4-10 h.

19. The method according to any one of claims 4 to 7, wherein: In step (2), the hydrothermal crystallization conditions include: performing crystallization at a temperature of 100-200° C. for 20-80 hours.

20. The method according to any one of claims 4 to 7, wherein: The calcination conditions include: temperature of 400-800° C. and time of 1-15 hours.

21. A titanium silicon molecular sieve prepared according to the method according to any one of claims 4 to 20.

22. The titanium silicalite molecular sieve according to claim 21, wherein: The pore size of the titanium silicate molecular sieve is 0.1-2 nm, and the specific surface area is 440-580 m 2 / g, with a total pore volume of 0.4-0.6cm 3 / g; external surface area is 50-200m 2 / g, micropore volume is 0.13-0.2cm 3 / g; the particle size of the molecular sieve particles is 100-250nm; the crystallinity of the molecular sieve is ≥50%.

23. The titanium silicalite molecular sieve according to claim 21, wherein: The molar ratio of titanium to silicon in the titanium silicalite molecular sieve is 0.001-0.04:

1.

24. The titanium silicon molecular sieve according to claim 23, wherein: The molar ratio of titanium to silicon in the titanium silicalite molecular sieve is 0.005-0.025:

1.

25. The titanium silicalite molecular sieve according to claim 21, wherein: In the infrared spectrum of the titanium silicate molecular sieve, the wave number is 960cm -1 The peak area and wave number are 800cm -1 The ratio of the peak areas is 0.4-1.

5.

26. A method for catalytically oxidizing cycloalkanes, the method comprising: In the presence of a catalyst, cycloalkane and peroxide are contacted to react, wherein the catalyst comprises the titanium silicon molecular sieve described in claim 1, 2, 3, 21, 22, 23, 24 or 25.

27. The method according to claim 26, wherein: The cycloalkane is selected from C3-C 15 of cycloalkanes.

28. The method according to claim 27, wherein: The cycloalkane is selected from C4-C8 cycloalkane.

29. The method according to claim 28, wherein: The cycloalkane is selected from at least one of cyclohexane, cyclopentane and methylcyclohexane.

30. The method of claim 26, wherein: The peroxide is selected from at least one of tert-butyl hydroperoxide, cyclohexyl hydroperoxide, isopropyl hydroperoxide, cumene hydroperoxide, hydrogen peroxide, sodium percarbonate and sodium perborate.

31. The method of claim 26, wherein: The reaction conditions include: the weight ratio of the catalyst to the cycloalkane is 1:(1-20); the molar ratio of the cycloalkane to the peroxide is 1:(0.1-10).

32. The method of claim 26, wherein: The reaction conditions include: temperature of 40-100° C. and time of 1-8 h.

Citation Information

Patent Citations

  • A hierarchical porous titanium-silicon molecular sieve and its synthesis method

    CN106145151B

  • Hierarchical porous titanium-silicon molecular sieve as well as preparation method thereof and olefin epoxidation method

    CN108726528A

  • Interior surface coating structure mesoporous titanium silicate molecular sieve material and preparation method and use thereof

    CN101417809A

  • Method for preparing mesoporous titanium silicate molecular sieve

    CN101456562A

  • Self-assembly method for preparing multi-stage structure SAPO-34 molecular sieve

    CN108249457A