A method for preparing a two-component water-based coating
By using the hydrothermal method to prepare corrosion-resistant cadmium-doped Fe3O4 nanosphere particles and directional adsorption of silica shells in water-based polyurethane coatings, the problem of insufficient resistance of water-based polyurethane in the coating field is solved, and the corrosion resistance and dispersion of the coating are improved. , achieving efficient coating performance improvement.
Patent Information
- Application Number
- CN202310503994.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-05-06
AI Technical Summary
The application of water-based polyurethane in the coating field is limited by its insufficient solvent resistance, weather resistance, and heat resistance. The structure and performance of existing superhydrophobic coatings are unstable and difficult to prepare on a large scale.
The hydrothermal method is used to prepare corrosion-resistant cadmium-doped Fe3O4 nanosphere particles under extremely high temperature conditions, and is activated and removed by pickling to directionally adsorb the silica shell to form a magnetic suspension with high suspension and stability as a water-based coating filler. , combined with the preparation method of two-component polyurethane coating, to improve the corrosion resistance and dispersion of the coating.
The corrosion resistance and tensile strength of the coating are significantly improved, the service life of the magnetic coating is enhanced, and the preparation of high-purity magnetic particles and good dispersion in polyurethane coatings are achieved.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings and relates to a two-component water-based coating filler, a polyurethane composite coating and a preparation method thereof. Background Art
[0002] Waterborne polyurethane refers to a polyurethane emulsion in which polyurethane is dispersed using water as a solvent. Solvent-based polyurethane is widely used, but the use of organic solvents can cause air pollution and is toxic. In recent years, people have paid more and more attention to environmental issues, which has promoted the development and research of waterborne polyurethane. Waterborne polyurethane is widely used in adhesives, coatings and other fields, and has attracted much attention due to its environmental friendliness and safety. The characteristics of polyurethane are good wear resistance, high load-bearing capacity, high tear strength, and resistance to low temperatures, oils, and ozone. In addition, the advantages of a variety of raw materials and adjustable molecular structures have made polyurethane more deeply used in industries such as elastomers, foam plastics, coatings, and adhesives. It must be admitted that polyurethane itself also has its own shortcomings, such as poor solvent resistance, weather resistance, and heat resistance, which greatly reduces the breadth of its application in coatings. At present, the methods of waterborne polyurethane modification can be divided into acrylic modification, epoxy resin modification, polysiloxane modification, and natural product modification according to different modifiers. Recently, polymer composites have attracted great attention. Inorganic nanoparticles can improve the mechanical properties, optical properties, thermal properties, corrosion resistance, magnetic properties, etc. of polymer materials.
[0003] Magnetic nanoparticles have potential applications in biomedicine, industry, and military due to their inherent magnetic properties, microstructure, large specific surface area, surface charge, and low toxicity. Due to its biocompatibility and chemical stability, ferroferric oxide has attracted much attention and has been used in targeted drug delivery systems. A variety of different methods have been used to develop this material. Due to its hydrophobicity, magnetic materials can be easily polymerized. Surface modification helps to improve the stability of nanoparticles and can provide additional functional groups that may be used in other applications. One way to avoid agglomeration of nanoparticles is to coat their surface with a layer of water-soluble material, which is usually ferroferric oxide as the core and a layer of other materials on it. Common coating materials are multi-metal oxides or other inorganic materials as shells, including titanium dioxide, silicon dioxide, aluminum oxide, zirconium dioxide, etc. The use of silicon dioxide and its derivatives on the surface of magnetic nanoparticles may help improve their surface properties, and because silicon dioxide is an inert compound, it can provide good acid and alkali resistance and high temperature stability. At the same time, silicon dioxide has high transmittance in the ultraviolet light region, so it can be used in anti-reflection materials, and combined with ferrosoferric oxide can achieve stronger electromagnetic loss performance.
[0004] For example, CN102807775B discloses a method for preparing waterproof and oil-proof magnetic SiO2 / Fe3O4 composite particles, comprising: dissolving FeCl2·4H2O, Na2SO3, polyvinyl pyrrolidone and NaOH in deionized water, reacting at 100°C to 180°C for 8h to 16h, and obtaining Fe3O4 particles after separation, washing and drying; uniformly dispersing Fe3O4 particles in ethanol, adding ammonia water, adding tetraethyl orthosilicate while stirring, and continuing to stir at 5°C to 50°C for 8h to 16h, and obtaining waterproof and oil-proof magnetic SiO2 / Fe3O4 composite particles after separation, washing and drying, and preparing products by encapsulating fluorosilane to improve performance, with simple production process, strong production feasibility and high yield. The waterproof and oil-proof magnetic SiO2 / Fe3O4 composite particles or products of the present invention have good waterproof and oil-proof properties and can be widely used in coatings, medical machinery, steel corrosion protection and the like.
[0005] Such as CN109627906B a kind of super-hydrophobic graphene anticorrosion coating of double-layer intermixed structure and preparation method thereof, belong to super-hydrophobic anticorrosion coating technical field, can solve the current super-hydrophobic coating structure and performance instability, super-hydrophobic coating anticorrosion performance is poor, and can not be prepared on a large scale and other problems. The present invention comprises the following steps: first, synthesize a kind of nanoparticle oily dispersion with low surface energy, and graphene / resin composite oily dispersion with good dispersibility;Secondly, graphene / resin composite oily dispersion and nanoparticle oily dispersion are sprayed on metal substrate successively, and the coating of double-layer intermixed structure is prepared. Relative to traditional super-hydrophobic anticorrosion coating, hydrophobicity and anticorrosion performance are more excellent, surface structure and performance are more stable, and can be prepared in a large area, accelerate the engineering application of super-hydrophobic coating in anticorrosion field. Summary of the invention
[0006] The present invention provides a method for preparing a two-component water-based paint, comprising preparing corrosion-resistant cadmium-doped Fe3O4 nanosphere particles under harsh (extremely high temperature) hydrothermal conditions, then obtaining high-purity magnetic particles by acid washing, activation and impurity removal, and using the magnetic nanospheres as cores to directionally adsorb silicon oxide shells on their surfaces to obtain a highly suspended, highly compatible and stable magnetic suspension. When used as a filler for water-based paints, the filler is highly dispersed in the coating, and the coating has good physical and chemical properties, such as tensile strength and corrosion resistance.
[0007] A method for preparing a two-component water-based paint filler comprises the following steps:
[0008] (1) Add 5-8mM FeCl3 . 6H2O, 0.5-1 mM CdCl2 .6H2O metal salt is added to an ethanol-deionized water solution, and after stirring evenly, 3-4 g / L tetrahydroxypropylethylenediamine and 1-2 g / L ethylenediaminetetraacetic acid composite complexing agent are added in sequence, and then 0.02-0.04 g / L 2,2'-bipyridine is added as a stabilizer, 10-15 mL NaBH4 is added as a reducing agent, and stirred evenly, and then sodium acetate is used as an alkali source to adjust the pH to 7.5-8.5 to obtain a precursor solution;
[0009] (2) Place the above precursor solution in an unlined stainless steel hydrothermal reactor, use nitrogen to exhaust the air in the reactor, then seal the reactor, heat it to 300-310°C at 5-10°C / min, keep it warm for 24-48 hours, and cool it naturally to room temperature.
[0010] (3) Magnetic separation of hydrothermal products, and activation and acid washing purification: The activation and acid washing purification is to place the magnetic separation hydrothermal products in a mixed solution of 98wt.% H2SO4 and 30wt.% H2O2 in a volume ratio of 1-2:1 for 2-3 minutes at a temperature of 30°C and stirring with a motor. After activation and acid washing purification, the products are repeatedly washed with deionized water and ethanol in sequence until they are neutral, and a 10-20wt.% magnetic particle suspension is prepared. The solvent of the suspension is composed of a polyether-modified silicone wetting agent, ethanol and deionized water.
[0011] (4) Add ammonia water to the magnetic particle suspension prepared in step (3), stir for 10-20 minutes, add ethyl silicate, stir with a motor for 12-14 hours at a temperature of 10-14°C, then filter and wash the product, and vacuum dry it to obtain (Cd-Fe)O x @SiO2 filler.
[0012] In certain embodiments, the content of the polyether-modified silicone wetting agent is 4-5 wt.%.
[0013] In certain embodiments, the volume ratio of ethanol to deionized water in step (1) and step (3) is 1:7-9.
[0014] In some embodiments, the saturation magnetic intensity of the magnetic particles after the activation and acid washing purification in step (3) is 62.7emu / g, the remanence is 4.23emu / g, and the coercive force is Hc=41.8G.
[0015] In certain embodiments, (Cd—Fe)O x @The saturation magnetic intensity of SiO2 filler is 25.3 emu / g.
[0016] In certain embodiments, the amount of ethyl silicate used is 3-4 g, and the amount of ammonia water used is 5-8 mL.
[0017] In certain embodiments, (Cd—Fe)O x The size of the core is 20-70 nm, and the thickness of the SiO2 shell is 10-30 nm.
[0018] In certain embodiments, the (Cd—Fe)O x @SiO2 filler is ultrasonically dispersed in deionized water containing a wetting agent, (Cd-Fe)O x @The mass concentration of SiO2 is 40-50wt%, and the mass concentration of the wetting agent is 1-2wt.%.
[0019] A method for preparing a two-component water-based coating comprises the following steps:
[0020] (A) Preparation method of component A: After the water-based hydroxy acrylic resin, wetting dispersant, defoamer, leveling agent and deionized water are uniformly stirred according to the formula, the filler suspension is added and mixed at a high speed of 800-1200 rpm, and then the cosolvent and thixotropic thickener are added and mixed at a medium speed of 600-800 rpm.
[0021] (B) Preparation method of component B: fully mix the hydrophilic modified isocyanate curing agent and propylene glycol diacetate to prepare the component.
[0022] (C) When in use, component A and component B are mixed evenly in a mass ratio of (5.5-10):1, and then sprayed on the surface of the substrate.
[0023] The filler suspension is prepared by the following steps.
[0024] (1) Add 5-8mM FeCl3 . 6H2O, 0.5-1 mM CdCl2 . 6H2O metal salt is added to an ethanol-deionized water solution, and after stirring evenly, 3-4 g / L tetrahydroxypropylethylenediamine and 1-2 g / L ethylenediaminetetraacetic acid composite complexing agent are added in sequence, and then 0.02-0.04 g / L 2,2'-bipyridine is added as a stabilizer, 10-15 mL NaBH4 is added as a reducing agent, and stirred evenly, and then sodium acetate is used as an alkali source to adjust the pH to 7.5-8.5 to obtain a precursor solution;
[0025] (2) Place the above precursor solution in an unlined stainless steel hydrothermal reactor, use nitrogen to exhaust the air in the reactor, then seal the reactor, heat it to 300-310°C at 5-10°C / min, keep it warm for 24-48 hours, and cool it naturally to room temperature.
[0026] (3) Magnetic separation of hydrothermal products, and activation and acid washing purification: The activation and acid washing purification is to place the magnetic separation hydrothermal products in a mixed solution of 98wt.% H2SO4 and 30wt.% H2O2 in a volume ratio of 1-2:1 for 2-3 minutes at a temperature of 30°C and stirring with a motor. After activation and acid washing purification, the products are repeatedly washed with deionized water and ethanol in sequence until they are neutral, and a 10-20wt.% magnetic particle suspension is prepared. The solvent of the suspension is composed of a polyether-modified silicone wetting agent, ethanol and deionized water.
[0027] (4) Add ammonia water to the magnetic particle suspension prepared in step (3), stir for 10-20 minutes, add ethyl silicate, stir with a motor for 12-14 hours at a temperature of 10-14°C, then filter and wash the product, and vacuum dry it to obtain (Cd-Fe)O x @SiO2 filler, the (Cd-Fe)O x @SiO2 filler is ultrasonically dispersed in deionized water containing a wetting agent to obtain a filler suspension, (Cd-Fe)O x @The mass concentration of SiO2 is 40-50wt%, and the mass concentration of the wetting agent is 1-2wt.%.
[0028] A water-based two-component polyurethane coating comprises a component A and a component B; the mass ratio of the component A to the component B is (5.5-10):1.
[0029] The component A comprises the following components in parts by weight: 40 to 65 parts of waterborne hydroxy acrylic resin, 0.5 to 3 parts of wetting and dispersing agent, 0.5 to 3 parts of defoaming agent, 5 to 10 parts of cosolvent, 10 to 25 parts of filler suspension, 0.5 to 3 parts of leveling agent, 0.5 to 5 parts of thixotropic thickener, and 15 to 25 parts of deionized water;
[0030] The B component includes the following components in parts by mass: 60-80 parts of a hydrophilic modified isocyanate curing agent and 10-15 parts of propylene glycol diacetate.
[0031] The wetting and dispersing agent is selected from at least one of TEGO 4100, TEGO 755W, and BYK-190; the defoaming agent is selected from at least one of BYK022, BYK093, TEGO Airex 901W, and TEGO Foamex 810.
[0032] The co-solvent is selected from at least one of propylene glycol methyl ether, ethylene glycol butyl ether and dipropylene glycol methyl ether.
[0033] The leveling agent is selected from at least one of TEGO-450, BYK-381, TEGO Glide 410, and TEGO Glide 4100; and the thixotropic thickener is selected from at least one of Borchi 0620 and RHEOLATE 299.
[0034] The present invention adopts a hydrothermal method to prepare magnetic nano-Fe3O4, which refers to using water and ethanol as hydrothermal reaction media, reacting in a closed inert atmosphere reactor at a high temperature of 300-310°C and a high pressure of approximately 20-40Mpa. The hydrothermal filling degree here is 40-80%, preferably 75%. At 310°C, the pressure inside the reactor is approximately 32MPa. During the reaction, FeCl3 . 6H2O and CdCl2 . 6H2O is used as the metal source, and the two-component composite complexing agent with tetrahydroxypropylethylenediamine and ethylenediaminetetraacetic acid EDTA can effectively complex iron and cadmium ions, shorten the distance between the two, and facilitate the formation of an alloy structure. Then 2,2'-bipyridine is added as a stabilizer to stabilize the metal ion state, and then NaBH4 is used as a reducing agent to reduce part of Fe 3+ Fe 2+ , and Cd 2+ Cd is reduced, sodium acetate is used as an alkali source, and after dehydration, cadmium-doped Fe3O4 magnetic particles are generated. Under extremely high hydrothermal temperature and pressure conditions, the saturation magnetic intensity of the cadmium-doped Fe3O4 magnetic particles obtained is reduced, but compared with Fe3O4 or other FeO X Or CdO has extremely high corrosion resistance. Based on the above properties, Fe3O4, FeO X Or CdO is used for impurity removal, and the magnetic particles obtained after purification are high-purity cadmium-doped Fe3O4 magnetic particles. At the same time, in order to prepare a magnetic core-shell structure, it is necessary to introduce active groups on the surface of the above-mentioned cadmium-doped Fe3O4 magnetic nanoparticles. The active groups are mainly hydroxyl groups. Sulfuric acid will react with excess, easily corroded FeOx and CdO. The purified high-purity cadmium-doped Fe3O4 magnetic particles undergo the following reaction in sulfuric acid and hydrogen peroxide: H2SO4+H2O2→H3O + +HSO4 - +O, to achieve hydroxylation on the surface of cadmium-doped Fe3O4 magnetic particles. During the purification and activation process, it should be noted that the acquisition time should not be longer than 4 minutes to avoid excessive corrosion.
[0035] Then, silicon oxide is directional adsorbed on the surface of Fe3O4 magnetic particles doped with cadmium hydroxylate. The directional adsorption mechanism is: alkaline conditions are selected, and ammonia water is used to provide hydroxide. TEOS is first hydrolyzed under alkaline conditions. The mechanism is OH -First, it undergoes a nucleophilic reaction with silicon nuclei to generate silanol, and hydrogen bonds are formed between the hydroxyl groups of the silanol and the hydroxyl groups on the surface of the cadmium-doped Fe3O4 magnetic particles. Then, further condensation occurs on the basis of hydrogen bond bridging. At the same time, silanol is dehydrogenated under alkaline conditions to form a Lewis base, which continues to react with other silicon nuclei and dehydrates (or dealcoholizes) to polymerize, slowly generating a network structure, and finally forming a SiO2 film on the surface of the cadmium-doped Fe3O4 magnetic particles.
[0036] See attached Figure 1 From the energy spectrum, it can be seen that the cadmium-doped Fe3O4 magnetic particles-SiO2 exist in the form of core-shell, wherein the cadmium-doped Fe3O4 is the core with a size of 54nm, and the silicon oxide is the shell with a shell size of 26nm. The magnetic nanoparticles are highly evenly dispersed in the coating without obvious agglomeration. See the attached Figure 2 .
[0037] Beneficial technical effects
[0038] (1) The present invention first prepares relatively corrosion-resistant cadmium-doped Fe3O4 magnetic particles, and then effectively purifies the components of the magnetic particles through an acid washing and activation step, while simultaneously introducing hydroxyl groups on their surface.
[0039] (2) By introducing hydroxyl groups in a directional manner, a slightly thorny silicon oxide coating is coated on the surface of the magnetic particle filler, which can significantly increase the (Cd-Fe)O x @SiO2 filler is soluble in water and highly dispersed in the polyurethane coating. It has good coating compatibility and significantly improves the physical and chemical properties of polyurethane, such as tensile strength.
[0040] (3) By introducing hydroxyl groups in a directional manner, a slightly thorny silicon oxide coating is coated on the surface of the magnetic particle filler, and the coating improves the (Cd-Fe)O x The chemical stability of the coating can be improved, especially the corrosion resistance of the coating and the service life of the magnetic coating can be increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Attached Figure 1 (Cd-Fe)O x @Energy spectrum of SiO2 filler.
[0042] Attached Figure 2 (Cd-Fe)O x @Dispersion diagram of SiO2 filler in polyurethane. DETAILED DESCRIPTION Example 1
[0043] A method for preparing a two-component water-based paint filler comprises the following steps:
[0044] (1) Add 6.5 mM FeCl3. 6H2O, 0.75 mM CdCl2 . 6H2O metal salt is added to an ethanol-deionized water solution, the volume ratio of ethanol to deionized water is 1:8, and after stirring evenly, 3.5g / L tetrahydroxypropylethylenediamine and 1.5g / L ethylenediaminetetraacetic acid composite complexing agent are added in sequence, and then 0.03g / L 2,2'-bipyridine is added as a stabilizer, 12.5mL NaBH4 is added as a reducing agent, and stirred evenly, and then sodium acetate is used as an alkali source, and the pH is adjusted to 8 to obtain a precursor solution;
[0045] (2) placing the above precursor solution in an unlined stainless steel hydrothermal reactor, exhausting the air in the reactor with nitrogen, and then sealing the reactor, heating it to 305°C at a rate of 7.5°C / min, keeping it at that temperature for 36 hours, and cooling it naturally to room temperature;
[0046] (3) Magnetic separation of hydrothermal products, and activation and acid washing purification: The activation and acid washing purification is to place the magnetic separation hydrothermal products in a mixed solution of 98wt.% H2SO4 and 30wt.% H2O2 in a volume ratio of 1.5:1 for 2.5 minutes at a temperature of 30°C and motor stirring. After activation and acid washing purification, the products are repeatedly washed with deionized water and ethanol in sequence until they are neutral. The saturation magnetic intensity of the magnetic particles after activation and acid washing purification is 62.7 emu / g, the remanence is 4.23emu / g, and the coercive force is Hc=41.8G. A 15wt.% magnetic particle suspension is prepared. The solvent of the suspension is composed of 4.5wt.% polyether-modified siloxane wetting agent, ethanol and deionized water. The volume ratio of ethanol to deionized water is 1:8.
[0047] (4) Add 6.5 mL of aqueous ammonia to the magnetic particle suspension prepared in step (3), stir for 15 min, add 3.5 g of ethyl silicate, stir for 13 h with a motor at 12 °C, then filter, wash, and vacuum dry the product to obtain (Cd-Fe)O x @SiO2 filler, (Cd-Fe)O x @The saturation magnetic intensity of SiO2 filler is 25.3 emu / g.
[0048] The (Cd-Fe)O x @SiO2 filler is ultrasonically dispersed in deionized water containing a wetting agent, (Cd-Fe)O x @The mass concentration of SiO2 is 45wt%, the mass concentration of the wetting agent is 1.5wt.%, and the filler suspension obtained is.
[0049] Comparative Example 1
[0050] A method for preparing a two-component water-based paint filler comprises the following steps:
[0051] (1) Add 6.5 mM FeCl3 . 6H2O, 0.75 mM CdCl2 . 6H2O metal salt was added to an ethanol-deionized water solution, the volume ratio of ethanol to deionized water was 1:8, and after stirring evenly, 5g / L tetrahydroxypropylethylenediamine and 12.5mLNaBH4 were added in sequence as a reducing agent, and stirred evenly. Then, sodium acetate was used as an alkali source, and the pH was adjusted to 8 to obtain a precursor solution.
[0052] (2) The precursor solution was placed in an unlined stainless steel hydrothermal reactor, and the air in the reactor was exhausted with nitrogen. The reactor was then sealed and heated to 230°C at a rate of 7.5°C / min, kept at this temperature for 36 h, and then naturally cooled to room temperature.
[0053] (3) Magnetic separation of hydrothermal products, and activation and acid washing purification: The activation and acid washing purification is to place the magnetic separation hydrothermal products in a mixed solution of 98wt.% H2SO4 and 30wt.% H2O2 in a volume ratio of 1.5:1 for 2.5 minutes at a temperature of 30°C and stirring with a motor. After activation and acid washing purification, the products are repeatedly washed with deionized water and ethanol in sequence until neutral, and a 15wt.% magnetic particle suspension is prepared. The solvent of the suspension is composed of 4.5wt.% polyether-modified siloxane wetting agent, ethanol and deionized water, and the volume ratio of ethanol to deionized water is 1:8.
[0054] (4) Add 6.5 mL of aqueous ammonia to the magnetic particle suspension prepared in step (3), stir for 15 min, add 3.5 g of ethyl silicate, stir for 13 h with a motor at 12 °C, then filter, wash, and vacuum dry the product to obtain (Cd-Fe)O x @SiO2 filler.
[0055] The (Cd-Fe)O x @SiO2 filler is ultrasonically dispersed in deionized water containing a wetting agent, (Cd-Fe)O x @The mass concentration of SiO2 is 45wt%, and the mass concentration of the wetting agent is 1.5wt.%.
[0056] Comparative Example 2
[0057] A method for preparing a two-component water-based paint filler comprises the following steps:
[0058] (1) Add 6.5 mM FeCl3 .6H2O and metal salt are added to an ethanol-deionized water solution, the volume ratio of ethanol to deionized water is 1:8, and after stirring evenly, 3.5g / L tetrahydroxypropylethylenediamine and 1.5g / L ethylenediaminetetraacetic acid composite complexing agent are added in sequence, and then 0.03g / L 2,2'-bipyridine is added as a stabilizer and 12.5mL NaBH4 is added as a reducing agent, and stirred evenly. Then, sodium acetate is used as an alkali source, and the pH is adjusted to 8 to obtain a precursor solution.
[0059] (2) The precursor solution was placed in an unlined stainless steel hydrothermal reactor, and the air in the reactor was exhausted with nitrogen. The reactor was then sealed and heated to 305°C at a rate of 7.5°C / min, kept at this temperature for 36 h, and then naturally cooled to room temperature.
[0060] (3) Magnetic separation of hydrothermal products, and activation and acid washing purification: The activation and acid washing purification is to place the magnetic separation hydrothermal products in a mixed solution of 98wt.% H2SO4 and 30wt.% H2O2 in a volume ratio of 1.5:1 for 2.5 minutes at a temperature of 30°C and stirring with a motor. After activation and acid washing purification, the products are repeatedly washed with deionized water and ethanol in sequence until neutral, and a 15wt.% magnetic particle suspension is prepared. The solvent of the suspension is composed of 4.5wt.% polyether-modified siloxane wetting agent, ethanol and deionized water, and the volume ratio of ethanol to deionized water is 1:8.
[0061] (4) Add 6.5 mL of aqueous ammonia to the magnetic particle suspension prepared in step (3), stir for 15 min, add 3.5 g of ethyl silicate, stir for 13 h with a motor at 12 °C, then filter, wash, and vacuum dry the product to obtain (Cd-Fe)O x @SiO2 filler.
[0062] The (Cd-Fe)O x @SiO2 filler is ultrasonically dispersed in deionized water containing a wetting agent, (Cd-Fe)O x @The mass concentration of SiO2 is 45wt%, and the mass concentration of the wetting agent is 1.5wt.%.
[0063] Comparative Example 3
[0064] A method for preparing a two-component water-based paint filler comprises the following steps:
[0065] (1) Add 6.5 mM FeCl3 . 6H2O, 0.75 mM CdCl2 .6H2O metal salt was added to an ethanol-deionized water solution, the volume ratio of ethanol to deionized water was 1:8, and after stirring evenly, 3.5 g / L tetrahydroxypropylethylenediamine and 1.5 g / L ethylenediaminetetraacetic acid composite complexing agent were added in sequence, and then 0.03 g / L 2,2'-bipyridine was added as a stabilizer and 12.5 mL NaBH4 was added as a reducing agent, and stirred evenly. Then, sodium acetate was used as an alkali source, and the pH was adjusted to 8 to obtain a precursor solution.
[0066] (2) The precursor solution was placed in an unlined stainless steel hydrothermal reactor, and the air in the reactor was exhausted with nitrogen. The reactor was then sealed and heated to 305°C at a rate of 7.5°C / min, kept at this temperature for 36 h, and then naturally cooled to room temperature.
[0067] (3) Magnetic separation of hydrothermal products: preparing a 15 wt.% magnetic particle suspension, wherein the solvent of the suspension consists of 4.5 wt.% polyether-modified siloxane wetting agent, ethanol and deionized water, and the volume ratio of ethanol to deionized water is 1:8.
[0068] (4) Add 6.5 mL of aqueous ammonia to the magnetic particle suspension prepared in step (3), stir for 15 min, add 3.5 g of ethyl silicate, stir for 13 h with a motor at 12 °C, then filter, wash, and vacuum dry the product to obtain (Cd-Fe)O x @SiO2 filler.
[0069] The (Cd-Fe)O x @SiO2 filler is ultrasonically dispersed in deionized water containing a wetting agent, (Cd-Fe)O x @The mass concentration of SiO2 is 45wt%, the mass concentration of the wetting agent is 1.5wt.%, and the filler suspension obtained is.
[0070] There is no substantial difference between the preparation process of Example 1 and Comparative Examples 1-3. The main difference is that there is no complexing agent and stabilizer in Comparative Document 1, no cadmium salt in Comparative Document 2, and no activation step in Comparative Document 3. After the hydrothermal products of magnetic separation in step (3) of Example 1 and Comparative Examples 1-3 were vacuum dried, a corrosion test was performed. Samples of equal mass were immersed in a 5wt.% saline solution for 15 minutes. The corrosion rates of Example 1 and Comparative Examples 1-3 were 93.5wt.%, 78.5wt.%, 80.2wt.%, and 93.4wt.%, respectively. The corrosion efficiency was further tested for 30 minutes. The corrosion rates of Example 1 and Comparative Examples 1-3 are 91.2wt.%, 65.5wt.%, 66.2wt.%, and 91.3wt.%, respectively. There is no essential difference in the corrosion rate of Example 1 at 15min and 30min, which clearly proves that the product is a corrosion-resistant magnetic particle. The corrosion resistance of the magnetic material comes from cadmium doping under high temperature and high pressure hydrothermal conditions. Under the same conditions, if no complexing agent and stabilizer are added in Comparative Example 1, the hydrothermal temperature is low, and the corrosion efficiency is high, which is attributed to the formation of no alloy. The corrosive substances are iron oxides and cadmium oxides, and the effect is similar to that of Comparative Example 2 without adding cadmium salt. In addition, Comparative Example 3 is not essentially different from Example 1 because the treatment steps before activation are similar. Example 2
[0071] The suspensions prepared in Example 1 and Comparative Example 3 were used as fillers for polyurethane.
[0072] A method for preparing a two-component water-based coating.
[0073] (A) Preparation method of component A: After the water-based hydroxy acrylic resin, wetting dispersant, defoamer, leveling agent and deionized water are stirred evenly according to the formula amount, the filler suspension is added and stirred at a high speed of 1000 rpm to mix evenly, and then the co-solvent and thixotropic thickener are added and mixed at a medium speed of 700 rpm to mix evenly.
[0074] (B) Preparation method of component B: fully mix the hydrophilic modified isocyanate curing agent and propylene glycol diacetate to prepare the component.
[0075] (C) When in use, component A and component B are mixed evenly in a mass ratio of (7.5):1, and then sprayed on the surface of the substrate. Example 3
[0076] A water-based two-component polyurethane coating comprises a component A and a component B; the mass ratio of the component A to the component B is 7.5:1.
[0077] The component A comprises the following components in parts by weight: 52 parts of water-based hydroxy acrylic resin, 1.5 parts of wetting and dispersing agent, 1.5 parts of defoaming agent, 7.5 parts of cosolvent, 20 parts of filler suspension, 1.5 parts of leveling agent, 2.5 parts of thixotropic thickener, and 20 parts of deionized water;
[0078] The B component includes the following components in parts by mass: 70 parts of a hydrophilic modified isocyanate curing agent and 12.5 parts of propylene glycol diacetate.
[0079] The wetting and dispersing agent is selected from BYK-190.
[0080] The defoamer is selected from BYK093.
[0081] The cosolvent is selected from ethylene glycol butyl ether.
[0082] The leveling agent is selected from TEGO Glide 4100.
[0083] The thixotropic thickener is selected from RHEOLATE 299.
[0084] The suspension prepared in Example 1 was used as the filler of polyurethane.
[0085] Comparative Example 4
[0086] A water-based two-component polyurethane coating comprises a component A and a component B; the mass ratio of the component A to the component B is 7.5:1.
[0087] The component A comprises the following components in parts by weight: 52 parts of water-based hydroxy acrylic resin, 1.5 parts of wetting and dispersing agent, 1.5 parts of defoaming agent, 7.5 parts of cosolvent, 20 parts of filler suspension, 1.5 parts of leveling agent, 2.5 parts of thixotropic thickener, and 20 parts of deionized water;
[0088] The B component includes the following components in parts by mass: 70 parts of a hydrophilic modified isocyanate curing agent and 12.5 parts of propylene glycol diacetate.
[0089] The wetting and dispersing agent is selected from BYK-190.
[0090] The defoamer is selected from BYK093.
[0091] The cosolvent is selected from ethylene glycol butyl ether.
[0092] The leveling agent is selected from TEGO Glide 4100.
[0093] The thixotropic thickener is selected from RHEOLATE 299.
[0094] The suspension prepared in Comparative Example 3 is used as a filler for polyurethane.
[0095] Comparative Example 5
[0096] A water-based two-component polyurethane coating comprises a component A and a component B; the mass ratio of the component A to the component B is (7.5):1.
[0097] The component A comprises the following components in parts by weight: 52 parts of water-based hydroxy acrylic resin, 1.5 parts of wetting and dispersing agent, 1.5 parts of defoaming agent, 7.5 parts of cosolvent, 20 parts of filler suspension, 1.5 parts of leveling agent, 2.5 parts of thixotropic thickener, and 20 parts of deionized water;
[0098] The B component includes the following components in parts by mass: 70 parts of a hydrophilic modified isocyanate curing agent and 12.5 parts of propylene glycol diacetate.
[0099] The wetting and dispersing agent is selected from BYK-190.
[0100] The defoamer is selected from BYK093.
[0101] The cosolvent is selected from ethylene glycol butyl ether.
[0102] The leveling agent is selected from TEGO Glide 4100.
[0103] The thixotropic thickener is selected from RHEOLATE 299.
[0104] The filler suspension preparation process is as follows: It includes the following steps:
[0105] (1) Add 6.5 mM FeCl3 . 6H2O, 0.75 mM CdCl2 . 6H2O metal salt is added to an ethanol-deionized water solution, the volume ratio of ethanol to deionized water is 1:8, and after stirring evenly, 3.5g / L tetrahydroxypropylethylenediamine and 1.5g / L ethylenediaminetetraacetic acid composite complexing agent are added in sequence, and then 0.03g / L 2,2'-bipyridine is added as a stabilizer, 12.5mL NaBH4 is added as a reducing agent, and stirred evenly, and then sodium acetate is used as an alkali source, and the pH is adjusted to 8 to obtain a precursor solution;
[0106] (2) placing the above precursor solution in an unlined stainless steel hydrothermal reactor, exhausting the air in the reactor with nitrogen, and then sealing the reactor, heating it to 305°C at a rate of 7.5°C / min, keeping it at that temperature for 36 hours, and cooling it naturally to room temperature;
[0107] (3) Magnetic separation of hydrothermal products and activation and acid washing purification: The activation and acid washing purification is to place the magnetic separation hydrothermal products in a mixed solution of 98wt.% H2SO4 and 30wt.% H2O2 in a volume ratio of 1.5:1 for 2.5 minutes at a temperature of 30°C and with motor stirring. After activation and acid washing purification, the products are repeatedly washed with deionized water and ethanol in sequence until they are neutral.
[0108] The (Cd-Fe)O x The filler was ultrasonically dispersed in deionized water containing a wetting agent, the mass concentration of (Cd-Fe)O was 45 wt%, and the mass concentration of the wetting agent was 1.5 wt.%, to obtain a filler suspension.
[0109]
[0110] As shown in the above table, the main difference between Example 3 and Comparative Example 4 is whether the fillers are different, and the further difference is whether the fillers have been purified and activated. The difference between Example 3 and Comparative Example 5 is whether the coating treatment is performed. The coating is applied to the surface of the metal substrate, and then the polarization potential is tested, and the corrosion current density is converted. The corrosion current density of Example 3 is significantly higher than that of Comparative Example 4 and Comparative Example 5. The difference of Comparative Example 5 mainly lies in whether it has been purified and activated. Without purification and activation, the hydrothermal product composition is more complex, and more importantly, there is no functional group on the surface, which affects the subsequent directional coating of silicon oxide. In addition, as shown in Comparative Example 5, without silicon oxide coating, the single (Cd-Fe)O x The filler has poor corrosion resistance and (Cd-Fe)O x Poor dispersibility in the coating and filler agglomeration will affect the corrosion resistance of the coating. The most direct manifestation of agglomeration is the reduction of tensile strength, as shown above.
[0111] The embodiments described above provide a detailed description of the technical solutions of the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications and improvements made within the scope of the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a two-component water-based coating, Features The steps include: (A) Preparation method of component A: After the water-based hydroxy acrylic resin, wetting dispersant, defoamer, leveling agent and deionized water are uniformly stirred according to the formula amount, the filler suspension is added and mixed at a high speed of 800-1200 rpm, and then the cosolvent and thixotropic thickener are added and mixed at a medium speed of 600-800 rpm; The component A comprises the following components in parts by weight: 40 to 65 parts of waterborne hydroxy acrylic resin, 0.5 to 3 parts of wetting and dispersing agent, 0.5 to 3 parts of defoaming agent, 5 to 10 parts of cosolvent, 10 to 25 parts of filler suspension, 0.5 to 3 parts of leveling agent, 0.5 to 5 parts of thixotropic thickener, and 15 to 25 parts of deionized water; (B) Preparation method of component B: fully mixing a hydrophilic modified isocyanate curing agent and propylene glycol diacetate; (C) When used, component A and component B are mixed evenly in a mass ratio of (5.5-10):1, and then sprayed on the surface of the substrate; The filler suspension is prepared by the following steps: (1) Add 5-8 mM FeCl 3 . 6H 2 O, 0.5-1 mM CdCl 2 . 6H 2 O metal salt is added to the ethanol-deionized water solution, stirred evenly, 3-4 g / L tetrahydroxypropylethylenediamine, 1-2 g / L ethylenediaminetetraacetic acid complexing agent are added in sequence, and then 0.02-0.04 g / L 2,2'-bipyridine is added as a stabilizer, and 10-15 mL NaBH 4 As a reducing agent, stir evenly, then use sodium acetate as an alkali source, adjust the pH to 7.5-8.5, and obtain a precursor solution; (2) placing the above precursor solution in an unlined stainless steel hydrothermal reactor, exhausting the air in the reactor with nitrogen, and then sealing the reactor, heating it to 300-310°C at 5-10°C / min, keeping it at that temperature for 24-48h, and cooling it naturally to room temperature; (3) Magnetic separation of hydrothermal products and activation acid washing purification: The activation acid washing purification is to place the magnetic separation hydrothermal products in a 98wt.%H 2 SO 4 and 30wt.%H 2 O 2 The mixture is treated in a mixed solution for 2-3 minutes at a temperature of 30°C with a motor stirring, and after activation and acid washing, it is repeatedly washed with deionized water and ethanol in sequence until it becomes neutral, and a 10-20wt.% magnetic particle suspension is prepared, wherein the solvent of the suspension is composed of a polyether-modified siloxane wetting agent, ethanol and deionized water; (4) Add ammonia water to the magnetic particle suspension prepared in step (3), stir for 10-20 minutes, add ethyl silicate, stir with a motor for 12-14 hours at a temperature of 10-14°C, then filter and wash the product, and vacuum dry it to obtain (Cd-Fe)O x @SiO 2 Filler, the (Cd-Fe)O x @SiO 2 The filler is ultrasonically dispersed in deionized water containing a wetting agent to obtain a filler suspension, (Cd-Fe)O x @SiO 2 The mass concentration is 40-50wt%, and the mass concentration of the wetting agent is 1-2wt.%.
2. A method for preparing a two-component water-based coating as claimed in claim 1, It is characterized in that The wetting and dispersing agent is selected from at least one of TEGO 4100, TEGO 755W, and BYK-190; The defoamer is selected from at least one of BYK022, BYK093, TEGO Airex 901W, and TEGO Foamex 810; and the cosolvent is selected from at least one of propylene glycol methyl ether, ethylene glycol butyl ether, and dipropylene glycol methyl ether.
3. A method for preparing a two-component water-based coating as claimed in claim 1, It is characterized in that The leveling agent is selected from at least one of TEGO-450, BYK-381, TEGO Glide 410, and TEGO Glide 4100; and the thixotropic thickener is selected from at least one of Borchi 0620 and RHEOLATE 299.
4. A method for preparing a two-component water-based coating as claimed in claim 1, Features The content of the polyether modified silicone wetting agent is 4-5wt.%.
5. A method for preparing a two-component water-based coating as claimed in claim 1, Features The volume ratio of ethanol to deionized water in step (1) and step (3) is 1:7-9.
6. A method for preparing a two-component water-based coating as claimed in claim 1, Features The amount of the ethyl silicate used is 3-4 g, and the amount of the ammonia water used is 5-8 mL.