Preparation method and application of ZnO@ZnNiCo-LDH composite material

Through the preparation of ZnO@ZnNiCo-LDH composite material, the problems of low conductivity and poor stability of existing electrode materials are solved, and the electrochemical performance of supercapacitors is improved, which is suitable for supercapacitor positive electrodes.

CN116344224BActive Publication Date: 2024-11-15NORTHEAST DIANLI UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310171718.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-28
Publication Date
2024-11-15
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

The low conductivity and poor stability of existing supercapacitor electrode materials limit their practical application in supercapacitors.

Method used

The preparation method of ZnO@ZnNiCo-LDH composite material is used to synthesize ZnO through raw materials such as zinc acetate, sodium citrate, sodium hydroxide, and other raw materials, and combine chemical substances such as 2-methylimidazole and cobalt nitrate hexahydrate to form ZnO@ZIF-8/ ZIF-67 composite was etched by nickel nitrate hexahydrate and cobalt nitrate hexahydrate to generate ZnO@ZnNiCo-LDH, increasing the conductivity and cyclic stability of the material.

Benefits of technology

It improves the conductivity and cyclic stability of the material, enhances the active site of the redox reaction, improves the electrochemical performance of the supercapacitor, has high specific capacitance and good rate performance, and is suitable for the positive electrode of the supercapacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116344224B_ABST
    Figure CN116344224B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a ZnO@ZnNiCo‑LDH composite material, which uses zinc acetate, sodium citrate and sodium hydroxide as raw materials, synthesizes ZnO solid by stirring, then uses ZnO solid as a zinc source, Co(NO3)2·6H2O as a cobalt source, 2‑methylimidazole as a ligand, and oil bath heating to obtain ZnO@ZIF‑8 / ZIF‑67, and then uses Co(NO3)2·6H2O and Ni(NO3)2·6H2O cobalt etching to obtain the ZnO@ZnNiCo‑LDH composite material. An application is also provided for use in a supercapacitor positive electrode. The composite material prepared by the present invention has high specific capacitance, good rate performance and cycle stability, and can be widely used in a supercapacitor positive electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of supercapacitor electrode materials, and specifically relates to a preparation method and application of a ZnO@ZnNiCo-LDH composite material. Background Art

[0002] Supercapacitors, also known as electrochemical capacitors, are a new type of component that stores energy through the interfacial double layer formed between electrodes and electrolytes. Their capacitance far exceeds that of ordinary capacitor devices. In addition, supercapacitors have many unique advantages, such as fast charging speed, which can be completed in a very short time, strong discharge capacity and high energy conversion efficiency; long service life, high safety factor and large temperature range, but the low energy density limits the large-scale use of supercapacitors. Electrode materials play a decisive role in the performance of supercapacitors. Designing and manufacturing electrode materials with special structures can improve the energy density of supercapacitors while maintaining other properties, thereby preparing supercapacitors with higher performance, which is a significant task. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a preparation method and application of a ZnO@ZnNiCo-LDH composite material in view of the deficiencies of the above-mentioned prior art. The ZnO@ZnNiCo-LDH composite material has high specific capacitance, good rate performance and cycle stability, and can be widely used in supercapacitor positive electrodes.

[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a ZnO@ZnNiCo-LDH composite material, the method comprising:

[0005] S1. Mix zinc acetate and deionized water, perform ultrasonic treatment for 15 to 30 minutes and magnetic stirring for 30 to 40 minutes to obtain solution A, add sodium citrate to the solution A, perform magnetic stirring for 30 to 40 minutes to obtain solution B; add sodium hydroxide to the solution B while stirring, perform magnetic stirring for 2 hours to obtain solution C;

[0006] S2, after centrifuging the solution C obtained in S1, the precipitate is washed with deionized water for 2 to 3 times, then washed with anhydrous ethanol for 2 to 3 times, and dried under vacuum drying conditions at a temperature of 60°C to 70°C for 12h to 24h to obtain a white powder, i.e. ZnO solid;

[0007] S3, dispersing the ZnO solid obtained in S2 in deionized water, and stirring evenly with a magnetic force to obtain a solution D; dispersing 2-methylimidazole in DMF and stirring evenly with a magnetic force to obtain a solution E; mixing the solution D and the solution E, and stirring and mixing them in an oil bath at a temperature of 70° C. to 90° C. for 10 h to 20 h to obtain a solution F;

[0008] S4, after centrifuging the solution F obtained in S3, the precipitate was washed with DMF for 2 to 3 times, and then washed with anhydrous ethanol for 2 to 3 times, and dried under vacuum drying conditions at a temperature of 60°C to 70°C for 12h to 24h to obtain a milky white powder, namely ZnO@ZIF-8;

[0009] S5. Disperse the ZnO@ZIF-8 obtained in S4 in methanol a, ultrasonically disperse for 15 minutes, and then add Co(NO3)2·6H2O while stirring to obtain solution G; disperse 2-methylimidazole in methanol b, and stir evenly by magnetic stirring to obtain solution H; add the solution H to the solution G, stir for 30 minutes, and then centrifuge. Wash the precipitate with methanol for 2 to 3 times, and dry it under vacuum drying conditions at a temperature of 60°C to 70°C for 12h to 24h to obtain a purple powder, namely ZnO@ZIF-8 / ZIF-67;

[0010] S6. Disperse the ZnO@ZIF-8 / ZIF-67 obtained in S5 in ethanol, stir and mix for 30 minutes to obtain solution I, add Co(NO3)2·6H2O and Ni(NO3)2·6H2O to the solution I while stirring to obtain a mixed solution J, then add hexamethylenetetramine and stir evenly to obtain a solution K, heat and reflux at 80°C for 1 hour, cool to room temperature, and centrifuge. Wash the precipitate with deionized water for 2 to 3 times, then wash with anhydrous ethanol for 2 to 3 times, and dry under vacuum drying conditions at 60°C to 70°C for 12 to 24 hours to obtain a light green powder, which is the ZnO@ZnNiCo-LDH composite material.

[0011] Preferably, the dosage ratio of zinc acetate, deionized water, sodium citrate and sodium hydroxide in S1 is 1.5 g:60 mL:4.514 g:1 g.

[0012] Preferably, the rotation speed of the magnetic stirring in S1 is 400 r / min to 600 r / min.

[0013] Preferably, the centrifugal speeds of S2, S4, S5 and S6 are all 3000 r / min to 8000 r / min, and the centrifugal time is all 3 min to 5 min.

[0014] Preferably, the usage ratio of the ZnO solid, deionized water, 2-methylimidazole and DMF in S3 is 0.25 g:24 mL:4 g:72 mL.

[0015] Preferably, the magnetic stirring time in S3 is 10 min to 20 min, and the magnetic stirring speed is 300 r / min to 500 r / min.

[0016] Preferably, the usage ratio of ZnO@ZIF-8, methanol a, Co(NO3)2·6H2O, 2-methylimidazole and methanol b in S5 is 0.5 g:30 mL:0.9 g:3.28 g:100 mL.

[0017] Preferably, the usage ratio of ZnO@ZIF-8 / ZIF-67, ethanol, Co(NO3)2·6H2O, Ni(NO3)2·6H2O and hexamethylenetetramine in S6 is 80 mg:100 mL:200 mg:200 mg:120 mg.

[0018] The present invention also provides application of the ZnO@ZnNiCo-LDH composite material prepared as above, wherein the ZnO@ZnNiCo-LDH composite material is applied in a positive electrode of a supercapacitor.

[0019] Transition metal hydroxides are typical pseudocapacitive materials. The type of metal hydroxide that has been studied more in supercapacitors is layered metal hydroxide LDH. LDH is a material with a layered structure, which is composed of two or more metal hydroxides, in which metal cations can be flexibly combined. In addition, the anions in LDH have a high exchange capacity and can enter the interlayer space of LDH through the exchange process. Transition metal oxides have good thermal stability and chemical stability, and are easy to synthesize, moderate in cost, abundant in reserves, and environmentally friendly. Commonly used transition metal oxides include MnO2, ZnO, etc.

[0020] As a supercapacitor electrode material, ZnCoNi-LDH has the advantages of high specific capacitance and high energy density, but its low conductivity and poor stability limit its practical application in supercapacitors.

[0021] Transition metal oxides can serve as a good conductive substrate to reduce the stacking of LDH layers during the charge and discharge process, thereby effectively improving the conductivity and cycle performance of ZnCoNi-LDH. Therefore, a preparation method of ZnO@ZnNiCo-LDH composite materials is proposed.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] The invention uses zinc acetate, sodium citrate and sodium hydroxide as raw materials, synthesizes ZnO by stirring, then uses ZnO as a zinc source, cobalt nitrate hexahydrate as a cobalt source, and 2-methylimidazole as a ligand, and heats in an oil bath at 70°C to obtain a ZnO@ZIF-8 / ZIF-67 complex, and then uses nickel nitrate hexahydrate and cobalt nitrate hexahydrate to etch the ZnO@ZIF-8 / ZIF-67 complex to generate ZnO@ZnNiCo-LDH. The material forms a lamellar LDH on the surface of the oxide microsphere while maintaining the spherical morphology of ZnO. The electrode material with this morphology has a large specific surface area, and increases the oxidation reduction rate. The introduction of ZnO reduces the stacking of LDH layers and improves the overall conductivity of the material. It also improves the cycle stability of the material, which has great application value for the electrochemical performance of supercapacitors. The preparation method is simple, the reaction conditions are mild, and the equipment requirements are low, which is conducive to reducing costs. By adjusting the amount of ZnO added, ZnO@ZnNiCo-LDH composite materials with different proportions can be prepared. The prepared ZnO@ZnNiCo-LDH composite materials have high specific capacitance, good rate performance and cycle stability, and can be widely used in supercapacitor positive electrodes.

[0024] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the XRD pattern of the ZnO@ZnNiCo-LDH composite material prepared in Example 1 of the present invention and the corresponding standard card.

[0026] Figure 2 This is the SEM image of the ZnO@ZnNiCo-LDH composite material prepared in Example 1 of the present invention.

[0027] Figure 3 This is the nitrogen adsorption-desorption isotherm curve of the ZnO@ZnNiCo-LDH composite material prepared in Example 1 of the present invention.

[0028] Figure 4 Cyclic voltammograms of the ZnO@ZnNiCo-LDH composite material prepared in Example 1 of the present invention at different scan rates.

[0029] Figure 5 This is a constant current charge and discharge diagram of the ZnO@ZnNiCo-LDH composite material prepared in Example 1 of the present invention at different current densities.

[0030] Figure 6 This is a cycle performance diagram of the ZnO@ZnNiCo-LDH composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0031] Example 1

[0032] The preparation method of the ZnO@ZnNiCo-LDH composite material of this embodiment is as follows:

[0033] S1. 1.5 g of zinc acetate was mixed with 60 mL of deionized water, and the mixture was ultrasonicated for 15 min and magnetically stirred at a speed of 400 r / min for 40 min to obtain solution A. 4.514 g of sodium citrate was added to the solution A, and magnetically stirred at a speed of 400 r / min for 40 min to obtain solution B. 1 g of sodium hydroxide was added to the solution B while stirring, and magnetically stirred for 2 h to obtain solution C.

[0034] S2, after centrifuging the solution C obtained in S1 at a speed of 3000 r / min for 3 minutes, the precipitate was washed twice with deionized water, then washed twice with anhydrous ethanol, and dried under vacuum drying conditions at a temperature of 70° C. for 12 hours to obtain a white powder, i.e., ZnO solid;

[0035] S3, 0.25 g of the ZnO solid obtained in S2 was dispersed in 24 mL of deionized water, and magnetically stirred for 20 min at a speed of 300 r / min, and stirred evenly to obtain solution D; 4 g of 2-methylimidazole was dispersed in 72 mL of DMF, and magnetically stirred for 20 min at a speed of 300 r / min, and stirred evenly to obtain solution E; the solution D and solution E were mixed, and stirred and mixed in an oil bath at a temperature of 70° C. for 10 h to obtain solution F;

[0036] S4, centrifuging the solution F obtained in S3 at a speed of 3000 r / min for 3 min, washing the precipitate twice with DMF, then washing twice with anhydrous ethanol, and drying under vacuum drying conditions at a temperature of 70° C. for 12 h to obtain a milky white powder, namely ZnO@ZIF-8;

[0037] S5. Disperse 0.5 g of ZnO@ZIF-8 obtained in S4 in 30 mL of methanol a, and after ultrasonic dispersion for 15 min, add 0.9 g of Co(NO3)2·6H2O while stirring to obtain solution G; disperse 3.28 g of 2-methylimidazole in 100 mL of methanol b, and stir evenly with magnetic stirring to obtain solution H; add the solution H to the solution G, stir for 30 min, centrifuge at a speed of 3000 r / min for 3 min, wash the precipitate twice with methanol, and dry it at a vacuum drying condition of 70°C for 12 h to obtain a purple powder, namely ZnO@ZIF-8 / ZIF-67;

[0038] S6. Disperse 80 mg of ZnO@ZIF-8 / ZIF-67 obtained in S5 in 100 mL of ethanol, stir and mix for 30 min to obtain solution I, add 200 mg of Co(NO3)2·6H2O and 200 mg of Ni(NO3)2·6H2O to solution I while stirring to obtain a mixed solution J, then add 120 mg of hexamethylenetetramine and stir evenly to obtain a solution K, heat to reflux at 80°C for 1 h, cool to room temperature, centrifuge at 3000 r / min for 3 min, wash the precipitate twice with deionized water, then wash twice with anhydrous ethanol, and dry under vacuum drying conditions at 70°C for 12 h to obtain a light green powder, which is the ZnO@ZnNiCo-LDH composite material.

[0039] This embodiment also provides an application of the ZnO@ZnNiCo-LDH composite material prepared as above, wherein the ZnO@ZnNiCo-LDH composite material is applied in a positive electrode of a supercapacitor.

[0040] like Figure 1 As shown, the diffraction peaks of the ZnO@ZnNiCo-LDH composite material prepared in this embodiment at 2θ=11.34°, 22.74°, 33.45°, 34.41°, 38.76°, 59.98°, and 61.25° can be attributed to the characteristic diffraction peaks of crystal planes such as (003), (006), (101), (012), (015), (110), and (113), and these peaks are all characteristic diffraction peaks of LDH, and the diffraction peaks at 2θ=31.74°, 34.38°, 47.48°, and 56.53° can be attributed to the characteristic diffraction peaks of crystal planes such as (100), (002), (102), and (110), and these peaks are all characteristic diffraction peaks of ZnO, which can indicate that the prepared material is a ZnO@ZnNiCo-LDH composite material.

[0041] Figure 2 : is a SEM picture of the ZnO@ZnNiCo-LDH composite material prepared in this example, which is a flower-like material that forms lamellar ZnNiCo-LDH on the surface of ZnO microspheres.

[0042] Figure 3 is the nitrogen adsorption-desorption isotherm of the ZnO@ZnNiCo-LDH composite material prepared in this embodiment. Figure 3 As shown, the BET specific surface area is 137.38 m 2 / g, there are more active sites for redox reactions, which is conducive to the full progress of electrochemical reactions.

[0043] Figure 4is the cyclic voltammogram of the ZnO@ZnNiCo-LDH composite material prepared in this example at different scan rates, such as Figure 4 As shown, the CV curve shows obvious redox peaks, which proves that the material is a typical pseudocapacitive material.

[0044] In addition, as the scan rate increases, the peak current of the redox peak increases significantly, indicating that the redox rate on the electrode accelerates;

[0045] At the same time, the overall shape of the curve does not change much, and the corresponding redox peak is well maintained, which means that the polarization phenomenon of the electrode is not obvious.

[0046] Figure 5 is a constant current charge and discharge diagram of the ZnO@ZnNiCo-LDH composite material prepared in this example at different current densities, such as Figure 5 As shown, at 0.5, 1, 2, 5A·g -1 The specific capacitance at different current densities is 1012, 851, 758, and 488 F·g -1 , indicating that the material has a higher specific capacitance.

[0047] Figure 6 This is the cycle performance diagram of the ZnO@ZnNiCo-LDH composite material prepared in this example, as shown in Figure 6 As shown, the specific capacitance of the ZnO@ZnNiCo-LDH composite material can still maintain 75.05% of the initial value after 1000 cycles, indicating that the material has good cycle stability.

[0048] Example 2

[0049] The preparation method of the ZnO@ZnNiCo-LDH composite material of this embodiment is as follows:

[0050] S1. 1.5 g of zinc acetate was mixed with 60 mL of deionized water, and the mixture was ultrasonicated for 30 min and magnetically stirred at a speed of 600 r / min for 30 min to obtain solution A. 4.514 g of sodium citrate was added to the solution A, and magnetically stirred at a speed of 600 r / min for 30 min to obtain solution B. 1 g of sodium hydroxide was added to the solution B while stirring, and magnetically stirred for 2 h to obtain solution C.

[0051] S2, centrifuging the solution C obtained in S1 at a speed of 8000 r / min for 5 min, washing the precipitate with deionized water for 3 times, then washing with anhydrous ethanol for 3 times, and drying under vacuum drying conditions at a temperature of 60° C. for 24 h to obtain a white powder, i.e. ZnO solid;

[0052] S3, 0.25 g of the ZnO solid obtained in S2 was dispersed in 24 mL of deionized water, and magnetically stirred for 10 min at a speed of 500 r / min, and stirred evenly to obtain solution D; 4 g of 2-methylimidazole was dispersed in 72 mL of DMF, and magnetically stirred for 10 min at a speed of 500 r / min, and stirred evenly to obtain solution E; the solution D and solution E were mixed, and stirred and mixed in an oil bath at a temperature of 90° C. for 20 h to obtain solution F;

[0053] S4, centrifuging the solution F obtained in S3 at a speed of 8000 r / min for 5 min, washing the precipitate with DMF for 3 times, then washing with anhydrous ethanol for 3 times, and drying under vacuum drying conditions at a temperature of 60° C. for 24 h to obtain a milky white powder, namely ZnO@ZIF-8;

[0054] S5. Disperse 0.5 g of ZnO@ZIF-8 obtained in S4 in 30 mL of methanol a, and after ultrasonic dispersion for 15 min, add 0.9 g of Co(NO3)2·6H2O while stirring to obtain solution G; disperse 3.28 g of 2-methylimidazole in 100 mL of methanol b, and stir evenly with magnetic stirring to obtain solution H; add the solution H to the solution G, stir for 30 min, centrifuge at a speed of 8000 r / min for 5 min, wash the precipitate with methanol 3 times, and dry it at a vacuum drying condition of 60°C for 24 h to obtain a purple powder, namely ZnO@ZIF-8 / ZIF-67;

[0055] S6. Disperse 80 mg of ZnO@ZIF-8 / ZIF-67 obtained in S5 in 100 mL of ethanol, stir and mix for 30 min to obtain solution I, add 200 mg of Co(NO3)2·6H2O and 200 mg of Ni(NO3)2·6H2O to solution I while stirring to obtain a mixed solution J, then add 120 mg of hexamethylenetetramine and stir evenly to obtain a solution K, heat to reflux at 80°C for 1 h, cool to room temperature, centrifuge at 8000 r / min for 5 min, wash the precipitate 3 times with deionized water, then wash 3 times with anhydrous ethanol, and dry at 60°C under vacuum drying conditions for 24 h to obtain a light green powder, which is the ZnO@ZnNiCo-LDH composite material.

[0056] This embodiment also provides an application of the ZnO@ZnNiCo-LDH composite material prepared as above, wherein the ZnO@ZnNiCo-LDH composite material is applied in a positive electrode of a supercapacitor.

[0057] The specific surface area of ​​the ZnO@ZnNiCo-LDH composite material prepared in this example is 136.54 m 2 / g, there are more active sites for redox reactions, which is conducive to the full progress of electrochemical reactions.

[0058] The ZnO@ZnNiCo-LDH composite material prepared in this example has a -1 The specific capacitance at the current density is 1009F·g -1 , indicating that the material has a higher specific capacitance.

[0059] The ZnO@ZnNiCo-LDH composite material prepared in this embodiment can still maintain 76.13% of the initial specific capacitance after 1000 cycles, and has good cycle stability.

[0060] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a ZnO@ZnNiCo-LDH composite material, characterized in that: The method is: S1. Mix zinc acetate and deionized water, perform ultrasonic treatment for 15 to 30 minutes and magnetic stirring for 30 to 40 minutes to obtain solution A, add sodium citrate to the solution A, perform magnetic stirring for 30 to 40 minutes to obtain solution B; Add sodium hydroxide to the solution B while stirring, and stir magnetically for 2 hours to obtain solution C; S2, after centrifuging the solution C obtained in S1, the precipitate is washed with deionized water for 2 to 3 times, then washed with anhydrous ethanol for 2 to 3 times, and dried under vacuum drying conditions at a temperature of 60°C to 70°C for 12h to 24h to obtain a white powder, i.e. ZnO solid; S3, dispersing the ZnO solid obtained in S2 in deionized water, and stirring evenly with a magnetic force to obtain a solution D; dispersing 2-methylimidazole in DMF and stirring evenly with a magnetic force to obtain a solution E; mixing the solution D and the solution E, and stirring and mixing them in an oil bath at a temperature of 70° C. to 90° C. for 10 h to 20 h to obtain a solution F; S4, after centrifuging the solution F obtained in S3, the precipitate was washed with DMF for 2 to 3 times, and then washed with anhydrous ethanol for 2 to 3 times, and dried under vacuum drying conditions at a temperature of 60°C to 70°C for 12h to 24h to obtain a milky white powder, namely ZnO@ZIF-8; S5, dispersing the ZnO@ZIF-8 obtained in S4 in methanol a, ultrasonically dispersing for 15 min, and then adding Co(NO3)2·6H2O while stirring to obtain solution G; Disperse 2-methylimidazole in methanol b, stir evenly with a magnetic stirrer to obtain a solution H; add the solution H to the solution G, stir for 30 minutes, centrifuge, wash the precipitate with methanol for 2 to 3 times, and dry it under vacuum drying conditions at a temperature of 60° C. to 70° C. for 12 hours to 24 hours to obtain a purple powder, namely ZnO@ZIF-8 / ZIF-67; S6. Disperse the ZnO@ZIF-8 / ZIF-67 obtained in S5 in ethanol, stir and mix for 30 minutes to obtain solution I, add Co(NO3)2·6H2O and Ni(NO3)2·6H2O to the solution I while stirring to obtain a mixed solution J, then add hexamethylenetetramine and stir evenly to obtain a solution K, heat and reflux at 80°C for 1 hour, cool to room temperature, and centrifuge. Wash the precipitate with deionized water for 2 to 3 times, then wash with anhydrous ethanol for 2 to 3 times, and dry under vacuum drying conditions at 60°C to 70°C for 12 to 24 hours to obtain a light green powder, which is the ZnO@ZnNiCo-LDH composite material.

2. The method for preparing a ZnO@ZnNiCo-LDH composite material according to claim 1, characterized in that: The dosage ratio of zinc acetate, deionized water, sodium citrate and sodium hydroxide described in S1 is 1.5g:60mL:4.514g:1g.

3. The method for preparing a ZnO@ZnNiCo-LDH composite material according to claim 1, characterized in that: In S1, the rotation speed of the magnetic stirring is 400 r / min to 600 r / min.

4. The method for preparing a ZnO@ZnNiCo-LDH composite material according to claim 1, characterized in that: The centrifugal speeds of S2, S4, S5 and S6 are all 3000 r / min to 8000 r / min, and the centrifugal time is all 3 min to 5 min.

5. The method for preparing a ZnO@ZnNiCo-LDH composite material according to claim 1, characterized in that: The usage ratio of ZnO solid, deionized water, 2-methylimidazole and DMF in S3 is 0.25g:24mL:4g:72mL.

6. The method for preparing a ZnO@ZnNiCo-LDH composite material according to claim 1, characterized in that: The magnetic stirring time in S3 is 10 min to 20 min, and the magnetic stirring speed is 300 r / min to 500 r / min.

7. The method for preparing a ZnO@ZnNiCo-LDH composite material according to claim 1, characterized in that: The usage ratio of ZnO@ZIF-8, methanol a, Co(NO3)2·6H2O, 2-methylimidazole and methanol b described in S5 is 0.5 g:30 mL:0.9 g:3.28 g:100 mL.

8. The method for preparing a ZnO@ZnNiCo-LDH composite material according to claim 1, characterized in that: The usage ratio of ZnO@ZIF-8 / ZIF-67, ethanol, Co(NO3)2·6H2O, Ni(NO3)2·6H2O and hexamethylenetetramine described in S6 is 80 mg:100 mL:200 mg:200 mg:120 mg.

9. An application of a ZnO@ZnNiCo-LDH composite material prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The ZnO@ZnNiCo-LDH composite material is used in the positive electrode of a supercapacitor.