Amorphous carbon coated graphite and preparation method thereof
By introducing boron carbide powder and oxidation intercalation treatment in graphite chemical technology, combined with phenolic resin coating, the problems of high graphitization temperature and layer fallout are solved, the graphitization degree and electrochemical performance are improved, and more efficient lithium ions are achieved Embedded and stable graphite material.
Patent Information
- Application Number
- CN202310421536.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-04-19
AI Technical Summary
In the existing graphite chemical technology, the graphitization temperature is high, the graphite layer is prone to fall off during charging and discharging, and the particle size is difficult to regulate during granulation, which affects the degree of graphitization and electrochemical properties.
High-temperature graphitization is performed by adding boron carbide powder to anthracite, followed by oxidation intercalation and phenolic resin coating treatment, graphite covering amorphous carbon is formed, the graphitization temperature is reduced, and the graphite layer spacing and structural stability are improved.
The graphitization degree and electrochemical performance are significantly improved, the spacing between graphite layers increases, the embedding and removal of lithium ions is smoother, the graphite sheet layer is not easy to fall off during charging and discharge, and the reversible capacity and cycling performance are greatly improved.
Smart Images

Figure BDA0004187007610000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of graphite chemical industry, and in particular to graphite coated with amorphous carbon and a preparation method thereof. Background Art
[0002] As a high-quality negative electrode material for lithium-ion batteries, graphite has excellent electrochemical properties. Graphite can be obtained by high-temperature graphitization of anthracite, but it has the characteristics of low graphitization degree, high graphitization temperature and high energy consumption. Boron, as an excellent catalyst, can reduce the graphitization temperature and increase the graphitization degree, but the interlayer spacing of graphite catalyzed by boron is small, which is not conducive to the insertion and removal of lithium ions. By oxidative intercalation and carbon coating modification of graphite after catalytic graphitization, the interlayer spacing of graphite can be increased, and its graphite layer is not easy to fall off during the charge and discharge process, which can significantly improve the reversible specific capacity and cycle performance.
[0003] Chinese patent CN 105294105A discloses a method for preparing a carbon-bonded boron carbide and graphite composite material. Boron carbide powder and graphite powder with different particle size distributions are fully mixed with anhydrous ethanol and phenolic resin, granulated, and the density of the formed body is increased by multiple preforming and one-time final forming. The formed body is placed in a vacuum atmosphere sintering furnace and filled with a mixed gas of nitrogen, argon or helium and methane, ethylene or propane for enhanced sintering. By fully mixing phenolic resin with boron carbide powder and graphite powder, a phenolic resin film of a certain thickness is formed on the particle surfaces of boron carbide particles and graphite powder. The phenolic resin is used to initially combine the boron carbide powder particles and graphite powder particles through pressure and curing. Then, the green body is sintered at high temperature to convert the phenolic resin into carbon connection, and the filled gas is also converted into carbon, which penetrates into the pores of the green body to achieve further densification and strengthening of the green body. However, the catalytic effect of boron element in graphitization is not fully reflected, and there is a problem of regulating the particle size in the granulation process. The existing technology is slightly insufficient. Summary of the invention
[0004] Technical issues solved:
[0005] In view of the shortcomings of the prior art, the present application provides a graphite coated with amorphous carbon and a preparation method thereof, which solves the current problems such as the graphitization operating temperature is too high, the graphite layer is easy to fall off during the charging and discharging process, and the particle size regulation during the granulation process, so as to improve its graphitization degree and electrochemical performance.
[0006] Technical solution:
[0007] To achieve the above objectives, this application is implemented through the following technical solutions:
[0008] A method for preparing graphite coated with amorphous carbon, the method comprising the following steps:
[0009] S1: Adding boron carbide powder to deashed anthracite and grinding it thoroughly to obtain anthracite doped with boron, and then graphitizing it at 2200°C for 3h to obtain graphite catalyzed by boron;
[0010] S2: Pour the graphite catalyzed by boron into a beaker, then add a mixed solution containing an oxidant and an intercalation agent into the beaker to carry out an oxidation intercalation reaction, heat the reaction in a water bath at 40°C for 1 hour, and filter and dry to obtain graphite oxide;
[0011] S3: placing the oxidized graphite in a tubular furnace under protective gas for thermal reduction, the reaction temperature is 800°C, the heating rate is 2°C / min, and the temperature is kept constant for 1 hour to obtain oxidized micro-expanded layer graphite;
[0012] S4: dissolving phenolic resin powder in anhydrous ethanol to obtain a phenolic resin solution, then adding oxidized micro-expanded graphite to the phenolic resin solution and stirring thoroughly for carbon coating modification, and drying the mixed solution in an oven to obtain a carbon coating precursor;
[0013] S5: placing the carbon-coated precursor in a tubular furnace for high-temperature carbonization treatment, the carbonization temperature is 800-1000° C., the heating rate is 2° C. / min, and the temperature is kept constant for 1 hour after reaching the carbonization temperature to obtain graphite coated with amorphous carbon.
[0014] Preferably, the doping amount of the boron carbide powder in the first step is 3-15wt% of the mass of the deashed anthracite.
[0015] Preferably, the oxidant is concentrated sulfuric acid, concentrated nitric acid, perchloric acid or a mixture thereof.
[0016] Preferably, the intercalant is formic acid or acetic acid.
[0017] Preferably, the volume ratio of the oxidant to the intercalant is 0.5:1 to 2:1.
[0018] Preferably, the protective gas in the thermal reduction is nitrogen.
[0019] Preferably, the coating amount of the phenolic resin is 5 to 45 wt % of the oxidized micro-expanded graphite.
[0020] Preferably, the amount of anhydrous ethanol is 50 ml.
[0021] Preferably, the protective gas in the high-temperature carbonization treatment is nitrogen.
[0022] The present application also discloses graphite coated with amorphous carbon obtained by the above preparation method.
[0023] Principle of the invention:
[0024] The principle of this application is: by introducing boron element in graphitization, it can replace solid solution with carbon. Boron atoms are electron-deficient atoms, which can cause the covalent bonds between atoms to break, and the carbon structure is transformed from amorphous carbon to a three-dimensional ordered graphite structure. The graphite sheets can be slightly expanded by oxidants and intercalation agents, and the interlayer spacing can be appropriately increased, which is conducive to the transmission and diffusion of lithium ions inside the graphite. By wrapping amorphous carbon in the micro-expanded graphite, the structural stability of the material can be improved, and the occurrence of irreversible reactions can also be reduced.
[0025] Beneficial effects:
[0026] The present application provides a graphite coated with amorphous carbon and a preparation method thereof, which has the following beneficial effects:
[0027] 1. Compared with the traditional preparation method of coal-based graphite, the addition of boron element can not only reduce the graphitization temperature, but also greatly improve the graphitization degree of the obtained coal-based graphite, which can reach 99.1%.
[0028] 2. By micro-expanding the graphite, the interlayer spacing is larger than the ideal single crystal graphite interlayer spacing of 0.3354nm. The increase in interlayer spacing is more conducive to the embedding and removal of lithium ions between graphite sheets.
[0029] 3. By coating graphite with amorphous carbon, the graphite flakes are not easy to fall off during the charge and discharge process. After 110 cycles at a 1C rate, its reversible capacity can reach up to 317.8 mAh / g. The reversible capacity of the existing technology is less than 200.0 mAh / g. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0031] Embodiment 1:
[0032] A method for preparing graphite coated with amorphous carbon, the method comprising the following steps:
[0033] S1: 20 g of deashed anthracite and 0.6 g of boron carbide powder are mixed evenly and fully ground to obtain anthracite doped with boron, and then graphitized at 2200°C for 3 h to obtain graphite catalyzed by boron;
[0034] S2: Pour 10g of graphite catalyzed by boron into a beaker, then add a mixed solution containing 20ml of concentrated nitric acid and 20ml of formic acid into the beaker to carry out an oxidation intercalation reaction, heat the reaction in a water bath at 40°C for 1h, and filter and dry to obtain graphite oxide;
[0035] S3: placing the oxidized graphite in a tubular furnace for thermal reduction under a nitrogen atmosphere, the reaction temperature is 800°C, the heating rate is 2°C / min, and the temperature is kept constant for 1 hour to obtain oxidized micro-expanded layer graphite;
[0036] S4: dissolving 0.5 g of phenolic resin powder in 50 ml of anhydrous ethanol to prepare a phenolic resin solution, adding 5 g of oxidized micro-expanded graphite to the phenolic resin solution and stirring thoroughly for carbon coating modification, and drying the mixed solution in an oven to obtain a carbon coating precursor;
[0037] S5: The carbon-coated precursor is placed in a tubular furnace for high-temperature carbonization treatment under a nitrogen atmosphere, the carbonization temperature is 800-1000°C, the heating rate is 2°C / min, and after reaching 800°C, the temperature is kept constant for 1 hour to obtain graphite coated with amorphous carbon. Marked as A1, the graphitization degree, interlayer spacing and electrochemical performance of the graphite product are tested, and the test results are shown in Table 1.
[0038] Embodiment 2:
[0039] A method for preparing graphite coated with amorphous carbon, the method comprising the following steps:
[0040] S1: 20 g of deashed anthracite and 1 g of boron carbide powder are mixed evenly and fully ground to obtain anthracite doped with boron, and then graphitized at 2200°C for 3 h to obtain graphite catalyzed by boron;
[0041] S2: Pour 10g of graphite catalyzed by boron into a beaker, then add a mixed solution containing 20ml of concentrated nitric acid and 20ml of formic acid into the beaker to carry out an oxidation intercalation reaction, heat the reaction in a water bath at 40°C for 1h, and filter and dry to obtain graphite oxide;
[0042] S3: placing the oxidized graphite in a tubular furnace for thermal reduction under a nitrogen atmosphere, the reaction temperature is 800°C, the heating rate is 2°C / min, and the temperature is kept constant for 1 hour to obtain oxidized micro-expanded layer graphite;
[0043] S4: dissolving 1.5 g of phenolic resin powder in 50 ml of anhydrous ethanol to prepare a phenolic resin solution, adding 5 g of oxidized micro-expanded graphite to the phenolic resin solution and stirring thoroughly for carbon coating modification, and drying the mixed solution in an oven to obtain a carbon coating precursor;
[0044] S5: The carbon-coated precursor is placed in a tubular furnace for high-temperature carbonization treatment under a nitrogen atmosphere, the carbonization temperature is 800-1000°C, the heating rate is 2°C / min, and after reaching 800°C, the temperature is kept constant for 1 hour to obtain graphite coated with amorphous carbon. Marked as A2, the graphitization degree, interlayer spacing and electrochemical performance of the graphite product are tested, and the test results are shown in Table 1.
[0045] Comparative Example 1
[0046] No boron-doped graphitization treatment was performed, and other steps were the same as in Example 1.
[0047] S1: 20 g of deashed anthracite is placed in a graphite furnace and subjected to high temperature graphitization at 2200 °C for 3 h to obtain coal-based graphite;
[0048] S2: Pour 10g of coal-based graphite into a beaker, then add a mixed solution containing 20ml of concentrated nitric acid and 20ml of formic acid into the beaker to carry out an oxidation intercalation reaction, heat the reaction in a water bath at 40°C for 1h, and filter and dry to obtain graphite oxide;
[0049] S3: placing the oxidized graphite in a tubular furnace for thermal reduction under a nitrogen atmosphere, the reaction temperature is 800°C, the heating rate is 2°C / min, and the temperature is kept constant for 1 hour to obtain oxidized micro-expanded layer graphite;
[0050] S4: dissolving 0.5 g of phenolic resin powder in 50 ml of anhydrous ethanol to prepare a phenolic resin solution, adding 5 g of oxidized micro-expanded graphite to the phenolic resin solution and stirring thoroughly for carbon coating modification, and drying the mixed solution in an oven to obtain a carbon coating precursor;
[0051] S5: The carbon-coated precursor is placed in a tubular furnace for high-temperature carbonization treatment under a nitrogen atmosphere, the carbonization temperature is 800-1000°C, the heating rate is 2°C / min, and after reaching 800°C, the temperature is kept constant for 1 hour to obtain graphite coated with amorphous carbon. Marked as B1, the graphitization degree, interlayer spacing and electrochemical performance of the graphite product are tested, and the test results are shown in Table 1.
[0052] Comparative Example 2
[0053] No oxidation micro-expansion layer treatment was performed, and other steps were the same as in Example 1.
[0054] S1: 20 g of deashed anthracite and 0.6 g of boron carbide powder are mixed evenly and fully ground to obtain anthracite doped with boron, and then graphitized at 2200°C for 3 h to obtain graphite catalyzed by boron;
[0055] S2: dissolving 0.5 g of phenolic resin powder in 50 ml of anhydrous ethanol to prepare a phenolic resin solution, adding 5 g of graphite catalyzed by boron into the phenolic resin solution and stirring thoroughly for carbon coating modification, and drying the mixed solution in an oven to obtain a carbon coating precursor;
[0056] S3: The carbon-coated precursor is placed in a tubular furnace for high-temperature carbonization treatment under a nitrogen atmosphere, the carbonization temperature is 800-1000°C, the heating rate is 2°C / min, and after reaching 800°C, the temperature is kept constant for 1 hour to obtain graphite coated with amorphous carbon. Marked as B2, the graphitization degree, interlayer spacing and electrochemical performance of the graphite product are tested, and the test results are shown in Table 1.
[0057] Comparative Example 3
[0058] No amorphous carbon coating treatment was performed, and other steps were the same as in Example 1.
[0059] S1: 20 g of deashed anthracite and 0.6 g of boron carbide powder are mixed evenly and fully ground to obtain anthracite doped with boron, and then graphitized at 2200°C for 3 h to obtain graphite catalyzed by boron;
[0060] S2: Pour 10g of graphite catalyzed by boron into a beaker, then add a mixed solution containing 20ml of concentrated nitric acid and 20ml of formic acid into the beaker to carry out an oxidation intercalation reaction, heat the reaction in a water bath at 40°C for 1h, and filter and dry to obtain graphite oxide;
[0061] S3: The oxidized graphite was placed in a tubular furnace for thermal reduction under a nitrogen atmosphere, the reaction temperature was 800°C, the heating rate was 2°C / min, and the temperature was kept constant for 1 hour to obtain oxidized micro-expanded layer graphite. Marked as B3, the graphitization degree, interlayer spacing and electrochemical performance of the graphite product were tested, and the test results are shown in Table 1.
[0062] Table 1 Processing methods and performance test data of graphite products of embodiments and comparative examples
[0063]
[0064] It can be seen from the results of the embodiments, comparative examples and Table 1 that the graphitization degree of coal-based graphite is significantly improved after the addition of boron, the micro-expansion layer can increase the interlayer spacing of graphite, and the amorphous carbon coating can increase its reversible capacity and coulombic efficiency after 110 cycles. By adding boron, micro-expansion layer treatment and carbon coating, the graphitization degree, interlayer spacing, reversible capacity and coulombic efficiency are greatly improved.
[0065] The above is a detailed description of the present invention in combination with the embodiments, but the implementation methods of the present invention are not limited to the above embodiments. Improvements, replacements, and modifications made by those skilled in the art based on the inspiration of the present invention and without departing from the core guiding ideology of the present invention should all be within the scope of protection of the present invention.
Claims
1. A method for preparing graphite coated with amorphous carbon, characterized in that: The specific steps of this method are as follows: S1: Adding boron carbide powder to deashed anthracite and grinding it thoroughly to obtain anthracite doped with boron, and then graphitizing it at 2200°C for 3h to obtain graphite catalyzed by boron; S2: Pour the graphite catalyzed by boron into a beaker, then add a mixed solution containing an oxidant and an intercalation agent into the beaker to carry out an oxidation intercalation reaction, heat the reaction in a water bath at 40°C for 1 hour, and filter and dry to obtain graphite oxide; S3: placing the oxidized graphite in a tubular furnace under protective gas for thermal reduction, the reaction temperature is 800°C, the heating rate is 2°C / min, and the temperature is kept constant for 1 hour to obtain oxidized micro-expanded layer graphite; S4: dissolving phenolic resin powder in anhydrous ethanol to obtain a phenolic resin solution, then adding oxidized micro-expanded graphite to the phenolic resin solution and stirring thoroughly for carbon coating modification, and drying the mixed solution in an oven to obtain a carbon coating precursor; S5: placing the carbon-coated precursor in a tubular furnace for high-temperature carbonization treatment, the carbonization temperature is 800-1000° C., the heating rate is 2° C. / min, and the temperature is kept constant for 1 hour after reaching the carbonization temperature to obtain graphite coated with amorphous carbon.
2. The method for preparing graphite coated with amorphous carbon according to claim 1, characterized in that: The doping amount of the boron carbide powder in the first step is 3-15wt% of the mass of the deashed anthracite.
3. The method for preparing graphite coated with amorphous carbon according to claim 1, characterized in that: The oxidant is concentrated sulfuric acid, concentrated nitric acid, perchloric acid or a mixture thereof.
4. The method for preparing graphite coated with amorphous carbon according to claim 1, characterized in that: The intercalant is formic acid or acetic acid.
5. The method for preparing graphite coated with amorphous carbon according to claim 1, characterized in that: The volume ratio of the oxidant to the intercalant is 0.5:1 to 2:
1.
6. The method for preparing graphite coated with amorphous carbon according to claim 1, characterized in that: The protective gas in the thermal reduction is nitrogen.
7. The method for preparing graphite coated with amorphous carbon according to claim 1, characterized in that: The coating amount of the phenolic resin is 5-45wt% of the oxidized micro-expanded graphite.
8. The method for preparing graphite coated with amorphous carbon according to claim 1, characterized in that: The amount of anhydrous ethanol used is 50 ml.
9. The method for preparing graphite coated with amorphous carbon according to claim 1, characterized in that: The protective gas in the high temperature carbonization treatment is nitrogen.
10. A graphite coated with amorphous carbon obtained by the preparation method according to any one of claims 1 to 9.