A kind of supported noble metal oxide and preparation method thereof

By pH adjustment and high-energy ball milling on the carrier surface to form a strong noble metal-carrier interaction layer, the problem of uneven loading of precious metal oxides is solved, the catalytic activity and reaction efficiency are improved, and efficient and economical catalyst preparation is achieved.

CN116371403BActive Publication Date: 2024-10-01XIAN TAIJIN NEW ENERGY & MATERIALS SCI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310367563.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-01
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

It is difficult to achieve uniform loading of precious metal oxides on the surface of the carrier with existing technology, resulting in insufficient catalytic activity. In addition, traditional solution methods and ball milling methods have problems with uneven loading and high costs.

Method used

Through pH adjustment and ultrasonic treatment on the carrier surface, combined with high-energy ball milling, the precious metal ions and the carrier form a strong interaction layer, which increases the loading capacity and catalytic activity, and forms a highly dispersed and uniformly loaded catalyst through the sintering step.

Benefits of technology

It achieves uniform loading of noble metal oxides on the surface of the carrier, improves catalytic activity and reaction efficiency, reduces production costs, and the catalyst has good electronic conductivity and electrocatalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004167364840000011
    Figure HDA0004167364840000011
  • Figure HDA0004167364840000012
    Figure HDA0004167364840000012
  • Figure HDA0004167364840000021
    Figure HDA0004167364840000021
Patent Text Reader

Abstract

A supported noble metal oxide and a preparation method thereof, the method comprising the following steps: S1, preparing a carrier dispersion liquid A; S2, adjusting the pH value of the carrier dispersion liquid A obtained in S1; S3, preparing a precursor solution B; S4, mixing the carrier dispersion liquid A and the precursor solution B by high-energy ball milling; S5, synthesizing a catalyst precursor C; S6, synthesizing a highly dispersed powder catalyst D; S7, synthesizing a metal or metal oxide with an ultra-dispersed structure; the oxide is obtained by the above preparation method; after pre-treating the carrier, the carrier is fully contacted with the precursor solution by mechanical ball milling to be evenly dispersed, the coverage amount is adjusted by adjusting the stirring time, and the oxide particle size can be controlled by adjusting the temperature and time of the later sintering, thereby realizing the simple synthesis of noble metal supported nano oxides with high loading and high dispersion, and having the characteristics of simple operation and cost saving.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of membrane electrode catalyst preparation, and particularly relates to a supported noble metal oxide and a preparation method thereof. Background Art

[0002] Proton exchange membrane (PEM) water electrolysis is the most popular hydrogen production method at present, among which oxygen evolution reaction is the bottleneck reaction of PEM water electrolysis. Oxygen evolution overpotential is the main factor affecting the reaction efficiency, requiring the anode catalyst to have a high catalytic activity. The commonly used noble metals such as Ir, Ru and their oxides as catalysts can obtain high catalytic activity. However, the reserves of such metal elements are low and the prices are high, which cannot meet the needs of mass production and application of PEM. Therefore, supported noble metals have become the focus of research. The ideal oxygen evolution electrocatalyst should have high specific surface area and porosity, high electronic conductivity, good electrocatalytic performance, long-term mechanical and electrochemical stability, small bubble effect, cheap availability and non-toxicity, etc. Therefore, Ir, Ru and other noble metals / oxides with supported structures and binary and ternary alloys / mixed oxides based on them are more ideal catalyst materials.

[0003] As a traditional method for synthesizing metal-supported catalysts, the solution method is to evenly disperse the metal precursor and the carrier material with a high specific surface area, and then load the reduced metal nanostructure on the substrate. In fact, the traditional solution method cannot achieve uniform adhesion of the metal precursor on the carrier surface, and the metal or oxide on the carrier surface cannot be sufficiently covered to achieve the purpose of increasing the effective catalytic activity area.

[0004] Chinese patent CN111569867A discloses a method for preparing a loaded noble metal VOCs degradation catalyst by ball milling. The catalyst prepared by the inventive method is an inert material with high surface area and porosity (such as Al2O3, cordierite, etc.) and a transition metal oxide (Co3O4, MnO2, Fe3O4 and TiO2, etc.) as a carrier, and noble metal single atoms, clusters or nanoparticles such as noble metals Pt, Rh, Pd, Au, etc. are loaded by ball milling to prepare a catalyst for VOCs catalytic oxidation. First, a certain concentration of carrier dispersion solution A is configured, and after uniform dispersion, a noble metal precursor solution B is added, and solution B is added to solution A, uniformly stirred and adsorbed, and then placed in a planetary ball mill for liquid phase ball milling, and the catalyst is obtained by suction filtration and drying recovery. Different types of loaded noble metal catalysts can be obtained by controlling the carrier type, the concentration of the noble metal precursor and the ball milling process parameters. This method is suitable for VOCs catalysts with a porous structure. However, since ordinary solid phase particles generally have a low surface energy, it is not easy to achieve the combination of the two phases through physical adsorption. Simple mechanical grinding will cause the catalyst to be unevenly distributed on the carrier particles. At the same time, the catalyst loading is also limited by the surface morphology of the carrier, which is not conducive to improving the catalyst activity.

[0005] Chinese patent CN104741118A discloses a method for preparing a highly dispersed noble metal alloy catalyst, specifically a one-step synthesis of Au-Pt and Au-Ru noble metal alloy catalysts supported by mesoporous silica. The method synthesis process of the invention is simple, avoiding pollution and waste of resources in a complex synthesis process. The obtained noble metal alloy catalyst has the advantages of good dispersion of noble metal nanoparticles (average particle size ≈ 3.0nm) and well-developed mesoporous channels. At the same time, the noble metal nanoparticles are partially embedded in the pore walls of the mesoporous silica carrier, which can greatly improve the stability of the catalyst and extend the catalyst life. However, a simple stirring method cannot achieve a large-scale uniform load, and uneven loads will still occur when the supported catalyst is prepared in batches. Summary of the invention

[0006] In order to overcome the deficiencies of the above-mentioned prior art, the purpose of the present invention is to provide a supported precious metal oxide and a preparation method thereof, by adjusting the surface chemical potential of the carrier material by using a pH regulator, the loading amount of the catalyst on the carrier surface is increased; in addition, while the present invention utilizes mechanical ball milling to fully disperse the carrier and uniformly load the active substance on the carrier surface, the interaction between the precious metal ions and the carrier is promoted by mechanical energy; during the high-energy ball milling process, part of the mechanical energy is converted into internal energy, which promotes the diffusion of metal ions on the carrier surface, forms a metal-carrier strong interaction layer, and plays a role in increasing the catalytic activity of the precious metal; through the steps of ball milling, drying, grinding, and sintering, a precious metal catalyst for electrolysis of water with a uniform loading structure and excellent catalytic activity is obtained, which has the characteristics of improving reaction efficiency, saving costs and being easy to implement.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A method for preparing a supported noble metal oxide comprises the following steps:

[0009] Step S1, preparing carrier dispersion A: weigh a certain amount of carrier powder, add it to an alcohol solution and stir evenly to obtain a carrier dispersion A with a mass-volume concentration of 0.25-0.5 mg / mL; the alcohol solution can be one or a mixture of two or more of anhydrous ethanol, isopropanol, deionized water, and ethylene glycol in any ratio; the carrier is one or a mixture of two or more of a soluble or well-dispersible metal oxide, non-metal oxide, g-C3N4, open hollow carbon spheres, nanoporous carbon, and conductive carbon black XC72R in any ratio;

[0010] Step S2, adjusting the pH value of the carrier dispersion A obtained in step S1: adding a pH adjuster to the carrier dispersion A to adjust the pH of the carrier dispersion A to ≤ 6, adjusting the charge distribution on the carrier surface, and placing it in an ultrasonic environment with an ultrasonic frequency of 25 to 40 Hz and a temperature of 40 to 50° C. for 20 to 60 minutes;

[0011] Step S3, preparing precursor solution B: dissolving the noble metal compound in an alcohol solution to form a dispersion having a metal ion concentration of 0.4 to 1.2 mmol / L, namely, precursor solution B. The alcohol solution may be one of anhydrous ethanol, isopropanol, deionized water, and ethylene glycol, or a mixture of two or more in any ratio;

[0012] Step S4, high-energy ball milling and mixing the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3: the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 are mixed in a ratio of 20% to 50% of the mass of the metal element to the mass of the carrier, and the solution with uniform composition after stirring is poured into a ball milling jar, and the materials are added according to a material-to-ball ratio of 1: (1 to 6), the ball diameter is 1 mm to 8 mm, and grinding balls of different diameters are added in equal parts and proportions, the rotation speed is 800 to 1000 r / min, and the ball milling is performed for 6 to 16 hours;

[0013] Step S5, synthesizing catalyst precursor C: placing the ball-milled product in an oven at 80-110° C. for drying, and grinding to obtain catalyst precursor C;

[0014] Step S6, synthesizing highly dispersed powder catalyst D: placing the catalyst precursor C obtained in step S5 in a crucible and placing it in a muffle furnace, heating it to 450-550° C. at a rate of 2-5° C. / min, keeping the temperature for 1-4 hours, and cooling it in the furnace to obtain a highly dispersed powder catalyst D with a carrier structure;

[0015] Step S7, synthesizing a metal or metal oxide catalyst with an ultra-dispersed structure: using a centrifuge, sequentially using deionized water and anhydrous ethanol to centrifugally clean and dry the powdered catalyst several times, and finally obtaining a metal or metal oxide with an ultra-dispersed structure.

[0016] The pH adjuster in step S2 is one or a mixture of any two or more of oxalic acid, formic acid, acetic acid, nitric acid, sulfuric acid, sulfurous acid, hydrochloric acid, perchloric acid, chloric acid, hypochlorous acid, phosphoric acid, sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia water, potassium carbonate, potassium bicarbonate, sodium carbonate, and sodium bicarbonate.

[0017] The precious metal compound in step S3 is at least one of chloroiridic acid, iridium trichloride, bromoiridic acid, chloroplatinic acid, platinum tetrachloride, platinum oxide, ruthenium trichloride, chlororuthenic acid, potassium chlororuthenate, sodium chlororuthenate, and ammonium chlororuthenate.

[0018] A supported noble metal oxide is obtained by the above preparation method.

[0019] The beneficial effects of the present invention are:

[0020] 1. A supported noble metal oxide and a preparation method thereof, wherein step S2 pre-treats a high specific surface area carrier by adjusting the pH value of the carrier dispersion A obtained in step S1, and step S4 mechanically ball-mills the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 to allow the carrier to fully contact the precursor solution, so that the noble metal and the carrier form a strong interaction layer and are uniformly dispersed on the surface interface of the carrier, thereby adjusting the electronic structure of the catalyst and having the characteristic of enhancing the catalytic activity.

[0021] 2. In step S4 of the present invention, materials are added at a material-to-ball ratio of 1:(1-6), the ball diameter is 1 mm-8 mm, and grinding balls of different diameters are added in equal portions and proportions. The rotation speed is 800-1000 r / min, and the ball milling is performed for 6-16 hours. The coverage amount is adjusted by adjusting the stirring time. At the same time, the catalyst particle size can be controlled by adjusting the temperature and time of the later sintering through steps S5 to S7, thereby achieving a simple synthesis of precious metal-supported nanocatalysts with high loading and high dispersion, which has the characteristics of being easy to implement.

[0022] In summary, the present invention regulates the surface charge of the carrier material so that it has the property of adsorbing precious metal ions; uses high-energy ball milling to mechanically react the carrier with the precious metal precursor ions, so that the metal active components are more evenly distributed in the carrier pores and on the surface; and during calcination in step S7, since the powder catalyst is centrifugally cleaned and dried several times using deionized water and anhydrous ethanol in sequence, the valence state of the metal oxide can be relatively rich, and the operation is simple and cost-saving. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a scanning electron microscope image of the powder catalyst prepared by mechanical ball milling in Example 1 of the present invention.

[0024] Figure 2 This is a scanning electron microscope image of the powder catalyst prepared by mechanical ball milling in Example 2 of the present invention.

[0025] Figure 3 This is a scanning electron microscope image of the powder catalyst prepared by mechanical ball milling in Example 3 of the present invention.

[0026] Figure 4 This is a scanning electron microscope image of a powder catalyst prepared in a comparative example of the present invention.

[0027] Figure 5 1 is a polarization curve diagram of Example 1 of the present invention and Comparative Example 1.

[0028] Figure 6 The cyclic voltammetry curves of Example 1 of the present invention and Comparative Example 1 are shown in FIG. DETAILED DESCRIPTION

[0029] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0030] Example 1

[0031] A method for preparing a supported noble metal oxide comprises the following steps:

[0032] Step S1, preparing carrier dispersion A: 20 mL of 0.5 mg / mL TiO2 solution with a particle size of 1 μm, the solvent is ethanol;

[0033] Step S2, adding 40 μL of acetic acid and 20 μL of deionized water to the carrier dispersion A obtained in step S1, placing the dispersion in an ultrasonic environment at an ultrasonic frequency of 28 Hz and a temperature of 45° C. for 40 min to uniformly disperse the carrier in the solvent, and obtaining a carrier dispersion A having a pH of 5.5;

[0034] Step S3, preparing a precursor solution B: the noble metal precursor solution B is a mixed solution of Ir metal ions and Ru metal ions mixed in a molar ratio of 1:1 with a concentration of 1 mmol / L, and the solvent is ethanol;

[0035] Step S4, the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 are mixed at a ratio of 50% of the mass of the metal element to the mass of the carrier, and the solution with uniform composition after stirring is poured into a ball mill, and the materials are added at a material-ball ratio of 1:2, the ball diameter is 1mm to 8mm, and grinding balls of different diameters are added in equal parts and proportions, the rotation speed is 800r / min, and the ball milling is carried out for 16h;

[0036] Step S5, drying the ball-milled product in an oven at 100° C., and obtaining a catalyst precursor C after grinding;

[0037] Step S6: Place the catalyst precursor C obtained in step S5 in a crucible and place it in a muffle furnace, heat it to 500°C at a rate of 5°C / min, keep it warm for 2 hours, and cool it in the furnace to obtain a highly dispersed powder catalyst Ir having a carrier structure. 0.5 Ru 0.5 O2@TiO2;

[0038] Step S7: using a centrifuge to centrifuge and clean and dry the powdered catalyst several times using deionized water and anhydrous ethanol in sequence, and finally obtaining a metal or metal oxide with an ultra-dispersed structure.

[0039] Example 2

[0040] A method for preparing a supported noble metal oxide comprises the following steps:

[0041] Step S1, preparing carrier dispersion solution A: 20 mL of 0.5 mg / mL SiO2 solution with a particle size of 200 nm, the solvent is ethanol;

[0042] Step S2, adding 40 μL of acetic acid and 20 μL of deionized water to the carrier dispersion A obtained in step S1, and placing it in an ultrasonic environment with an ultrasonic frequency of 40 Hz and a temperature of 40° C. for 20 minutes to make the carrier evenly dispersed in the solvent, to obtain a carrier dispersion A adjusted to pH 6;

[0043] Step S3, preparing precursor solution B: 1 mmol / L chloroiridic acid solution, the solvent is ethanol;

[0044] Step S4, the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 are mixed at a ratio of 50% of the mass of the metal element to the mass of the carrier, and the solution with uniform composition after stirring is poured into a ball mill, and the materials are added at a material-ball ratio of 1:2, the ball diameter is 1mm to 8mm, and grinding balls of different diameters are added in equal parts and proportions, the rotation speed is 900r / min, and the ball milling is performed for 6h;

[0045] Step S5, drying the ball-milled product in an oven at 100° C., and obtaining a catalyst precursor C after grinding;

[0046] Step S6, placing the catalyst precursor C obtained in step S5 in a crucible and placing it in a muffle furnace, heating it to 500° C. at a rate of 5° C. / min, keeping the temperature for 2 hours, and cooling it in the furnace to obtain a highly dispersed powder catalyst IrO2 / SiO2 with a carrier structure;

[0047] Step S7: using a centrifuge to centrifuge and clean and dry the powdered catalyst several times using deionized water and anhydrous ethanol in sequence, and finally obtaining a metal or metal oxide with an ultra-dispersed structure.

[0048] Example 3

[0049] A method for preparing a supported noble metal oxide comprises the following steps:

[0050] Step S1, preparing carrier dispersion solution A: 20 mL of 0.25 mg / mL conductive carbon black XC72R solution, the solvent is ethanol;

[0051] Step S2, adding 20 μL of hydrogen peroxide, 20 μL of acetic acid, and 20 μL of deionized water to the carrier dispersion A obtained in step S1, and placing it in an ultrasonic environment with an ultrasonic frequency of 28 Hz and a temperature of 50° C. for 30 minutes to make the carrier evenly dispersed in the solvent, to obtain a carrier dispersion A adjusted to pH 6;

[0052] Step S3, preparing precursor solution B: 1 mmol / L chloroplatinic acid solution, the solvent is ethanol;

[0053] Step S4, the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 are mixed at a ratio of 20% of the mass of the metal element to the mass of the carrier, and the solution with uniform composition after stirring is poured into a ball mill, and the materials are added at a material-ball ratio of 1:1, the ball diameter is 1mm to 8mm, and grinding balls of different diameters are added in equal parts and proportions, the rotation speed is 1000r / min, and the ball milling is carried out for 10h;

[0054] Step S5, drying the ball-milled product in an oven at 100° C., and obtaining a catalyst precursor C after grinding;

[0055] Step S6, placing the catalyst precursor C obtained in step S5 in a crucible and placing it in a muffle furnace, heating it to 550° C. at a rate of 5° C. / min, keeping the temperature for 2 hours, and cooling it in the furnace to obtain a highly dispersed powder catalyst Pt / C with a carrier structure;

[0056] Step S7: using a centrifuge to centrifuge and clean and dry the powdered catalyst several times using deionized water and anhydrous ethanol in sequence, and finally obtaining a metal or metal oxide with an ultra-dispersed structure.

[0057] Example 4

[0058] A method for preparing a supported noble metal oxide comprises the following steps:

[0059] Step S1, preparing carrier dispersion solution A: 20 mL of 0.4 mg / mL TiO2 solution with a particle size of 1 μm, and the solvent is ethanol;

[0060] Step S2, adding 40 μL of acetic acid and 20 μL of deionized water to the carrier dispersion A obtained in step S1, and placing it in an ultrasonic environment with an ultrasonic frequency of 40 Hz and a temperature of 45° C. for 60 min to uniformly disperse the carrier in the solvent, and obtaining an adjusted carrier dispersion A with a pH of 5.5;

[0061] Step S3, preparing precursor solution B: 1 mmol / L chloroiridic acid solution, the solvent is ethanol;

[0062] Step S4, the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 are mixed at a ratio of 50% of the mass of the metal element to the mass of the carrier, and the solution with uniform composition after stirring is poured into a ball mill, and the materials are added at a material-ball ratio of 1:4, the ball diameter is 1mm to 8mm, and grinding balls of different diameters are added in equal parts and proportions, the rotation speed is 1000r / min, and the ball milling is carried out for 10h;

[0063] Step S5, drying the ball-milled product in an oven at 100° C., and obtaining a catalyst precursor C after grinding;

[0064] Step S6, placing the catalyst precursor C obtained in step S5 in a crucible and placing it in a muffle furnace, heating it to 450° C. at a rate of 5° C. / min, keeping the temperature for 1 hour, and cooling it in the furnace to obtain a highly dispersed powder catalyst IrO2@TiO2 with a carrier structure;

[0065] Step S7: using a centrifuge to centrifuge and clean and dry the powdered catalyst several times using deionized water and anhydrous ethanol in sequence, and finally obtaining a metal or metal oxide with an ultra-dispersed structure.

[0066] Comparative Example 1

[0067] First, prepare the carrier dispersion solution A: 20mL 0.5mg / mL TiO2 solution with a particle size of 1μm, and the solvent is ethanol; the noble metal precursor solution B is a mixed solution of Ir metal ions and Ru metal ions at a molar ratio of 1:1 with a concentration of 1mmol / L, and the solvent is ethanol; the solution A and solution B are mixed at a ratio of 50% of the mass of the metal element to the mass of the carrier. After stirring in a magnetic stirrer for 30 minutes, it is dried at 100 degrees Celsius and ground, placed in a muffle furnace, and heated to 500°C at a speed of 5°C / min, kept warm for 2 hours, and cooled with the furnace to obtain a powder catalyst Ir 0.5 Ru 0.5 O2@TiO2.

[0068] Depend on Figure 1 , Figure 4 By comparison, the present invention adds a ball milling process, and a planetary ball mill is used in the embodiment to make the catalyst particles distinct and avoid agglomeration; at the same time, a chemical treatment method of the carrier is used, that is, first preparing a carrier dispersion A, then adjusting the pH value of the carrier dispersion A obtained in step S1, and finally preparing a precursor solution B, so that iridium oxide is fully loaded on the surface of the spherical TiO2, which plays a positive role in increasing the effective active area.

[0069] The electrochemical performance of the catalyst was measured in an electrochemical workstation with an electrolyte of 0.5 mol / L H2SO4 at room temperature. A catalyst-coated glassy carbon (GC) electrode (diameter: 3 mm), an Ag / AgCl electrode, and a platinum sheet were used as the working electrode, reference electrode, and counter electrode, respectively. 4 mg of catalyst powder was added to a mixed solution containing 200 μL of ethanol and 200 μL of Nafion aqueous solution (5% by volume, ethanol as solvent), and ultrasonically dispersed for 15 minutes to form a uniform ink, which was evenly coated on the GC to form a working electrode.

[0070] Depend on Figure 5Polarization curves show that, after the surface treatment of the carrier, the noble metal solution is evenly dispersed on the carrier surface during ball milling, and interacts with the carrier under mechanical action to form a noble metal-carrier strong interaction layer. The formation of this structure effectively improves the catalytic activity of the noble metal oxide, reaching 50 mA / cm -2 The electrolysis voltage required for the current density was reduced from 1.58V to 1.48V.

[0071] at the same time, Figure 6 The CV graph shown indicates that the present invention effectively increases the effective active area of ​​the oxide and obtains better catalytic activity.

[0072] In summary, the present invention adopts a high-energy ball milling method with a rotation speed of 800-1000 r / min to increase the dispersion capacity of effective catalytic ions, and at the same time effectively performs surface ion modification on the carrier, thereby increasing the adsorption capacity of the carrier for metal ions, thereby increasing the loading amount of effective catalytic components on the carrier. By this method, an electrolytic water oxygen evolution oxide with high electronic conductivity and good electrocatalytic performance is prepared.

[0073] The above is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

Claims

1. A method for preparing a supported noble metal oxide, characterized in that: The specific steps include: Step S1, preparing carrier dispersion A: weigh a certain amount of carrier powder, add it to an alcohol solution and stir evenly to obtain a carrier dispersion A with a mass-volume concentration of 0.25-0.5 mg / mL; the alcohol solution can be one or a mixture of two or more of anhydrous ethanol, isopropanol, deionized water, and ethylene glycol in any ratio; the carrier is one or a mixture of two or more of a soluble or well-dispersible metal oxide, non-metal oxide, g-C3N4, open hollow carbon spheres, nanoporous carbon, and conductive carbon black XC72R in any ratio; Step S2, adjusting the pH value of the carrier dispersion A obtained in step S1: adding a pH adjuster to the carrier dispersion A to adjust the pH of the carrier dispersion A to ≤ 6, adjusting the charge distribution on the carrier surface, and placing it in an ultrasonic environment with an ultrasonic frequency of 25 to 40 Hz and a temperature of 40 to 50° C. for 20 to 60 minutes; Step S3, preparing precursor solution B: dissolving the noble metal compound in an alcohol solution to form a dispersion having a metal ion concentration of 0.4 to 1.2 mmol / L, namely, precursor solution B. The alcohol solution may be one of anhydrous ethanol, isopropanol, deionized water, and ethylene glycol, or a mixture of two or more in any ratio; Step S4, high-energy ball milling and mixing the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3: the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 are mixed in a ratio of 20% to 50% of the mass of the metal element to the mass of the carrier, and the solution with uniform composition after stirring is poured into a ball milling jar, and the materials are added according to a material-to-ball ratio of 1: (1 to 6), the ball diameter is 1 mm to 8 mm, and grinding balls of different diameters are added in equal parts and proportions, the rotation speed is 800 to 1000 r / min, and the ball milling is performed for 6 to 16 hours; Step S5, synthesizing catalyst precursor C: placing the ball-milled product in an oven at 80-110° C. for drying, and grinding to obtain catalyst precursor C; Step S6, synthesizing highly dispersed powder catalyst D: placing the catalyst precursor C obtained in step S5 in a crucible and placing it in a muffle furnace, heating it to 450-550° C. at a rate of 2-5° C. / min, keeping the temperature for 1-4 hours, and cooling it in the furnace to obtain a highly dispersed powder catalyst D with a carrier structure; Step S7, synthesizing a metal or metal oxide catalyst with an ultra-dispersed structure: using a centrifuge, sequentially using deionized water and anhydrous ethanol to centrifugally clean and dry the powdered catalyst several times, and finally obtaining a metal or metal oxide with an ultra-dispersed structure.

2. The method for preparing a supported noble metal oxide according to claim 1, characterized in that: The pH adjuster in step S2 is one or a mixture of any two or more of oxalic acid, formic acid, acetic acid, nitric acid, sulfuric acid, sulfurous acid, hydrochloric acid, perchloric acid, chloric acid, hypochlorous acid, phosphoric acid, sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia water, potassium carbonate, potassium bicarbonate, sodium carbonate, and sodium bicarbonate.

3. The method for preparing a supported noble metal oxide according to claim 1, characterized in that: The precious metal compound in step S3 is at least one of chloroiridic acid, iridium trichloride, bromoiridic acid, chloroplatinic acid, platinum tetrachloride, platinum oxide, ruthenium trichloride, chlororuthenic acid, potassium chlororuthenate, sodium chlororuthenate, and ammonium chlororuthenate.

4. A method for preparing a supported noble metal oxide, characterized in that: The specific steps include: Step S1, preparing carrier dispersion A: 20 mL of 0.5 mg / mL TiO2 solution with a particle size of 1 μm, the solvent is ethanol; Step S2, adding 40 μL of acetic acid and 20 μL of deionized water to the carrier dispersion A obtained in step S1, placing the dispersion in an ultrasonic environment at an ultrasonic frequency of 28 Hz and a temperature of 45° C. for 40 min to uniformly disperse the carrier in the solvent, and obtaining a carrier dispersion A having a pH of 5.5; Step S3, preparing a precursor solution B: the noble metal precursor solution B is a mixed solution of Ir metal ions and Ru metal ions mixed in a molar ratio of 1:1 with a concentration of 1 mmol / L, and the solvent is ethanol; Step S4, the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 are mixed at a ratio of 50% of the mass of the metal element to the mass of the carrier, and the solution with uniform composition after stirring is poured into a ball mill, and the materials are added at a material-ball ratio of 1:2, the ball diameter is 1mm to 8mm, and grinding balls of different diameters are added in equal parts and proportions, the rotation speed is 800r / min, and the ball milling is carried out for 16h; Step S5, drying the ball-milled product in an oven at 100° C., and obtaining a catalyst precursor C after grinding; Step S6: Place the catalyst precursor C obtained in step S5 in a crucible and place it in a muffle furnace, heat it to 500°C at a rate of 5°C / min, keep it warm for 2 hours, and cool it in the furnace to obtain a highly dispersed powder catalyst Ir having a carrier structure. 0.5 Ru 0.5 O2@TiO2; Step S7: using a centrifuge to centrifuge and clean and dry the powdered catalyst several times using deionized water and anhydrous ethanol in sequence, and finally obtaining a metal or metal oxide with an ultra-dispersed structure.

5. A method for preparing a supported noble metal oxide, characterized in that: The specific steps include: Step S1, preparing carrier dispersion solution A: 20 mL of 0.5 mg / mL SiO2 solution with a particle size of 200 nm, the solvent is ethanol; Step S2, adding 40 μL of acetic acid and 20 μL of deionized water to the carrier dispersion A obtained in step S1, and placing it in an ultrasonic environment with an ultrasonic frequency of 40 Hz and a temperature of 40° C. for 20 minutes to make the carrier evenly dispersed in the solvent, to obtain a carrier dispersion A adjusted to pH 6; Step S3, preparing precursor solution B: 1 mmol / L chloroiridic acid solution, the solvent is ethanol; Step S4, the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 are mixed at a ratio of 50% of the mass of the metal element to the mass of the carrier, and the solution with uniform composition after stirring is poured into a ball mill, and the materials are added at a material-ball ratio of 1:2, the ball diameter is 1mm to 8mm, and grinding balls of different diameters are added in equal parts and proportions, the rotation speed is 900r / min, and the ball milling is performed for 6h; Step S5, drying the ball-milled product in an oven at 100° C., and obtaining a catalyst precursor C after grinding; Step S6, placing the catalyst precursor C obtained in step S5 in a crucible and placing it in a muffle furnace, heating it to 500° C. at a rate of 5° C. / min, keeping the temperature for 2 hours, and cooling it in the furnace to obtain a highly dispersed powder catalyst IrO2 / SiO2 with a carrier structure; Step S7: using a centrifuge to centrifuge and clean and dry the powdered catalyst several times using deionized water and anhydrous ethanol in sequence, and finally obtaining a metal or metal oxide with an ultra-dispersed structure.

6. A method for preparing a supported noble metal oxide, characterized in that: The specific steps include: Step S1, preparing carrier dispersion solution A: 20 mL of 0.25 mg / mL conductive carbon black XC72R solution, the solvent is ethanol; Step S2, adding 20 μL of hydrogen peroxide, 20 μL of acetic acid, and 20 μL of deionized water to the carrier dispersion A obtained in step S1, and placing it in an ultrasonic environment with an ultrasonic frequency of 28 Hz and a temperature of 50° C. for 30 minutes to make the carrier evenly dispersed in the solvent, to obtain a carrier dispersion A adjusted to pH 6; Step S3, preparing precursor solution B: 1 mmol / L chloroplatinic acid solution, the solvent is ethanol; Step S4, the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 are mixed at a ratio of 20% of the mass of the metal element to the mass of the carrier, and the solution with uniform composition after stirring is poured into a ball mill, and the materials are added at a material-ball ratio of 1:1, the ball diameter is 1mm to 8mm, and grinding balls of different diameters are added in equal parts and proportions, the rotation speed is 1000r / min, and the ball milling is carried out for 10h; Step S5, drying the ball-milled product in an oven at 100° C., and obtaining a catalyst precursor C after grinding; Step S6, placing the catalyst precursor C obtained in step S5 in a crucible and placing it in a muffle furnace, heating it to 550° C. at a rate of 5° C. / min, keeping the temperature for 2 hours, and cooling it in the furnace to obtain a highly dispersed powder catalyst Pt / C with a carrier structure; Step S7: using a centrifuge to centrifuge and clean and dry the powdered catalyst several times using deionized water and anhydrous ethanol in sequence, and finally obtaining a metal or metal oxide with an ultra-dispersed structure.

7. A method for preparing a supported noble metal oxide, characterized in that: The specific steps include: Step S1, preparing carrier dispersion solution A: 20 mL of 0.4 mg / mL TiO2 solution with a particle size of 1 μm, and the solvent is ethanol; Step S2, adding 40 μL of acetic acid and 20 μL of deionized water to the carrier dispersion A obtained in step S1, and placing it in an ultrasonic environment with an ultrasonic frequency of 40 Hz and a temperature of 45° C. for 60 min to uniformly disperse the carrier in the solvent, and obtaining an adjusted carrier dispersion A with a pH of 5.5; Step S3, preparing precursor solution B: 1 mmol / L chloroiridic acid solution, the solvent is ethanol; Step S4, the carrier dispersion A obtained in step S2 and the precursor solution B obtained in step S3 are mixed at a ratio of 50% of the mass of the metal element to the mass of the carrier, and the solution with uniform composition after stirring is poured into a ball mill, and the materials are added at a material-ball ratio of 1:4, the ball diameter is 1mm to 8mm, and grinding balls of different diameters are added in equal parts and proportions, the rotation speed is 1000r / min, and the ball milling is carried out for 10h; Step S5, drying the ball-milled product in an oven at 100° C., and obtaining a catalyst precursor C after grinding; Step S6, placing the catalyst precursor C obtained in step S5 in a crucible and placing it in a muffle furnace, heating it to 450° C. at a rate of 5° C. / min, keeping the temperature for 1 hour, and cooling it in the furnace to obtain a highly dispersed powder catalyst IrO2@TiO2 with a carrier structure; Step S7: using a centrifuge to centrifuge and clean and dry the powdered catalyst several times using deionized water and anhydrous ethanol in sequence, and finally obtaining a metal or metal oxide with an ultra-dispersed structure.

8. A supported noble metal oxide, characterized in that: Obtained by the preparation method according to any one of claims 1 to 7.