A method for preparing photocatalytic materials using ternary precursor high magnetic waste and its application
By coating and modifying dopamine and loading titanium dioxide on the ternary precursor high-magnetic waste, combined with the magnetic solid-liquid separation method, a photocatalytic material with excellent photocatalytic performance and magnetic recovery was prepared, which solved the problems of resource waste and environmental pollution. Reduces photocatalyst cost and is suitable for wastewater treatment.
Patent Information
- Application Number
- CN202310088131.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-01-19
AI Technical Summary
The existing technology cannot effectively utilize the ternary precursor high-magnetic waste as photocatalyst material, resulting in resource waste and environmental pollution. Moreover, the cost of commonly used photocatalyst carriers is high and there is a lack of convenient recycling methods.
By coating and modifying the ternary precursor high-magnetic waste with dopamine solution and mixing it with titanium dioxide, the photocatalytic material is prepared using the magnetic solid-liquid separation method to retain high magnetic responsiveness and achieve improved photocatalytic performance and magnetic recovery.
The prepared photocatalytic material has excellent photocatalytic performance, reduces the cost of the photocatalyst carrier, realizes convenient magnetic recovery, is suitable for wastewater treatment, and avoids waste of resources and environmental pollution.
Smart Images

Figure CN116371465B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste recycling, and in particular to a method for preparing a photocatalytic material by utilizing ternary precursor high-magnetic waste and its application. Background Art
[0002] Lithium-ion power batteries are currently the most widely used power batteries. However, the performance of lithium battery positive electrode materials is largely affected by ternary precursors, so the research on ternary precursors has received more and more attention. At present, in the production process of ternary precursors, due to the limitations of existing technology and production lines, it is inevitable that the produced ternary precursors are rich in highly magnetic impurities. Therefore, it is necessary to remove these highly magnetic wastes through demagnetization screening to ensure that the physical and chemical properties of the ternary precursors are not affected. As the production capacity increases, the removed high-magnetic waste continues to accumulate, which not only leads to a waste of resources, but also leads to space occupation and environmental pollution.
[0003] At present, the high magnetic waste of ternary precursor is generally processed to recover its metal elements or recycled as raw materials to prepare precursors. For example, CN108199106A, CN103526028A, and CN111003734A all process high magnetic waste and recycle its metal elements; CN107902704A separates the magnetic substances in the high magnetic materials and prepares them into positive electrode precursor products.
[0004] Highly magnetic waste retains the advantages of large contact area and high specific surface area of the ternary precursor and has certain adsorption sites. Currently, there is no existing technology to recycle it for the preparation of photocatalyst materials. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method and application of preparing photocatalytic materials using ternary precursor high magnetic waste. The photocatalytic material has excellent photocatalytic performance and magnetic recovery, and can be widely used in wastewater treatment.
[0006] To achieve the above object, in a first aspect of the present invention, the present invention provides a method for preparing a photocatalytic material using a ternary precursor high magnetic waste, comprising the following steps:
[0007] The ternary precursor high magnetic waste is coated and modified with a dopamine solution to obtain a ternary precursor high magnetic waste modified with a polydopamine coating layer;
[0008] The ternary precursor high magnetic waste modified by the polydopamine coating layer is evenly mixed with titanium dioxide, so that the titanium dioxide grows on the surface of the polydopamine coating layer, and the photocatalytic material is obtained by magnetic separation of solid and liquid and drying.
[0009] As a preferred embodiment of the present invention, the preparation process of the dopamine solution includes: adding dopamine hydrochloride into water, mixing evenly, and then adding Tris buffer to adjust the pH to 8-11 to obtain the dopamine solution.
[0010] As a preferred embodiment of the present invention, the material-liquid ratio of dopamine hydrochloride to water is (0.5-4) g:1L.
[0011] As a preferred embodiment of the present invention, the solid-liquid ratio of the ternary precursor high magnetic waste to the dopamine solution is 1g: (100-200)ml.
[0012] As a preferred embodiment of the present invention, the weight ratio of the ternary precursor high magnetic waste modified by the polydopamine coating layer and titanium dioxide is (3-6):1.
[0013] As a preferred embodiment of the present invention, the ternary precursor high magnetic waste modified by the polydopamine coating layer is evenly mixed with titanium dioxide in a strong alkaline solution by a hydrothermal reaction.
[0014] As a preferred embodiment of the present invention, the strong alkaline solution includes at least one of a sodium hydroxide solution, a potassium hydroxide solution, a barium hydroxide solution, and a calcium hydroxide solution.
[0015] As a preferred embodiment of the present invention, the temperature of the hydrothermal reaction is 120 to 160° C., and the time is 12 to 24 hours.
[0016] As a preferred embodiment of the present invention, the magnetic field strength of the magnetic separation solid-liquid separation is 10000-15000 GS.
[0017] In a second aspect of the present invention, the present invention provides the use of the photocatalytic material prepared by the method described above in wastewater treatment.
[0018] The beneficial effects of the present invention are as follows: (1) the present invention uses the ternary precursor high magnetic waste as a template, coats and modifies it, and then allows titanium dioxide nanoparticles to be in-situ loaded and grown on the surface of the polydopamine coating layer of the ternary precursor, and finally separates the solid and liquid by magnetic separation and dries it to obtain a material with excellent photocatalytic performance and magnetic recovery, which can be widely used in wastewater treatment; (2) the present invention uses the ternary precursor high magnetic waste accumulated in the ternary precursor production process as a carrier, which greatly reduces the high cost of the currently commonly used photocatalyst carriers, achieves the purpose of cost reduction, energy saving, and green environmental protection, and the prepared photocatalytic material retains the high magnetic responsiveness of the ternary precursor high magnetic waste itself, so that the magnetic properties of the solid photocatalytic material can be realized by applying an external electromagnetic field. Recycling does not require additional loading of other magnetic functional components, the process is convenient, and the cost is further reduced; (3) The photocatalytic material prepared by the present invention has better photocatalytic performance than the single ternary precursor high magnetic waste and the single nano titanium dioxide, and can better catalyze the degradation of wastewater. Among them, the prepared photocatalytic material uses dopamine modification to provide highly active functional groups, and through the synergistic effect of the ternary precursor high magnetic waste carrier and the nano titanium dioxide particles, it can efficiently remove organic pollutants in the water. In addition, the micron-level size of the ternary precursor high magnetic material can realize the convenient recovery of the photocatalyst, and the active components will not agglomerate and disperse in the water to cause secondary pollution, and it is suitable for mass transfer enhancement in large areas of water in wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a diagram showing the catalytic degradation of methylene blue by the photocatalyst material prepared in Example 1 under light and dark conditions;
[0020] Figure 2 The photocatalyst material prepared in Example 1 is a diagram before and after the catalytic degradation of methylene blue;
[0021] Figure 3 This is the XRD pattern of the photocatalytic material prepared in Example 1;
[0022] Figure 4 This is the XPS graph of the photocatalytic material prepared in Example 1;
[0023] Figure 5 This is the hysteresis loop diagram of the photocatalytic material prepared in Example 1. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0026] In the present invention, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0027] In the present invention, there is no particular limitation on the specific dispersion and stirring treatment methods.
[0028] The reagents or instruments used in the present invention without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.
[0029] The embodiment of the present invention provides a method for preparing a photocatalytic material using a ternary precursor high magnetic waste, comprising the following steps:
[0030] The ternary precursor high magnetic waste is coated and modified with a dopamine solution to obtain a ternary precursor high magnetic waste modified with a polydopamine coating layer;
[0031] The ternary precursor high magnetic waste modified by the polydopamine coating layer is evenly mixed with titanium dioxide, so that the titanium dioxide grows on the surface of the polydopamine coating layer, and the photocatalytic material is obtained by magnetic separation of solid and liquid and drying.
[0032] The present invention uses a ternary precursor high magnetic waste as a template, coats and modifies it, and then allows titanium dioxide nanoparticles to grow on the surface of the polydopamine coating layer of the ternary precursor through in-situ loading, and finally separates the solid and liquid through magnetic separation and dries, thereby obtaining a product with excellent photocatalytic performance and magnetic recovery, which can be widely used in wastewater treatment.
[0033] The present invention uses the accumulated high-magnetic waste of the ternary precursor in the production process of the ternary precursor as a carrier, which greatly reduces the high cost of the currently commonly used photocatalyst carriers, achieving the purpose of cost reduction, energy saving, and green environmental protection.
[0034] It should be noted that the ternary precursor high magnetic waste is the waste generated in the ternary precursor production process in the field, wherein the ternary precursor high magnetic waste is a mixture of nickel cobalt manganese hydroxide and magnetic foreign matter; the main components of the ternary precursor high magnetic waste used in the method for preparing photocatalytic materials of the present invention are not specifically limited, as long as it has high magnetic responsiveness, that is, as long as the ternary precursor high magnetic waste contains Ni, Co, Mn, and MI, the method of the present invention can be used to prepare photocatalytic materials.
[0035] Exemplarily, the components of the ternary precursor high magnetic waste are mainly as follows (by weight): 22% Ni, 20.5% Co, 32.5% Mn, MI>200ppm. The present invention is not limited to the listed values, and other values of Ni, Co, Mn, and MI are also applicable to the present invention.
[0036] Among them, MI refers to magnetic metal foreign matter, which is a general term for magnetic single substances, alloys, and oxides (excluding Ni), such as Fe, Cr, Zn and their corresponding alloys and oxides.
[0037] The prepared photocatalytic material retains the high magnetic responsiveness of the ternary precursor high magnetic waste itself, so that magnetic recovery of solid photocatalytic materials can be achieved through an external electromagnetic field, without the need for additional loading of other magnetic functional components. The process is convenient and further reduces costs.
[0038] The photocatalytic material prepared by the present invention has better photocatalytic performance than single ternary precursor high magnetic waste and single nano titanium dioxide, and can better catalytically degrade wastewater. The prepared photocatalytic material uses dopamine modification to provide highly active functional groups, and efficiently removes organic pollutants in water through the synergistic effect of the ternary precursor high magnetic waste carrier and the nano titanium dioxide particles. In addition, the micron-scale size of the ternary precursor high magnetic material can realize convenient recovery of the photocatalyst, and the active components will not agglomerate and disperse in the water to cause secondary pollution. The photocatalytic material is suitable for mass transfer enhancement in large areas of water in wastewater treatment.
[0039] In one embodiment, the preparation process of the dopamine solution includes: adding dopamine hydrochloride into water, mixing evenly, and then adding Tris buffer to adjust the pH to 8-11 to obtain the dopamine solution.
[0040] It should be noted that the Tris buffer is a Tris-HCl buffer.
[0041] In one embodiment, the material-liquid ratio of dopamine hydrochloride to water is (0.5-4) g:1L, preferably (0.5-2) g:1L.
[0042] In one embodiment, the solid-liquid ratio of the ternary precursor high magnetic waste to the dopamine solution is 1 g: (100-200) ml.
[0043] In one embodiment, the weight ratio of the ternary precursor high magnetic waste modified by the polydopamine coating layer and titanium dioxide is (3-6):1.
[0044] Exemplarily, after the coating modification, magnetic separation and drying are also included. The specific methods of magnetic separation and drying can be carried out by filtration and drying according to actual specific circumstances in the art.
[0045] For example, the drying temperature may be 40-60°C.
[0046] In one embodiment, the ternary precursor high magnetic waste modified with a polydopamine coating layer is evenly mixed with titanium dioxide in a strong alkaline solution by a hydrothermal reaction.
[0047] In one embodiment, the strong alkaline solution includes at least one of a sodium hydroxide solution, a potassium hydroxide solution, a barium hydroxide solution, and a calcium hydroxide solution.
[0048] Exemplarily, the strong alkaline solution is 8-10 mol / L sodium hydroxide solution, and the material-to-solid ratio of the strong alkaline solution to the polydopamine coating-modified ternary precursor high magnetic waste is (100-200) ml:1 g.
[0049] Exemplarily, the temperature of the hydrothermal reaction is 120-160° C., and the time is 12-24 hours.
[0050] In one embodiment, the magnetic field strength of magnetic separation solid-liquid separation is 10000-15000 GS.
[0051] One embodiment of the present invention provides the use of the photocatalytic material prepared above in wastewater treatment.
[0052] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.
[0053] Example 1
[0054] A method for preparing a photocatalytic material using ternary precursor high magnetic waste comprises the following steps:
[0055] (1) Add 4 g of dopamine hydrochloride to 2000 mL of pure water to prepare a 2 mg / mL dopamine hydrochloride solution, then add 0.1 mol / L Tris buffer to adjust the pH to 8 to obtain a dopamine solution for standby use;
[0056] (2) 10 g of high magnetic waste material (a mixture of nickel-cobalt-manganese hydroxide and magnetic foreign matter, wherein Ni:Co:Mn=22%:20.5%:32.5%, MI>200 ppm) screened out from the ternary precursor production workshop was placed in a dopamine solution to be used, stirred at room temperature for 8 h, and sent to a magnetic separator for magnetic separation at a magnetic field strength of 10,000 GS to achieve solid-liquid separation, and then placed in a vacuum drying oven and dried at 60° C. to obtain a ternary precursor high magnetic waste material modified with a polydopamine coating layer;
[0057] (3) 10 g of the ternary precursor high magnetic waste modified with a polydopamine coating layer and 2 g of P25 nano-titanium dioxide were placed in 200 ml of a 10 mol / L sodium hydroxide solution and reacted hydrothermally at 160 ° C for 24 h. The mixed solution was sent to a magnetic separator for magnetic separation at a magnetic field strength of 12000 GS to achieve solid-liquid separation, and then placed in a vacuum drying oven and dried at 60 ° C to obtain a photocatalytic material.
[0058] The photocatalytic material prepared in this example was added to a methylene blue solution at a liquid-to-solid ratio of 1:2000. The degradation rate was recorded every 10 minutes under light and dark conditions. The degradation curve within 60 minutes was as shown in FIG. Figure 1 As shown in the figure, the degradation before and after 60 minutes under light conditions is as follows Figure 2 shown.
[0059] The XRD spectrum of the photocatalytic material prepared in this example is as follows Figure 3 As shown, from Figure 3 It can be seen that an obvious sharp characteristic peak of TiO2 appears at the corresponding position, which belongs to anatase TiO2, indicating that the prepared photocatalyst material has successfully loaded nano-titanium dioxide particles.
[0060] The XPS spectrum of the photocatalytic material prepared in this example is as follows Figure 4 As shown, from Figure 4 It can be seen that the ternary precursor high magnetic waste-based photocatalytic functional material contains 4 elements, among which the N element comes from the modification of the polydopamine coating layer, and the Ti element comes from the loading of nano-TiO2, which further illustrates that the photocatalytic material prepared by this method has successfully been modified with dopamine and loaded with nano-titanium dioxide particles.
[0061] The hysteresis loop of the photocatalytic material prepared in this example is shown in Figure 5 As shown, from Figure 5 It can be seen that the hysteresis loop is "S"-shaped, the magnetization curve and the demagnetization curve are consistent, and there is no hysteresis phenomenon, the remanence and coercive force are equal to 0, indicating that the prepared ternary precursor high magnetic waste-based photocatalyst has excellent magnetic responsiveness.
[0062] Example 2
[0063] A method for preparing a photocatalytic material using ternary precursor high magnetic waste comprises the following steps:
[0064] (1) adding 4 g of dopamine hydrochloride into 1000 mL of pure water to prepare a 4 mg / mL dopamine hydrochloride solution, and then adding 0.1 mol / L Tris buffer to adjust the pH to 11 to obtain a dopamine solution for standby use;
[0065] (2) 8 g of high magnetic waste material (a mixture of nickel-cobalt-manganese hydroxide and magnetic foreign matter, wherein Ni:Co:Mn=22%:20.5%:32.5%, MI>200 ppm) screened out from the ternary precursor production workshop was placed in a dopamine solution to be used, stirred at room temperature for 8 h, and sent to a magnetic separator for magnetic separation at a magnetic field strength of 10,000 GS to achieve solid-liquid separation, and then placed in a vacuum drying oven and dried at 60° C. to obtain a ternary precursor high magnetic waste material modified with a polydopamine coating layer;
[0066] (3) 8 g of the ternary precursor high magnetic waste modified with a polydopamine coating layer and 6 g of P25 nano-titanium dioxide were placed in 200 ml of a 10 mol / L sodium hydroxide solution and reacted hydrothermally at 160 ° C for 24 h. The mixed solution was sent to a magnetic separator for solid-liquid separation at a magnetic field strength of 12000 GS, and then placed in a vacuum drying oven and dried at 60 ° C to obtain a photocatalytic material.
[0067] Example 3
[0068] A method for preparing a photocatalytic material using ternary precursor high magnetic waste comprises the following steps:
[0069] (1) 4 g of dopamine hydrochloride was added to 200 mL of pure water to prepare a 0.5 mg / mL dopamine hydrochloride solution, and then 0.1 mol / L Tris buffer was added to adjust the pH to 9 to obtain a dopamine solution for standby use;
[0070] (2) 3 g of high magnetic waste material (a mixture of nickel-cobalt-manganese hydroxide and magnetic foreign matter, wherein Ni:Co:Mn=22%:20.5%:32.5%, MI>200 ppm) screened out from the ternary precursor production workshop was placed in a dopamine solution to be used, stirred at room temperature for 8 h, and sent to a magnetic separator for magnetic separation at a magnetic field strength of 10,000 GS to achieve solid-liquid separation, and then placed in a vacuum drying oven and dried at 60° C. to obtain a ternary precursor high magnetic waste material modified with a polydopamine coating layer;
[0071] (3) 3 g of the ternary precursor high magnetic waste modified with a polydopamine coating layer and 1 g of P25 nano-titanium dioxide were placed in 200 ml of a 10 mol / L sodium hydroxide solution and reacted hydrothermally at 160 ° C for 24 h. The mixed solution was sent to a magnetic separator for magnetic separation at a magnetic field strength of 12000 GS to achieve solid-liquid separation, and then placed in a vacuum drying oven and dried at 60 ° C to obtain a photocatalytic material.
[0072] Comparative Example 1
[0073] Comparative Example 1 is a ternary precursor high magnetic waste.
[0074] Comparative Example 2
[0075] Comparative Example 2 is P25 type nano titanium dioxide.
[0076] Test Case
[0077] The materials of Examples 1 to 3 and Comparative Examples 1 to 2 were added to a methylene blue solution (solid-to-liquid ratio of 1:2000), respectively. The degradation rates of the methylene blue solution were tested for 10 min and 60 min under light. The test results are shown in Table 1.
[0078] Table 1
[0079] 10min degradation rate / % 60min degradation rate / % Example 1 58.69 96.71 Example 2 57.59 97.13 Example 3 59.07 97.34 Comparative Example 1 3.29 4.11 Comparative Example 2 45.39 86.91
[0080] It can be seen from the table that the photocatalytic material of the present invention has excellent photocatalytic performance and can effectively degrade methylene blue, wherein the ternary precursor high magnetic waste carrier and the nano titanium dioxide particles have a synergistic effect.
[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing photocatalytic materials using ternary precursor high magnetic waste, characterized in that: The following steps are involved: The ternary precursor high magnetic waste is coated and modified with a dopamine solution to obtain a ternary precursor high magnetic waste modified with a polydopamine coating layer; The ternary precursor high magnetic waste modified by the polydopamine coating layer is mixed evenly with titanium dioxide, so that the titanium dioxide grows on the surface of the polydopamine coating layer, and the solid-liquid separation is performed by magnetic separation, and the photocatalytic material is obtained by drying. The solid-liquid ratio of the ternary precursor high magnetic waste to the dopamine solution is 1g: (100-200)ml; The weight ratio of the polydopamine coating modified ternary precursor high magnetic waste and titanium dioxide is (3-6):1; The polydopamine coating layer modified ternary precursor high magnetic waste and titanium dioxide are mixed evenly in a strong alkaline solution in a hydrothermal reaction manner; The ternary precursor high magnetic waste is a mixture of nickel, cobalt, manganese hydroxide and magnetic foreign matter.
2. The method for preparing photocatalytic materials using ternary precursor high magnetic waste according to claim 1, characterized in that: The preparation process of the dopamine solution comprises: adding dopamine hydrochloride into water, mixing evenly, and then adding Tris buffer to adjust the pH to 8-11 to obtain the dopamine solution.
3. The method for preparing photocatalytic materials using ternary precursor high magnetic waste according to claim 2, characterized in that: The material-liquid ratio of the dopamine hydrochloride to water is (0.5-4) g:1L.
4. The method for preparing photocatalytic materials using ternary precursor high magnetic waste according to claim 1, characterized in that: The strong alkaline solution includes at least one of a sodium hydroxide solution, a potassium hydroxide solution, a barium hydroxide solution, and a calcium hydroxide solution.
5. The method for preparing photocatalytic materials using ternary precursor high magnetic waste according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 120-160° C. and the time is 12-24 hours.
6. The method for preparing photocatalytic materials using ternary precursor high magnetic waste according to claim 1, characterized in that: The magnetic field strength of the magnetic separation solid-liquid separation is 10000-15000 GS.
7. Use of the photocatalytic material prepared by the method according to any one of claims 1 to 6 in wastewater treatment.