Preparation method and application of microporous zirconium-based metal-organic framework material
By preparing the microporous zirconium-based metal organic framework material DUT-67, the problems of low adsorption capacity, poor stability and high cost of existing MOF materials in deep flue gas desulfurization and chlorofluorocarbon capture in the atmosphere have been solved, achieving high efficiency and low cost. Gas separation performance, suitable for advanced treatment of industrial flue gas and chlorofluorocarbons in the atmosphere.
Patent Information
- Application Number
- CN202211685644.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Existing MOF adsorbent materials have problems with low adsorption capacity, poor chemical stability, irreversible adsorption, poor separation performance, difficult regeneration and high synthesis costs in terms of deep desulfurization of flue gas and capture of chlorofluorocarbons in the atmosphere, making it difficult to achieve industrial preparation.
A method for preparing DUT-67, a microporous zirconium-based metal-organic framework material, is used to prepare a highly crystalline and high-purity porous material through the mixed reaction of polar organic solvents and formic acid with zirconium salts and thiophenedicarboxylic acid organic ligands. It has a three-dimensional network structure and rich pore structure, can efficiently adsorb SO2, R22 and R134a, and shows extremely high physical and chemical stability and hydrothermal stability.
It achieves efficient deep SO2 removal and selective capture of R22 and R134a, reduces regeneration energy consumption and synthesis costs, has industrial application potential, and promotes the application of MOF materials in other industrial gas separation fields.
Smart Images

Figure CN116376037B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of gas adsorption and sub-technology, and more specifically, relates to a preparation method and application of a microporous zirconium-based metal organic framework material. Background Art
[0002] The extensive use of fossil energy and refrigerants has released a huge amount of SO2 and chlorofluorocarbon refrigerants into the atmosphere, leading to very serious environmental problems such as acid rain, haze, greenhouse effect, and global warming, which have seriously threatened human survival, health, and sustainable development. As of 2018, 62.7Mt of SO2 has been emitted into the atmosphere. In addition to being oxidized by ozone and oxygen in the atmosphere into SO3 and dissolved in water vapor to form acid rain, SO2 entering the atmosphere will also react with ammonia in the atmosphere to produce PM 2.5, i.e., highly toxic haze particles. The former will cause acidification of water bodies and soil and poison surface vegetation, while the latter will enter the human lungs through the breathing process, causing serious respiratory system diseases and seriously endangering human health. In addition to consuming ozone in the atmosphere and causing ozone layer holes, most of the chlorofluorocarbons entering the atmosphere are greenhouse gases themselves, with a global warming potential (GWP) that is tens to thousands of times that of CO2, which will seriously aggravate global warming and accelerate the melting of polar glaciers and the rise of sea levels. Therefore, deep desulfurization of flue gas and efficient capture and recovery of chlorofluorocarbons leaked during chlorofluorocarbon production or dismantling of refrigeration equipment are urgent issues to be solved in the industry.
[0003] At present, traditional flue gas desulfurization in industry usually adopts limestone wet scrubbing or amine-based adsorbent treatment. However, these adsorption processes are usually irreversible and accompanied by energy-intensive processes, generating a large amount of waste liquid and waste solid. In addition, the limestone elution process cannot completely adsorb SO2, and there will always be 0.015-0.045% SO2 remaining, which will significantly affect the activity of adsorbents for removing carbon dioxide in other flue gas purification processes, and will also make the adsorbents used to reduce NO x Or the noble metal-based catalyst for catalytic combustion of CH4 is deactivated. As for the refrigerant leaked from the production workshop, there is no relevant capture and recovery technology. For the recovery of chlorofluoroalkane refrigerants in abandoned refrigeration equipment, the industry mainly adopts cooling method, compression condensation method, adsorption method, liquid push, pull method and composite recovery method. However, the above-mentioned traditional flue gas desulfurization and refrigerant recovery technologies have the disadvantages of high recovery cost and high energy consumption.
[0004] In comparison, the method based on the adsorption of porous materials and the deep separation of SO2 in flue gas and chlorofluorocarbons in the atmosphere under low energy consumption conditions is more energy-saving and environmentally friendly. Metal-organic framework materials (MOFs), as a new type of porous material that has developed most rapidly in recent years, have both inorganic metal nodes and organic bridging ligands, realizing the orderly unification of metal elements and organic ligands, and have extremely high specific surface area, huge pore volume, and a variety of topologies. They have the advantages of designable and controllable structures and functionalized solid frameworks. In the past decade, they have shown great application potential in the selective adsorption and separation of hydrocarbon gases, carbon capture, hydrogen / methane storage, and natural gas purification. For example, Chinese patent application CN105727736A discloses a metal organic framework material MOF-5 for removing sulfur dioxide, and its maximum sulfur dioxide removal amount is 1.5mmol / g; Chinese patent application CN115160586A discloses a mesoporous metal organic framework material that can simultaneously realize the modification of pore size and functional groups of mesoporous MOF, and the MOF material has strong adsorption and storage capacity for Freon gas. Although MOF materials have made certain progress in the adsorption and separation of SO2 and the capture of chlorofluorocarbons in the atmosphere, the current research results are still few and not in-depth. Many MOFs still have the disadvantages of low adsorption capacity, poor chemical stability, irreversible SO2 adsorption, and high synthesis cost. In addition, the research is not in-depth enough, and the interference of other coexisting gases and water vapor is rarely considered, which is far from the actual separation needs and separation scenarios. In addition to requiring MOFs as solid adsorbents to have excellent gas separation performance, their physical and chemical stability and hydrothermal stability are also very important for their actual industrial applications. Moreover, most of the MOFs materials reported so far for deep removal of SO2 and capture and separation of chlorofluoroalkanes in the atmosphere have extremely high raw material and synthesis costs, making them difficult to produce or prepare on a large scale and unable to meet the actual needs of industrial applications.
[0005] Therefore, there is an urgent need to provide a MOF material with high separation performance, high stability, low regeneration energy consumption and low cost, and to achieve deep flue gas desulfurization and efficient capture and recovery of chlorofluoroalkanes in the atmosphere. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of existing MOF-type adsorption materials, such as low adsorption capacity, poor chemical stability, irreversible adsorption, poor separation performance, difficult regeneration, high synthesis cost and difficulty in industrial preparation, and to provide a method for preparing a microporous zirconium-based metal organic framework material (DUT-67) with high separation performance, high stability, low regeneration energy consumption and low cost.
[0007] Another object of the present invention is to provide an application of the method for preparing the microporous zirconium-based metal organic framework material.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] A preparation method of a microporous zirconium-based metal organic framework material comprises the following steps: fully mixing a polar organic solvent and formic acid, then adding a zirconium salt and a thiophene dicarboxylic acid organic ligand, fully mixing, heating at 50-160° C. to complete the reaction, and post-treating to obtain the material;
[0010] Wherein, the polar organic solvent is N,N-dimethylacetamide (DMAC) or N,N-dimethylformamide (DMF);
[0011] The volume ratio of the polar organic solvent to formic acid is 2:0.5-2;
[0012] The molar ratio of the zirconium salt to the thiophene dicarboxylic acid organic ligand is 1:0.67-1.5.
[0013] After a long period of exploration, the present invention has prepared a porous material DUT-67 with high crystallinity, high purity and a three-dimensional network structure. The preparation method has been verified in the laboratory at the kg level and can stably prepare DUT-67. In addition, the synthesis process is simple, the cost is low, and it has extremely high industrial application potential and value.
[0014] Further, the molecular formula of the microporous zirconium-based metal organic framework material is Zr6O8(OH)8X4;
[0015] Wherein, X is a thiophenedicarboxylic acid organic ligand.
[0016] The framework of DUT-67 obtained by the preparation method of the present invention has a rich pore structure and extremely high porosity. Each metal cluster in the framework has 8 terminal H2O / OH - This group has a very high adsorption affinity for SO2, R22 and R134a. It can form hydrogen bonds with oxygen on sulfur dioxide molecules, Cl and F atoms on R22 and R134a molecules through H atoms, and can also form non-traditional hydrogen bonds with H atoms on the three molecules through O atoms, thereby enhancing its adsorption affinity and separation selectivity for these three gas molecules. It has excellent SO2 deep removal ability and selective capture performance of R22 and R134a, and can achieve deep desulfurization of industrial flue gas and selective separation and capture of low-concentration R22 and R134a in the atmosphere. In addition, DUT-67 exhibits extremely high physical and chemical stability and hydrothermal stability. It can still maintain its structural integrity at a high temperature of 225°C and after being immersed in 85°C hot water, seawater, acidic or alkaline solutions.
[0017] Preferably, the zirconium salt is any one of ZrOCl2, ZrCl4, and ZrO(NO3)2.
[0018] More preferably, the zirconium salt is any one of ZrOCl2·H2O, ZrOCl2·8H2O, ZrCl4, and ZrO(NO3)2·xH2O. Except for ZrCl4, some zirconium salts without crystal water, such as ZrOCl2, are expensive. Based on cost considerations, the present application selects a relatively cheap zirconium salt with crystal water.
[0019] Most preferably, the zirconium salt is ZrOCl2·8H2O.
[0020] Preferably, the thiophenedicarboxylic acid organic ligand is 2,5-thiophenedicarboxylic acid.
[0021] Preferably, the mixing ratio of the total volume of the polar organic solvent and formic acid to the total mass of the zirconium salt and the thiophene dicarboxylic acid organic ligand is 6.5 mL: 60-450 mg. When the microporous zirconium-based metal-organic framework material is produced in small batches, and large-sized DUT-67 single crystals are desired for structural analysis, and the in-situ X-ray single crystal diffraction technique is used to analyze the gas adsorption mechanism, that is, when the mass of the zirconium salt and the thiophene dicarboxylic acid organic ligand used for the reaction is less than 200 mg, the mixing ratio of the total volume of the polar organic solvent and formic acid to the total mass of the zirconium salt and the thiophene dicarboxylic acid organic ligand is 6.5 mL: 60-200 mg; when synthesizing high-purity crystalline powder DUT-67, the mixing ratio of the total volume of the polar organic solvent and formic acid to the total mass of the zirconium salt and the thiophene dicarboxylic acid organic ligand is It is 6.5mL:200~450mg; when an industrial reactor is used to produce the microporous zirconium-based metal-organic framework material of Kg level or above in a single time by stirring and reflux, that is, the mass of the zirconium salt and the thiophene dicarboxylic acid organic ligand used for the reaction is greater than 1Kg, the mixing ratio of the total volume of the polar organic solvent and formic acid to the total mass of the zirconium salt and the thiophene dicarboxylic acid organic ligand is 6.5mL:260~450mg. The ratio of the volume of the aforementioned organic solvent to the total mass of the metal salt and the organic ligand only affects the crystal size and morphology of the synthesized DUT-67, does not affect the framework structure, and does not change the product purity and phase.
[0022] Preferably, the time required for the reaction to be complete is 12 to 150 hours.
[0023] Preferably, the temperature at which the polar organic solvent and formic acid are fully mixed is 25-50°C.
[0024] Preferably, the sufficient mixing time is 1 to 60 minutes.
[0025] Furthermore, the thorough mixing method includes shaking, stirring and ultrasound.
[0026] Furthermore, the sufficient mixing method is ultrasound.
[0027] Preferably, the post-treatment operation further includes filtration, washing, soaking and drying.
[0028] Specifically, the post-treatment operation is as follows: after the reaction is complete, the supernatant is removed, DMF is added thereto, crystals on the bottle wall are removed by ultrasound, and then a solid product is obtained by suction filtration, the obtained solid product is first washed with DMF for 3 to 5 times to wash away the unreacted zirconium salt or 2,5-thiophene dicarboxylic acid organic ligand in the pores, and then soaked in deionized water for 1 day, and then washed with any one of anhydrous methanol, ethanol, or acetone for 3 to 5 times and soaked for 3 to 5 days, and the fresh soaking solvent is replaced 6 times a day, and after the DMF in the pores is completely replaced as the soaking solvent, a drying treatment is performed.
[0029] Furthermore, the drying is performed at room temperature first and then vacuum drying. The purpose of vacuum drying is to activate DUT-67, that is, to remove organic solvents such as DMF / DMAC or formic acid and low-boiling point organic solvents (such as anhydrous methanol, ethanol, acetone, etc.) used for exchange and removal in the pores of the DUT-67 framework, and to empty the pores of DUT-67 for adsorption of gas molecules such as SO2, R22 and R134a.
[0030] Specifically, the drying is first drying at room temperature for 12 hours, and then vacuum drying at a temperature of 50-120° C. and a vacuum degree of 0.001-0.1 torr for 12 hours to obtain an activated microporous zirconium-based metal organic framework material, namely, activated DUT-67.
[0031] In addition, the present invention also provides application of the preparation method in adsorption and separation of halogenated alkane gas and sulfur dioxide.
[0032] Preferably, the halogenated alkane gas includes difluorochloromethane (R22), 1,1,1,2-tetrafluoroethane (R134a), sulfur hexafluoride and carbon tetrafluoride, monofluorotrichloromethane, hexafluoroethane, tetrafluoromethane, octafluoropropane, dichlorodifluoromethane, chlorotrifluoromethane, pentafluorochloroethane, trifluoromethane.
[0033] More preferably, the halogenated alkane gas is difluorochloromethane and 1,1,1,2-tetrafluoroethane.
[0034] The present invention has the following beneficial effects: the microporous zirconium-based metal organic framework material DUT-67 described in the present invention is constructed by coordination between zirconium salt and organic ligand, and its synthesis method is simple and low in cost. The DUT-67 obtained by this method is a porous material with high crystallinity, high purity and three-dimensional network structure, and has excellent SO2 deep removal ability and selective capture performance of R22 and R134a, and has extremely high physical and chemical stability and hydrothermal stability, which provides a new method for improving the deep desulfurization of flue gas of porous solid adsorbent materials and the selective capture and separation of chlorofluoroalkanes in the atmosphere, and also provides different ways to develop new MOF materials with high separation performance, high stability and low cost, which is conducive to promoting and expanding the application of MOF materials in other industrial gas separation fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Schematic diagram of the microscopic crystal structure of DUT-67 prepared in Example 1.
[0036] Figure 2 is the X-ray diffraction (PXRD) pattern of DUT-67 prepared in Example 1.
[0037] Figure 3 is the 77K nitrogen isothermal full adsorption curve of DUT-67 prepared in Example 1 ( Figure 3 a) and pore size distribution diagram ( Figure 3 b).
[0038] Figure 4 The PXRD patterns of DUT-67 prepared in Example 1 before and after the physicochemical stability test.
[0039] Figure 5 Thermogravimetric analysis and PXRD patterns of DUT-67 prepared in Example 1 before and after thermal stability test.
[0040] Figure 6 This is the gas adsorption / desorption isotherm diagram of DUT-67 prepared in Example 1 for N2, O2, CO2, SO2, R22, and R134a.
[0041] Figure 7 This is a graph showing the adsorption selectivity data of SO2 / N2 and SO2 / CO2 mixed gases of different ratios at 298K calculated by IAST theory for DUT-67 prepared in Example 1.
[0042] Figure 8 This is a graph showing the adsorption selectivity data of R22 / R134a / CO2 mixed gases of different ratios at 298K calculated by IAST theory for DUT-67 prepared in Example 1.
[0043] Fig. 9 The DUT-67 column prepared in Example 1 was heated at 298 K and 40 mL min -1 The capture breakthrough curve of SO2 in the Air / SO2 (N2:O2:CO2:SO2 81.8:15:3:0.2) mixed gas at a flow rate of .
[0044] Fig.10 The packed column of DUT-67 prepared in Example 1 was heated at 273, 298 and 303 K, 40 mL min -1 The capture breakthrough curve of SO2 in the Air / SO2 (N2:O2:CO2:SO2 81.8:15:3:0.2) mixed gas at a flow rate of .
[0045] Fig.11 The DUT-67 column prepared in Example 1 was heated at 298 K, 50% humidity, and 40 mL min -1 Comparison curve of capture penetration of SO2 in Air / SO2 (N2:O2:CO2:SO2 81.8:15:3:0.2) mixed gas at flow rate.
[0046] Fig.12 The packed column of DUT-67 prepared in Example 1 was heated at 298K at 40 mL min -1 The cyclic capture breakthrough curve of SO2 in the Air / SO2 (N2:O2:CO2:SO2 81.8:15:3:0.2) mixed gas at a flow rate of .
[0047] Fig.13 The DUT-67 column prepared in Example 1 was heated at 298 K, 10 mL min -1 Selective capture and separation breakthrough curves of R22 and R134a in Air / R22 / R134a (80:10:10) mixture at a flow rate of .
[0048] Fig.14 The DUT-67 column prepared in Example 1 was heated at 298 K and 20 mL min -1 Selective capture and separation breakthrough curves of R22 and R134a in Air / R22 / R134a (98:1:1) mixture at a flow rate of .
[0049] Fig.15 The DUT-67 column prepared in Example 1 was heated at 298 K and 50 mL min -1 Selective capture and separation breakthrough curves of R22 and R134a in the Air / R22 / R134a (99.96:0.02:0.02) mixture at a flow rate of .
[0050] Fig.16 The DUT-67 column prepared in Example 1 was heated at 298 K, 10 mL min -1 Cyclic penetration test curve for the selective capture and separation of R22 and R134a in the Air / R22 / R134a (80:10:10) mixture at a flow rate of .
[0051] Fig.17 The DUT-67 column prepared in Example 1 was heated at 298 K, 50% relative humidity, 10 mL min -1 Selective capture and separation breakthrough curves of R22 and R134a in Air / R22 / R134a (80:10:10) mixture at a flow rate of .
[0052] Fig.18 Photos of the equipment (a) and product (b) used for the scaled-up synthesis of DUT-67 prepared in Example 7.
[0053] Fig.19 This is the PXRD pattern of the scaled-up synthetic product of DUT-67 prepared in Example 7. DETAILED DESCRIPTION
[0054] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0055] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0056] The relative molecular weight of ZrO(NO3)2xH2O in Example 5 is 231.23 g / mol.
[0057] Example 1 A method for preparing a microporous zirconium-based metal organic framework material
[0058] A method for preparing a microporous zirconium-based metal organic framework material comprises the following steps:
[0059] Take a 40 mL glass bottle with a polytetrafluoroethylene gasket on the lid, add 7.5 mL of anhydrous formic acid and 12 mL of N,N-dimethylacetamide (DMAC), shake well, weigh ZrOCl2·8H2O (120 mg, 0.372 mmol), 2,5-thiophenedicarboxylic acid (60 mg, 0.348 mmol), add to the above mixed solution, mix the reaction system evenly by ultrasound, cover the glass bottle tightly and react at 120°C for 72 h. Then take out the glass bottle and cool it to room temperature in air. The supernatant in the glass bottle was removed, and N,N-dimethylformamide (DMF) was added thereto. After the crystals on the bottle wall were removed by ultrasound, they were filtered and collected. After adding DMF to the obtained crystals and washing them repeatedly three times, they were soaked in deionized water for one day, washed with methanol three times and soaked for three days. Fresh methanol was replaced six times a day to completely exchange the DMF in the pores with methanol. The crystals were then dried at room temperature for 12 hours, and then vacuum dried at 50°C and a vacuum degree of 0.001 torr to 0.1 torr for 12 hours to obtain activated DUT-67.
[0060] Example 2 A method for preparing a microporous zirconium-based metal organic framework material
[0061] A method for preparing a microporous zirconium-based metal organic framework material comprises the following steps:
[0062] Take a 40 mL glass bottle with a polytetrafluoroethylene gasket on the lid, add 4 mL of anhydrous formic acid and 12.5 mL of N, N-dimethylacetamide (DMAC), shake well, weigh ZrOCl2·8H2O (200 mg, 0.620 mmol), 2,5-thiophenedicarboxylic acid (100 mg, 0.581 mmol), add to the above mixed solution, mix the reaction system evenly by ultrasound, cover the glass bottle tightly, react at 80 ° C for 140 h, and then take out the glass bottle and cool it to room temperature in air. The supernatant in the glass bottle was removed, and N,N-dimethylformamide (DMF) was added thereto. After the crystals on the bottle wall were removed by ultrasound, they were filtered and collected. After adding DMF to the obtained crystals and washing them repeatedly three times, they were soaked in deionized water for one day, washed with methanol three times and soaked for three days. Fresh methanol was replaced six times a day to completely exchange the DMF in the pores with methanol. The crystals were then dried at room temperature for 12 hours, and then vacuum dried at 50°C and a vacuum degree of 0.001 torr to 0.1 torr for 12 hours to obtain activated DUT-67.
[0063] Example 3 A method for preparing a microporous zirconium-based metal organic framework material
[0064] A method for preparing a microporous zirconium-based metal organic framework material comprises the following steps:
[0065] Take a 40 mL glass bottle with a polytetrafluoroethylene gasket on the lid, add 12.5 mL of anhydrous formic acid and 12.5 mL of N, N-dimethylacetamide (DMAC), shake well, weigh ZrOCl2·8H2O (230 mg, 0.714 mmol), 2,5-thiophenedicarboxylic acid (110 mg, 0.639 mmol), add to the above mixed solution, mix the reaction system evenly by ultrasound, cover the glass bottle tightly, react at 150°C for 12 h, and then take out the glass bottle and cool it to room temperature in air. The supernatant in the glass bottle was removed, and N,N-dimethylformamide (DMF) was added thereto. After the crystals on the bottle wall were removed by ultrasound, they were filtered and collected. After adding DMF to the obtained crystals and washing them repeatedly three times, they were soaked in deionized water for one day, washed with methanol three times and soaked for three days. Fresh methanol was replaced six times a day to completely exchange the DMF in the pores with methanol. The crystals were then dried at room temperature for 12 hours, and then vacuum dried at 50°C and a vacuum degree of 0.001 torr to 0.1 torr for 12 hours to obtain activated DUT-67.
[0066] Example 4 A method for preparing a microporous zirconium-based metal organic framework material
[0067] A method for preparing a microporous zirconium-based metal organic framework material comprises the following steps:
[0068] Take a 40 mL glass bottle with a polytetrafluoroethylene gasket, add 7.5 mL of anhydrous formic acid and 12 mL of N,N-dimethylformamide (DMF), shake well, weigh ZrOCl2·8H2O (120 mg, 0.372 mmol), 2,5-thiophenedicarboxylic acid (60 mg, 0.348 mmol), add to the above mixed solution, mix the reaction system evenly by ultrasound, cover the glass bottle tightly, react at 120°C for 72 h, then take out the glass bottle and cool to room temperature in air. The supernatant in the glass bottle was removed, and N,N-dimethylformamide (DMF) was added thereto. After the crystals on the bottle wall were removed by ultrasound, they were filtered and collected. After adding DMF to the obtained crystals and washing them repeatedly three times, they were soaked in deionized water for one day, washed with methanol three times and soaked for three days. Fresh methanol was replaced six times a day to completely exchange the DMF in the pores with methanol. The crystals were then dried at room temperature for 12 hours, and then vacuum dried at 50°C and a vacuum degree of 0.001 torr to 0.1 torr for 12 hours to obtain activated DUT-67.
[0069] Example 5 A method for preparing a microporous zirconium-based metal organic framework material
[0070] A method for preparing a microporous zirconium-based metal organic framework material comprises the following steps:
[0071] Take a 40mL glass bottle with a polytetrafluoroethylene gasket on the lid, add 7.5mL of anhydrous formic acid and 12mL of N,N-dimethylacetamide (DMAC), shake well, weigh ZrO(NO3)2xH2O (120mg, 0.519mmol), 2,5-thiophenedicarboxylic acid (60mg, 0.348mmol), add to the above mixed solution, mix the reaction system evenly by ultrasound, cover the glass bottle tightly and react at 120℃ for 72h. Then take out the glass bottle and cool it to room temperature in air. The supernatant in the glass bottle was removed, and N,N-dimethylformamide (DMF) was added thereto. After the crystals on the bottle wall were removed by ultrasound, they were filtered and collected. After adding DMF to the obtained crystals and washing them repeatedly three times, they were soaked in deionized water for one day, washed with methanol three times and soaked for three days. Fresh methanol was replaced six times a day to completely exchange the DMF in the pores with methanol. The crystals were then dried at room temperature for 12 hours, and then vacuum dried at 50°C and a vacuum degree of 0.001 torr to 0.1 torr for 12 hours to obtain activated DUT-67.
[0072] Example 6 A method for preparing a microporous zirconium-based metal organic framework material
[0073] A method for preparing a microporous zirconium-based metal organic framework material comprises the following steps:
[0074] Take a 40mL glass bottle with a polytetrafluoroethylene gasket on the lid, add 7.5mL of anhydrous formic acid and 12mL of N,N-dimethylacetamide (DMAC), shake well, weigh ZrCl4 (100mg, 0.429mmol), 2,5-thiophenedicarboxylic acid (60mg, 0.348mmol), add to the above mixed solution, mix the reaction system evenly by ultrasound, cover the glass bottle tightly and react at 120℃ for 72h. Then take out the glass bottle and cool it to room temperature in air. The supernatant in the glass bottle was removed, and N,N-dimethylformamide (DMF) was added thereto. After the crystals on the bottle wall were removed by ultrasound, they were filtered and collected. After adding DMF to the obtained crystals and washing them repeatedly three times, they were soaked in deionized water for one day, washed with methanol three times and soaked for three days. Fresh methanol was replaced six times a day to completely exchange the DMF in the pores with methanol. The crystals were then dried at room temperature for 12 hours, and then vacuum dried at 50°C and a vacuum degree of 0.001 torr to 0.1 torr for 12 hours to obtain activated DUT-67.
[0075] Example 7 A method for preparing a kilogram-level microporous zirconium-based metal organic framework material
[0076] A method for preparing a kilogram-level microporous zirconium-based metal-organic framework material comprises the following steps:
[0077] Add 10L of anhydrous formic acid and 15L of N,N-dimethylacetamide (DMAC) to a 40L industrial reactor, stir evenly, add ZrOCl2·8H2O (1.20kg, 3.72mol), 2,5-thiophenedicarboxylic acid (500g, 2.9mol), stir evenly, heat the reactor to 120℃, stir and reflux for 72h. Cool to room temperature in air. Filter and separate the product, wash it three times with DMF, soak it in deionized water for 1 day, filter and separate the product, wash it three times with methanol, and soak it in anhydrous methanol for 3 days, replace it with fresh methanol three times a day, completely exchange the DMF in the pores with methanol, and then dry it at room temperature for 12h to obtain pure DUT-67. According to the actual situation, weigh the DUT-67 prepared for expanded production as needed and further vacuum dry it to obtain activated DUT-67.
[0078] Experimental Example: Characterization and Performance Testing of DUT-67
[0079] The microscopic crystal structure of the obtained DUT-67 was confirmed by X-ray diffraction, and the schematic diagram of its microscopic crystal structure is shown in the figure Figure 1 As shown, the frame has a reo topology. There are two types of cavities in the frame. The inner diameter of the small cavity (yellow) Inner diameter of the large cavity (pink) Among them, the Zr6 cluster is 8-connected, that is, 8 2,5-thiophenedicarboxylic acids are connected to one Zr6 cluster.
[0080] The X-ray diffraction pattern (PXRD) of DUT-67 obtained by testing is as follows Figure 2 As shown in the figure, the diffraction peaks in the PXRD pattern of DUT-67 obtained by this method are narrow and sharp, which is in good agreement with the powder pattern of the single crystal simulation, proving that it has good crystallinity and is a pure phase. The powder pattern of the single crystal simulation is obtained based on the corresponding single crystal data converted by Mercury software.
[0081] In order to test the specific surface area of DUT-67 and analyze its pore size and pore volume, a 77K nitrogen isothermal adsorption test was performed on DUT-67. The test results are shown in Figure 3 As shown, the BET specific surface area is 1178.23 m 2 .g -1 , the aperture is and
[0082] In order to test the hydrothermal stability and physicochemical stability of the obtained DUT-67, the synthesized fresh samples were immersed in 85°C hot water, 12M and 6M hydrochloric acid, and 1M NaOH aqueous solution for 24 h, and immersed in seawater for one month. The PXRD data of the immersed samples were tested. The results are shown in Figure 2. Figure 4 As shown, the PXRD spectrum of DUT-67 after immersion in hot water, acid, alkaline solution or seawater is still in good agreement with the spectrum of freshly synthesized DUT-67, indicating that DUT-67 still maintains good structural integrity after immersion in various solutions and has excellent hydrothermal stability and acid-base stability.
[0083] In order to determine the thermal stability of DUT-67 in air, a thermal stability test was performed. Thermogravimetric analysis (TGA) was performed first, and the sample was heated at 10℃.min. -1 The temperature was raised to 800°C at a rate of Figure 5 As shown in a, the DUT-67 sample obtained by this method has the first platform at about 250°C, indicating that the sample has almost lost all the solvent in the pores at this temperature, that is, the structure of the sample begins to collapse after 250°C. At the same time, the present invention also conducted a variable temperature X-ray powder diffraction test, and the obtained DUT-67 samples were heated at 5°C.min. -1 The samples were gradually heated to 100°C, 120°C, 140°C, 160°C, 180°C, 220°C, 240°C, 260°C, 280°C and 300°C and kept at these temperatures for 10 minutes. The PXRD data at these temperatures were obtained. Figure 5 As shown in Figure b, the results are consistent with the TGA data. The PXRD patterns of DUT-67 treated at different temperatures are still consistent with the diffraction patterns of freshly synthesized DUT-67 (25°C), which proves that the obtained DUT-67 has good thermal stability and can still maintain the stability of the framework at a high temperature of 250°C.
[0084] In order to characterize the single-component adsorption performance of DUT-76 for the main components of air (N2, O2, CO2), SO2, R22 and R134a at 273 and 298 K, the single-component adsorption isotherms of these gases at two temperatures were tested. The results are shown in Figure 2. Figure 6 As shown, DUT-67 has low or even no adsorption performance for the main components of air, but exhibits excellent adsorption performance for SO2, R22 and R134a, indicating that DUT-67 has the potential for highly selective separation of Air / SO2 and Air / R22 / R134a. In addition, the desorption curves and adsorption curves of the adsorption isotherms of all gases in the figure change synchronously and overlap, indicating that the adsorption process is physical adsorption and the adsorption is reversible.
[0085] In order to further determine the separation selectivity of DUT-67 for CO2 in the mixed systems of Air / SO2 and Air / R22 / R134a (with the strongest adsorption competition) and SO2, R22 and R134a in the mixed systems, the ideal adsorbed solution theory (IAST) was used to calculate the two-component separation selectivity curves of SO2 / CO2, R22 / CO2 and R134a / CO2 at different molar ratios. The results are shown in Figure 2. Figure 7 and Figure 8 As shown, the results show that the IAST selectivity of the three two-component gases is >20, proving that DUT-67 can separate and capture SO2, R22 and R134a from flue gas and air with high selectivity.
[0086] In order to simulate the actual industrial separation process, a dynamic breakthrough experiment was used to evaluate the actual separation effect of DUT-67 on SO2 in the simulated flue gas Air / SO2 mixture (N2:O2:CO2:SO2=81.8:15:3:0.2). 1.0g of activated DUT-67 sample was filled into the packed column as the fixed bed of the adsorption tower, and then -1 The flow rate was introduced into the packed column, and the results were as follows Fig. 9 As shown, due to the low adsorption affinity of DUT-67 for N2, O2, and CO2, these three gases quickly penetrated the packed column. SO2 had a strong interaction with the framework of DUT-67 and could be adsorbed in large quantities in the pores of DUT-67. It began to pass through the packed column after 96 minutes. The SO2 in the mixed gas flowing through the column before 96 minutes was completely captured on the packed column, proving that DUT-67 can achieve efficient and highly selective separation and capture of SO2 in the mixed gas of N2:O2:CO2:SO2 (81.8:15:3:0.2).
[0087] In order to explore the separation effect under the working temperature in actual industrial production, an Air / SO2 (N2:O2:CO2:SO2=81.8:15:3:0.2) mixed gas was used with a gas flow rate of 40 mL min -1 , the separation curves at 273K (simulating winter temperature) and 303K (simulating summer temperature) were tested respectively. The results are as follows Fig.10 As shown, temperature has a significant effect on the separation effect of SO2. The SO2 capture amount of DUT-67 at 273K is about 2.11 times that at 298K and 2.46 times that at 303K, indicating that low temperature is conducive to the capture of SO2, and high temperature will reduce the separation effect.
[0088] In order to be close to the actual industrial production conditions, the effect of DUT-67 on the SO2 capture effect in the presence of water vapor was studied. Air / SO2 (N2:O2:CO2:SO2 (81.8:15:3:0.2)) mixed gas was used with a gas flow rate of 40 mL.min -1 , the separation effect at 50% humidity was tested, and the results are as follows Fig.11 As shown, after increasing the humidity, it was found that the SO2 penetration point was only 1.21 minutes earlier than the penetration point without humidity influence, indicating that water vapor has very little effect on the SO2 capture effect of DUT-67, proving that the material has good resistance to water vapor interference.
[0089] In order to test the recycling performance of the material, an Air / SO2 (N2:O2:CO2:SO2=81.8:15:3:0.2) mixed gas was used at 298K with a gas flow rate of 40 mL min -1 , the SO2 capture was tested three times in a cycle, and the results are as follows Fig.12 As shown, the results show that the time points at which SO2 passes through the filling column are consistent and the curves have good overlap, proving that the material has good stability and recycling performance.
[0090] In order to evaluate the separation performance of the material for low concentrations of R22 and R134a in the atmosphere, a mixture of Air / R22 / R134a (80:10:10; 98:1:1) was first used at 10 mL / min. -1 , 298K, the capture performance of DUT-67 for R22 and R134a in the air was tested. The results are as follows Fig.13 and 14 As shown, the DUT-67 material can completely capture R22 and R134a from the air onto the filling column, achieving air purification and selective recovery of R22 and R134a.
[0091] Since some chlorofluoroalkanes in the atmosphere will dissolve into the surface water of the ocean, surface seawater is usually collected for environmental monitoring, and then the chlorofluoroalkanes dissolved in the seawater are enriched by purging and capturing. Since the solubility of chlorofluoroalkanes in seawater is very low, in order to explore whether the material can be used to capture the extremely low concentration of R22 and R134a purged from seawater, a mixture of Air / R22 / R134a (99.6:0.02:0.02) was used at 50mL min -1 The capture effect of the sample on R22 and R134a in the mixed gas was tested at a flow rate of Fig.15 As shown, it was found that the sample could still capture R22 and R134a and R134a in the air containing only 0.02% on the column, proving that the material can be used as a high-efficiency capture adsorbent for the purge condensation capture detection of chlorofluoroalkanes in seawater.
[0092] In order to test the recycling performance of the material, a mixture of Air / R22 / R134a (80:10:10) was used at 10 mL / min. -1 The cyclic capture performance of DUT-67 for R22 and R134a in air was tested at 298K. The results of six cycles are as follows: Fig.16 As shown, the penetration points of R22 and R134a in each cycle are basically the same, indicating that the material has good recycling performance.
[0093] In order to study the effect of water vapor on the capture of R22 and R134a by DUT-67, a mixture of Air / R22 / R134a (80:10:10) was used at 10 mL min -1 , 298K, DUT-67 was tested for the capture of R22 and R134a in 50% humidity air. The results are as follows Fig.17 As shown, compared with the dry state ( Fig.13 ), the penetration time points of R22 and R134a are only slightly advanced, proving that the material has a high ability to resist water vapor interference.
[0094] In order to prove the feasibility of large-scale synthesis of this series of materials, the synthesis scale of DUT-67 was expanded. Fig.18 As shown, a 40L industrial reactor was used to synthesize 1.2kg of DUT-67 at one time, and the obtained product was characterized by PXRD. The results are as follows Fig.19 As shown, the PXRD pattern of the obtained DUT-67 is in good agreement with the single crystal data simulation pattern of DUT-67, which indicates that the product synthesized on a large scale has high purity and good crystallinity.
[0095] The crystal structure, physicochemical properties, and selective gas capture and separation performance of DUT-67 prepared in Examples 2 to 7 are substantially consistent with those of DUT-67 prepared in Example 1.
[0096] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. Application of microporous zirconium-based metal organic framework materials in the adsorption and separation of halogenated alkane gases, characterized in that: The preparation method of the microporous zirconium-based metal organic framework material comprises the following steps: fully mixing a polar organic solvent and formic acid, then adding a zirconium salt and a thiophene dicarboxylic acid organic ligand, fully mixing, heating at 80 to 150° C. to complete the reaction, and post-treating to obtain the microporous zirconium-based metal organic framework material; Wherein, the polar organic solvent is N,N-dimethylacetamide or N,N-dimethylformamide; The volume ratio of the polar organic solvent to formic acid is 2:0.5-2; The molar ratio of the zirconium salt to the thiophenedicarboxylic acid organic ligand is 1:0.67-1.5; The mixing ratio of the total volume of the polar organic solvent and formic acid to the total mass of the zirconium salt and the thiophenedicarboxylic acid organic ligand is 6.5 mL: 60-450 mg; The molecular formula of the microporous zirconium-based metal organic framework material is Zr6O8(OH)8X4; Wherein, X is a thiophenedicarboxylic acid organic ligand.
2. The use according to claim 1, characterized in that: The zirconium salt is any one of ZrOCl2, ZrCl4, and ZrO(NO3)2.
3. The application according to claim 1, characterized in that: The thiophenedicarboxylic acid organic ligand is 2,5-thiophenedicarboxylic acid.
4. The use according to claim 1, characterized in that: The time required for the reaction to be complete is 12 to 150 hours.
5. The use according to claim 1, characterized in that: The post-treatment operations also include filtration, washing, soaking and drying.
6. The use according to claim 5, characterized in that: The drying is performed at room temperature first and then vacuum drying.
7. The use according to claim 1, characterized in that: The halogenated alkane gas includes difluoromonochloromethane, 1,1,1,2-tetrafluoroethane, carbon tetrafluoride, monofluorotrichloromethane, hexafluoroethane, tetrafluoromethane, octafluoropropane, dichlorodifluoromethane, chlorotrifluoromethane, pentafluorochloroethane, and trifluoromethane.