Ultrasonic pre-modulation optimization of alloy directional solidification columnar crystal orientation single crystal preparation method
By applying an ultrasonic field to modulate the interface before directional solidification during the single crystal preparation process, the problem of the influence of ultrasound on the interface is solved, the efficiency and quality of single crystal preparation are improved, the cost is reduced, and the crystal planes of columnar crystals are consistent. sexual regulation.
Patent Information
- Application Number
- CN202310376713.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-04-11
AI Technical Summary
In the current single crystal preparation process, applying an ultrasonic field during the directional solidification process has a complex impact on the interface, which may destroy the directionality, resulting in unfavorable single crystal growth and high cost.
The ultrasonic field is applied before the directional solidification process. By modulating the initial state of the interface, the modulation effect of ultrasound on the stationary interface is used to avoid the destabilizing effect of ultrasound on the interface during the growth process and improve the crystal plane consistency of columnar crystal growth. Ultrasound is used to Pre-modulation and optimization of the preparation method of directional solidification columnar crystal-oriented single crystals of alloys.
It improves the efficiency and quality of single crystal preparation, reduces costs, realizes positive control of the consistency of columnar crystal planes, reduces the time and materials for removing impurity crystals, and improves the efficiency of single crystal preparation.
Smart Images

Figure CN116377577B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of advanced material preparation and processing, and in particular relates to a method for preparing an ultrasonic pre-modulated optimized alloy directional solidification columnar crystal oriented single crystal. Background Art
[0002] The production of high-quality single crystal rods is mainly achieved through the directional growth process. In the process of preparing single crystals by conventional seedless directional solidification, it usually goes through the seeding stage, which starts with the loss of stability of the static liquid-solid interface, and after a long distance of competitive selection of columnar crystals and elimination of impurity crystals, it enters the crystal selector for the subsequent single crystal growth process. The time and materials consumed in the seeding stage increase the cost of single crystal preparation.
[0003] On the other hand, ultrasonic field, as an important means of controlling the physical field of the solidification process, has been applied to a certain extent. The main effects of applying ultrasonic waves during free solidification are grain refinement, degassing, and elimination of segregation. However, applying ultrasonic fields during directional solidification will have a complex effect on the interface and may damage the orientation, which is not conducive to the growth of single crystals. At present, conventional ultrasonic directional solidification technology has not yet found a significant beneficial effect on the preparation of single crystals. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing alloy directional solidification columnar crystal oriented single crystals by ultrasonic pre-modulation optimization in view of the deficiencies in the above-mentioned prior art. The method applies an ultrasonic field before the directional solidification process, and modulates the initial state of the interface so that after the growth begins, the crystal plane consistency of the columnar crystal growth is greatly improved. The method not only utilizes the modulation effect of ultrasound on the static interface, but also avoids the destabilizing effect of ultrasound on the interface during the growth process. The method improves the efficiency of single crystal preparation and greatly reduces the cost, providing a new solution for improving the efficiency and quality of single crystal preparation.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing an alloy directional solidification columnar crystal oriented single crystal by ultrasonic pre-modulation optimization, the method comprising the following steps:
[0006] Step 1, material loading: loading an alloy rod for single crystal preparation in a crucible of an ultrasonic directional solidification device; the ultrasonic directional solidification device comprises a high temperature resistant pressure head located at the top of the crucible and an ultrasonic horn located at the bottom of the crucible, and the crucible is clamped and fixed by the high temperature resistant pressure head located at the top and the ultrasonic horn located at the bottom;
[0007] Step 2: Preload adjustment: adjust the preload of the high temperature resistant pressure head to the preset optimal preload;
[0008] Step 3: Vacuuming: evacuate the directional solidification vacuum chamber of the ultrasonic directional solidification device to the daily working vacuum, and then fill it with protective gas;
[0009] Step 4, heating initialization: start the heating system of the ultrasonic directional solidification device, make the heating temperature of the heating system reach the predetermined heating temperature T1, the alloy rod is completely located in the heating system, melted evenly and kept warm for a standing time t1, then stop heating; then start the motion system of the ultrasonic directional solidification device, make the alloy rod descend to the initial position of the alloy directional solidification, stop moving, and then stand for a standing time t2;
[0010] Step 5, ultrasonic pretreatment of the solidification interface: adjust the output frequency and output voltage of the ultrasonic driving power supply so that the end amplitude of the ultrasonic horn is greater than the preset amplitude threshold As0, start the ultrasonic system of the ultrasonic directional solidification device, make the ultrasonic wave act on the solid-liquid initial interface of the alloy directional solidification, and make the ultrasonic system of the ultrasonic directional solidification device work continuously for at least a time longer than the preset ultrasonic pretreatment time threshold ts0, and then turn off the ultrasonic vibration;
[0011] Step 6: Directional solidification: start the motion system and heating system of the ultrasonic directional solidification device to achieve directional solidification of the alloy rod from bottom to top;
[0012] Step 7. After directional solidification is completed, unload the alloy rod: After the alloy rod is completely solidified, turn off the motion system and heating system of the ultrasonic directional solidification device. After the heating system cools to room temperature, open the vacuum chamber of the ultrasonic directional solidification device and take out the alloy after directional solidification.
[0013] In the above-mentioned method for preparing columnar oriented single crystals by optimizing the ultrasonic pre-modulation of alloy directional solidification, the method for presetting the optimal preload force in step 2 is:
[0014] Step B1, setting a heating temperature Th for single crystal preparation;
[0015] Step B2: Look up the yield strength of the material used for the crucible at the heating temperature Th and the yield strength of the material used for the ultrasonic horn at the heating temperature Th in the material parameter table, compare the two values, and record the smaller value as the yield strength σ s ;
[0016] Step B3: Determine the value range of the preload force F as F min ~K F σ s ·S; where F min is the minimum value of the preload force F, K F is the safety factor of the preload force, S is the contact area between the ultrasonic horn and the crucible;
[0017] Step B4: Set the preload force F to Fmin The resonant frequency of the ultrasonic transducer is measured with an impedance analyzer and used as the working frequency. The ultrasonic system of the ultrasonic directional coagulation device is started and the output voltage of the ultrasonic driving power supply is adjusted so that the end amplitude of the ultrasonic horn is greater than A. min , and record the output voltage V of the ultrasonic driving power supply at this time; where A min is the minimum value of the end amplitude of the ultrasonic horn;
[0018] Step B5: Keep the output voltage V of the ultrasonic driving power supply unchanged. min ~K F σ s Within the value range of S, the value of the preload force F is changed several times. After each change of the preload force value, the resonance frequency of the ultrasonic transducer is measured with an impedance analyzer and used as the working frequency. The amplitude U of the crucible wall is then measured with a laser vibrometer. The change of the amplitude U of the crucible wall with the change of the preload force F is recorded and a curve is drawn. The curve fitting of is used to obtain the characteristic parameter f0 of the preload force and the characteristic parameter U0 of the crucible wall amplitude; where e is the natural logarithm;
[0019] Step B6: Compare k f f0 and K F σ s ·S size, the smaller value is determined as the optimal preload force; where k f is the characteristic coefficient of preload force.
[0020] In the above-mentioned method for preparing columnar oriented single crystals by optimizing the ultrasonic pre-modulation of alloy directionally solidified, the amplitude threshold As0 and the ultrasonic pre-treatment time threshold ts0 in step 5 are determined as follows:
[0021] Step 501: Perform multiple experiments using the method of steps 1 to 7. During multiple experiments, in step 5, select multiple different amplitude values within the maximum amplitude range of the end of the ultrasonic horn, and on the basis of each amplitude value, select the value of the amplitude at t min ~t max Select multiple different ultrasonic pretreatment times within the range, take longitudinal section samples after each alloy solidification, analyze the material crystal structure of a section of initial growth length L, check whether the longitudinal section is the same crystal plane, take out the minimum effective ultrasonic pretreatment time when the longitudinal section is the same crystal plane, determine the ultrasonic pretreatment time threshold ts0 corresponding to the amplitude, and obtain a set of corresponding values of amplitude As and ultrasonic pretreatment time threshold ts0; where t min is the minimum value of ultrasonic pretreatment time, t max is the maximum value of ultrasonic pretreatment time;
[0022] Step 502: According to the formula Fitting is performed to obtain the formula The constant term coefficient As0, exponential term coefficient As1 and power coefficient τ of the amplitude threshold As0 are obtained. Then, when As takes any value greater than the amplitude threshold As0, the formula The value of the ultrasonic pretreatment time threshold ts0 corresponding to As is calculated; wherein e is the natural logarithm and t is the time.
[0023] In the above-mentioned method for preparing columnar oriented single crystals by optimizing the ultrasonic pre-modulation of alloy, when checking whether the longitudinal section is the same crystal plane as described in step 501, an X-ray diffractometer is used to perform polycrystalline diffraction analysis. When the analysis result has only a single crystal plane diffraction peak, it is judged that the longitudinal section is the same crystal plane. Otherwise, it is judged that the longitudinal section is not the same crystal plane.
[0024] The above-mentioned method for preparing a columnar oriented single crystal by optimizing the directional solidification of an alloy by ultrasonic pre-modulation, wherein the t min The value of is 1min, and the t max The value of is 2h; the value of L is 5mm~10mm.
[0025] In the above-mentioned method for preparing columnar oriented single crystals by optimizing the directional solidification of alloys by ultrasonic pre-modulation, the motion system and the heating system of the ultrasonic directional solidification device are started in step 6 to realize the directional solidification of the alloy rod from bottom to top. The motion system moves at a growth speed V. The value range of the growth speed V is determined by:
[0026] When optimizing the cellular orientation of a material with a single-phase growth morphology, select Vc <V<Vd1;
[0027] When optimizing the dendrite trunk crystal orientation of a material with a predominantly single-phase growth morphology, select Vd1 <V<Vd2;
[0028] Among them, Vc is the transition speed from the flat interface to the cellular crystal of the material with a main single-phase growth morphology, Vd1 is the transition speed from the cellular crystal to the dendrite of the material with a main single-phase growth morphology, and Vd2 is the upper limit of the dendrite growth speed of the material with a main single-phase growth morphology.
[0029] In the above-mentioned method for preparing columnar oriented single crystals by optimizing the directional solidification of alloy by ultrasonic pre-modulation, the crucible is a bottomless crucible with an open bottom, and the top of the ultrasonic horn is provided with a boss protruding upward and used for inserting into the bottom of the crucible.
[0030] In the above-mentioned method for preparing columnar oriented single crystals by optimizing the directional solidification of alloys by ultrasonic pre-modulation, the length of the boss is 1 mm to 5 mm, and the outer diameter of the boss is 0.2 mm to 0.5 mm smaller than the inner diameter of the crucible.
[0031] In the above-mentioned method for preparing columnar oriented single crystals by ultrasonic pre-modulation optimized alloy directional solidification, the top boss of the ultrasonic transformer is directly inserted into the crucible, the top boss of the ultrasonic transformer directly contacts the bottom of the alloy rod loaded in the crucible, and the outer ring of the top boss of the ultrasonic transformer is in rigid contact with the crucible.
[0032] Compared with the prior art, the present invention has the following advantages:
[0033] 1. Before the directional solidification process, the present invention applies ultrasound to the bottom of the sample, so that the ultrasound acts on the initial interface of metal solidification to modulate the initial state of the interface. After the ultrasonic pretreatment is completed, the directional solidification is started; the modulation effect of ultrasound on the static interface is utilized, and the destabilizing effect of ultrasound on the interface during the growth process is avoided; and the positive regulation of the consistency of the columnar crystal surface is achieved.
[0034] 2. The present invention applies an ultrasonic field before the directional solidification process, and by modulating the initial state of the interface, the crystal plane consistency of the columnar crystal growth is greatly improved after the growth begins, which greatly reduces the time and materials required for removing impure crystals during directional solidification. The impurity crystals are removed in a relatively short time, the crystal orientation selection is completed, the efficiency of single crystal preparation is improved, and the cost is greatly reduced, providing a new solution for improving the efficiency and quality of single crystal preparation.
[0035] 3. The present invention fully analyzes the nonlinear influence of the solid-liquid phase ratio of the alloy rod on the acoustic field under the temperature gradient, and uses numerical simulation and experimental measurement to find the optimal value of parameters such as the optimal preload force, amplitude threshold, ultrasonic pretreatment time threshold, and growth rate. This can make the solid-liquid interface of the alloy directional solidification in a state of high sound intensity, realize strong ultrasonic treatment of the interface, and thus realize the modulation of the initial state of the interface.
[0036] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a flowchart of the method of the present invention;
[0038] Figure 2 It is a schematic structural diagram of the ultrasonic directional coagulation device used in the present invention;
[0039] Figure 3A The EBSD analysis diagram of the longitudinal section structure of the Al-4.5wt.%Cu alloy with a growth rate of V=100μm / s obtained by the method of the present invention;
[0040] Figure 3BThis is the EBSD analysis diagram of the longitudinal section structure of the Al-4.5wt.%Cu alloy with a growth rate of V=100μm / s obtained without ultrasonic pretreatment of the solidification interface;
[0041] Figure 3C This is a statistical diagram of crystallographic orientation difference distribution.
[0042] Description of reference numerals:
[0043] 1—ultrasonic driving power supply; 2—ultrasonic horn; 3—pressure sensor display;
[0044] 4—vacuum chamber; 5—elevator; 6—temperature controller;
[0045] 7—displacement display; 8—high temperature resistant pressure head; 9—controller;
[0046] 10—induction coil; 11—heating jacket; 12—elevator drive;
[0047] 13—cooler; 15—upper pressure rod; 16—spring;
[0048] 17—pressure sensor; 18—crucible; 20—alloy rod;
[0049] 21—induction heating power supply; 22—upper moving support plate; 23—heating jacket temperature sensor;
[0050] 24—upper insulation board; 25—lower insulation board; 26—insulation sleeve;
[0051] 28—Ultrasonic transducer. DETAILED DESCRIPTION
[0052] like Figure 1 As shown, the method for preparing an alloy directional solidification columnar crystal oriented single crystal by ultrasonic pre-modulation optimization of the present invention comprises the following steps:
[0053] Step 1, material loading: loading an alloy rod 20 for single crystal preparation into a crucible 18 of an ultrasonic directional solidification device; the ultrasonic directional solidification device comprises a high temperature resistant pressure head 8 located at the top of the crucible 18 and an ultrasonic horn 2 located at the bottom of the crucible 18, and the crucible 18 is clamped and fixed by the high temperature resistant pressure head 8 located at the top and the ultrasonic horn 2 located at the bottom;
[0054] In a specific implementation, the crucible 18 is a bottomless crucible; the top of the crucible 18 is a hot end for directional solidification, and the bottom of the crucible 18 is a cooling end for directional solidification.
[0055] Step 2: preload adjustment: adjust the preload of the high temperature resistant pressure head 8 to the preset optimal preload to achieve a good vibration state (vibration close to the maximum value);
[0056] In this embodiment, the method for presetting the optimal preload force in step 2 is:
[0057] Step B1, setting a heating temperature Th for single crystal preparation;
[0058] In specific implementation, the heating temperature Th is generally selected from 110% to 130% of the liquidus temperature TC of the alloy melt;
[0059] Step B2: Look up the yield strength of the material used for the crucible 18 at the heating temperature Th and the yield strength of the material used for the ultrasonic horn 2 at the heating temperature Th in the material parameter table, compare the two, and record the smaller value as the yield strength σ s ;
[0060] Step B3: Determine the value range of the preload force F as F min ~K F σ s ·S; where F min is the minimum value of the preload force F, K F is the safety factor of the preload force, S is the contact area between the ultrasonic horn 2 and the crucible 18;
[0061] In specific implementation, K F The value range of is 0.5~0.8;
[0062] Step B4: Set the preload force F to F min The resonant frequency of the ultrasonic transducer is measured by an impedance analyzer and used as the working frequency. The ultrasonic system of the ultrasonic directional coagulation device is started, and the output voltage of the ultrasonic driving power supply 1 is adjusted so that the end amplitude of the ultrasonic horn 2 is greater than A. min , and record the output voltage V of the ultrasonic driving power supply 1 at this time; where A min is the minimum value of the end amplitude of the ultrasonic horn 2;
[0063] In specific implementation, A min The value is 5um;
[0064] Step B5: Keep the output voltage V of the ultrasonic driving power supply 1 unchanged. min ~K F σ s S, change the value of the preload force F for many times. After each change of the preload force value, use an impedance analyzer to measure the resonant frequency of the ultrasonic transducer and use it as the working frequency. Then use a laser vibrometer to measure the amplitude U of the wall of the crucible 18. Record the change of the amplitude U of the wall of the crucible 18 with the change of the preload force F, and make a curve. The curve fitting of is used to obtain the characteristic parameter f0 of the preload force and the characteristic parameter U0 of the amplitude of the wall of the crucible 18; wherein e is the natural logarithm;
[0065] Step B6: Compare k f f0 and K F σ s ·S size, the smaller value is determined as the optimal preload force; where k f is the characteristic coefficient of preload force.
[0066] In specific implementation, F min The value of k is 10N, f The value range is 2 to 3.
[0067] Step 3: Vacuuming: evacuate the directional solidification vacuum chamber of the ultrasonic directional solidification device to the daily working vacuum, and then fill it with protective gas;
[0068] In specific implementation, the daily working vacuum is generally 1×10 -1 Pa to 1×10 -5 Pa, the protective gas is generally argon or nitrogen. Repeating the "vacuuming-filling protective gas" process 2-3 times can better remove the oxygen in the vacuum chamber 1; the final atmosphere state is generally 10Pa ~ 60000Pa protective gas.
[0069] This step can prevent the metal from oxidizing and also prevent the gas from expanding beyond 1 atmosphere during the heating and solidification process.
[0070] Step 4, heating initialization: start the heating system of the ultrasonic directional solidification device, make the heating temperature of the heating system reach the predetermined heating temperature T1, the alloy rod 20 is completely located in the heating system, melted evenly and kept warm for a standing time t1, then stop heating; then start the motion system of the ultrasonic directional solidification device, make the alloy rod 20 drop to the initial position of the alloy directional solidification, stop moving, and then stand for a standing time t2;
[0071] In the specific implementation, the optimal preload is maintained throughout the entire process of step 4; the value of the predetermined heating temperature T1 of the heating system is the same as the set heating temperature Th for single crystal preparation, generally 110% to 130% of the liquidus temperature TC of the alloy melt; the values of t1 and t2 are both 10min to 30min; the initial position of the alloy directional solidification is 1mm to 10mm from the bottom of the crucible 18 into the coolant of the cooling system of the ultrasonic directional solidification device;
[0072] Step 5, ultrasonic pretreatment of the solidification interface: adjust the output frequency and output voltage of the ultrasonic driving power supply 1 so that the end amplitude of the ultrasonic horn 2 is greater than the preset amplitude threshold As0, start the ultrasonic system of the ultrasonic directional solidification device, make the ultrasonic wave act on the initial interface of the directional solidification of the alloy, and make the ultrasonic system of the ultrasonic directional solidification device work continuously for at least a time longer than the preset ultrasonic pretreatment time threshold ts0, and then turn off the ultrasonic vibration;
[0073] In specific implementation, the resonance frequency of the ultrasonic transducer is measured with an impedance analyzer and used as the working frequency, and the output frequency of the ultrasonic driving power supply 1 is adjusted to the working frequency; when the ultrasonic driving power supply 1 used has a built-in output frequency adjustment function, the output frequency of the ultrasonic driving power supply 1 can be directly adjusted; when the ultrasonic driving power supply 1 used does not have a built-in output frequency adjustment function, an external AC signal source is connected to the ultrasonic driving power supply 1, and the output frequency of the ultrasonic driving power supply 1 is adjusted by adjusting the output frequency of the AC signal source. After the alloy rod 20 drops to the initial position of the alloy directional solidification, the ultrasonic amplitude transformer 2 enters the coolant of the cooling system of the ultrasonic directional solidification device, and the load changes. The output frequency of the ultrasonic driving power supply 1 is adjusted again, so that the ultrasonic pretreatment of the solidification interface can be performed more accurately, ensuring the processing accuracy.
[0074] During specific implementation, the end amplitude of the ultrasonic horn 2 is measured by a laser vibrometer.
[0075] In this embodiment, the amplitude threshold As0 and the ultrasonic pretreatment time threshold ts0 in step 5 are determined as follows:
[0076] Step 501: Perform multiple experiments using the method of steps 1 to 7. During multiple experiments, in step 5, select multiple different amplitude values within the maximum amplitude range of the end of the ultrasonic horn 2, and on the basis of each amplitude value, select the value of the amplitude at t min ~t max Select multiple different ultrasonic pretreatment times within the range, take longitudinal section samples after each alloy solidification, analyze the material crystal structure of a section of initial growth length L, check whether the longitudinal section is the same crystal plane, take out the minimum effective ultrasonic pretreatment time when the longitudinal section is the same crystal plane, determine the ultrasonic pretreatment time threshold ts0 corresponding to the amplitude, and obtain a set of corresponding values of amplitude As and ultrasonic pretreatment time threshold ts0; where t min is the minimum value of ultrasonic pretreatment time, t max is the maximum value of ultrasonic pretreatment time;
[0077] In this embodiment, when checking whether the longitudinal section is the same crystal plane as described in step 501, an X-ray diffractometer is used to perform polycrystalline diffraction analysis. When the analysis result has only a single crystal plane diffraction peak, it is judged that the longitudinal section is the same crystal plane, indicating that the orientation control is effective. Otherwise, it is judged that the longitudinal section is not the same crystal plane.
[0078] In addition, EBSD analysis can also be used to analyze the consistency of the crystal plane. For example, if the crystal plane orientation is less than 10°, it is judged that the longitudinal section is the same crystal plane, indicating that the orientation control is effective.
[0079] In this embodiment, the t min The value of is 1min, and the t max The value of is 2h; the value of L is 5mm~10mm.
[0080] Step 502: According to the formula Fitting is performed to obtain the formula The constant term coefficient As0, exponential term coefficient As1 and power coefficient τ of the amplitude threshold As0 are obtained. Then, when As takes any value greater than the amplitude threshold As0, the formula The value of the ultrasonic pretreatment time threshold ts0 corresponding to As is calculated; wherein e is the natural logarithm and t is the time.
[0081] Step 6: Directional solidification: starting the motion system and heating system of the ultrasonic directional solidification device to achieve directional solidification of the alloy rod 20 from bottom to top;
[0082] In this embodiment, when the motion system and heating system of the ultrasonic directional solidification device are started in step 6 to realize the directional solidification of the alloy rod 20 from bottom to top, the motion system moves at a growth speed V. The value range of the growth speed V is determined as follows:
[0083] When optimizing the cellular orientation of a material with a single-phase growth morphology, select Vc <V<Vd1;
[0084] When optimizing the dendrite trunk crystal orientation of a material with a predominantly single-phase growth morphology, select Vd1 <V<Vd2;
[0085] Among them, Vc is the transition speed from the flat interface to the cellular crystal of the material with a main single-phase growth morphology, Vd1 is the transition speed from the cellular crystal to the dendrite of the material with a main single-phase growth morphology, and Vd2 is the upper limit of the dendrite growth speed of the material with a main single-phase growth morphology.
[0086] During specific implementation, Vc, Vd1, and Vd2 are measured by experiments.
[0087] Step 7, after directional solidification is completed, unload the alloy rod 20: after the alloy rod 20 is completely solidified, turn off the motion system and heating system of the ultrasonic directional solidification device, after the heating system cools to room temperature, open the vacuum chamber of the ultrasonic directional solidification device, and take out the alloy after directional solidification.
[0088] like Figure 2 As shown, the ultrasonic directional coagulation device includes a vacuum chamber 4, an ultrasonic system, a heating system, a cooler 13 and a motion system;
[0089] An upper heat insulation board 24 is arranged at the upper part of the vacuum chamber 4, a lower heat insulation board 25 is arranged at the middle part of the vacuum chamber 4, the heating system is arranged at the upper part of the lower heat insulation board 25 in the vacuum chamber 4, the cooler 13 is arranged at the lower part of the lower heat insulation board 25 in the vacuum chamber 4, and the upper heat insulation board 24, the heating system, the lower heat insulation board 25 and the cooler 13 have a central cavity connected up and down; a crucible 18 for loading an alloy rod 20 for preparing a single crystal is arranged in the central cavity of the upper heat insulation board 24, the heating system and the lower heat insulation board 25, a high temperature resistant pressure head 8 is arranged at the top of the crucible 18, and an upper moving support plate 22, a pressure sensor 17, an upper pressure rod 15 and a spring 16 connected in sequence are arranged above the high temperature resistant pressure head 8 from top to bottom, and the high temperature resistant pressure head 8 is connected to the spring 16; the pressure sensor 17 is connected to the pressure sensing display 3;
[0090] In a specific implementation, the spring 16 is a nickel-based high-temperature spring; the spring 16 provides a preload force for the high-temperature resistant pressure head 8, the preload force is measured by the pressure sensor 17, and the pressure is displayed by the pressure sensor display 3;
[0091] The ultrasonic system includes an ultrasonic horn 2, an ultrasonic transducer 28 for providing vibration energy to the ultrasonic horn 2, and an ultrasonic driving power supply 1 for driving the ultrasonic transducer 28, wherein the ultrasonic transducer 28 is connected to the lower end of the ultrasonic horn 2, and the ultrasonic horn 2 is inserted into the central cavity of the cooler 13; the crucible 18 is clamped and fixed by a high temperature resistant pressure head 8 located at the top thereof and the ultrasonic horn 2 located at the bottom thereof;
[0092] The heating system comprises a temperature controller 6, an induction heating power supply 21, a heating sleeve 11, a heat preservation sleeve 26 sleeved on the outside of the heating sleeve 11, and an induction coil 10 arranged on the outside of the heat preservation sleeve 26; a heating sleeve temperature sensor 23 arranged in the heating sleeve 11 and used to collect the temperature of the heating sleeve 11 is inserted and connected to the top of the heating sleeve 11, the heating sleeve temperature sensor 23 is connected to the input end of the temperature controller 6, the induction heating power supply 21 is connected to the output end of the temperature controller 6, and the induction coil 10 is connected to the output end of the induction heating power supply 21;
[0093] In a specific implementation, the heating jacket 11 is a graphite heating jacket, the heating jacket temperature sensor 23 is a thermocouple, and the temperature controller 6 is a PID temperature controller;
[0094] The motion system includes an elevator 5 capable of driving the vacuum chamber 4, the heating system and the cooling system to move upward synchronously, an elevator driver 12 connected to the elevator 5, a controller 9 connected to the elevator driver 12 and a displacement display 7 connected to the controller 9; when the vacuum chamber 4, the heating system and the cooling system move upward synchronously, the crucible 18, the ultrasonic horn 2, the ultrasonic transducer 28 and the high temperature resistant pressure head 8 do not move, thereby realizing the directional solidification process of the alloy rod 20 from bottom to top.
[0095] In this embodiment, the crucible 18 is a bottomless crucible with an open bottom, and the top of the ultrasonic horn 2 is provided with a boss that protrudes upward and is used to be inserted into the bottom of the crucible 18 .
[0096] In this embodiment, the length of the boss is 1 mm to 5 mm, and the outer diameter of the boss is 0.2 mm to 0.5 mm smaller than the inner diameter of the crucible 18 to prevent the ultrasonic horn 2 from damaging the crucible 18 due to a large thermal expansion coefficient after heating.
[0097] In this embodiment, the top boss of the ultrasonic horn 2 is directly inserted into the crucible 18 , the top boss of the ultrasonic horn 2 directly contacts the bottom of the alloy rod 20 loaded in the crucible 18 , and the outer ring of the top boss of the ultrasonic horn 2 is in rigid contact with the crucible 18 .
[0098] When ultrasonic pretreatment of the solidification interface is performed in step five, ultrasonic waves are introduced from the alloy rod 20 and the bottom of the crucible 18 , and the ultrasound waves are simultaneously transmitted through the alloy rod 20 and the crucible 18 .
[0099] When directional solidification is performed in step six, the top of the crucible 18 is the hot end of the directional solidification, and the bottom of the crucible 18 is the cooling end of the directional solidification.
[0100] In order to verify the technical effect that the present invention can produce, the following experiments were conducted on the method for preparing directional solidified columnar oriented single crystals of alloys optimized by ultrasonic pre-modulation of the present invention:
[0101] The experiment takes the ultrasonic treatment process of Al-4.5wt.%Cu alloy as an example:
[0102] When loading materials in step 1, an Al-4.5wt.%Cu alloy rod 20 with a diameter of 10mm and a length of 110mm for single crystal preparation is loaded in the crucible 18 of the ultrasonic directional solidification device; the crucible 18 is loaded into the central cavity of the upper insulation board 24, the heating system and the lower insulation board 25, and the crucible 18 is clamped and fixed by the high temperature resistant pressure head 8 located at the top and the ultrasonic horn 2 located at the bottom; the crucible 18 is a graphite crucible with an inner diameter of 10mm, a wall thickness of 1mm and a height of 120mm; the outer diameter of the heating jacket 11 is 50mm, the inner diameter is 26mm and the height is 170mm; the outer diameter of the insulation jacket 26 is 70mm, the inner diameter is 54mm and the height is 175mm;
[0103] When the preload is adjusted and the optimal preload is set in step 2, the liquidus temperature of the Al-4.5wt.%Cu alloy is 650°C. Therefore, the heating temperature Th for preparing the Al-4.5wt.%Cu alloy single crystal is set to 1000°C in step B1; in step B2, the yield strength of the graphite material used for the crucible 18 at the heating temperature Th=1000°C is 14MPa, which is less than the yield strength of the 45 steel material used for the ultrasonic horn 2 at the heating temperature Th=1000°C. Therefore, σ s =14Mpa; F in step B3 min =10N,K F σ s S = 0.5 × 10 × 3.14 × 1 × 14 = 220 N, the value range of the preload force F is determined to be 10 N to 220 N; in step B4, A min =5μm, the end amplitude of the ultrasonic horn 2 is 10μm, and the output voltage V of the ultrasonic driving power supply 1 is recorded as 850V; in step B5, the output voltage V of the ultrasonic driving power supply 1 is kept at 850V, and f0=8.5N is obtained by fitting; in step B6, k f =2, k f f0=17N, much smaller than K F σ s S = 220N, so the optimal preload force is determined to be 17N.
[0104] When evacuating in step 3, after the directional solidification vacuum chamber of the ultrasonic directional solidification device is evacuated to 0.001Pa, argon gas is turned on to keep the flow rate at 2L / min and filled into the vacuum chamber to 5000Pa;
[0105] During the heating initialization in step 4, the heating temperature is set at 1000°C (actual temperature error ±1°C), the heating system of the ultrasonic directional solidification device is started, the heating temperature of the heating system reaches the predetermined heating temperature T1=1000°C, the alloy rod 20 is completely located in the heating system, and the alloy rod 20 is melted evenly and kept warm for 15 minutes before stopping the heating; then, the motion system of the ultrasonic directional solidification device is started, the alloy rod 20 is lowered to the initial position of the alloy directional solidification (the bottom of the crucible 18 enters the coolant of the cooling system of the ultrasonic directional solidification device by 5mm), and then stops moving, and then stands for 30 minutes;
[0106] During the ultrasonic pretreatment of the coagulation interface in step 5, the amplitude threshold As0 and the ultrasonic pretreatment time threshold ts0 are selected as follows: in step 501, multiple different amplitude values are selected in the amplitude range of 10 μm to 50 μm, and multiple different ultrasonic pretreatment time durations are selected in the range of 5 min to 2 h; in step 502, the amplitude threshold As0 obtained by fitting is 15 μm. When As takes any value greater than the amplitude threshold As0, the formula The value of the ultrasonic pretreatment time threshold ts0 corresponding to As is calculated;
[0107] In step 5, during ultrasonic pretreatment of the solidification interface, As is taken as 44 μm, and the formula It is calculated that ts0 = 2 min; after the ultrasonic system of the ultrasonic directional coagulation device works for 5 min, the ultrasonic vibration is turned off;
[0108] During directional solidification in step 6, the motion system and heating system of the ultrasonic directional solidification device are started, and a growth rate V=100 μm / s is adopted to achieve directional solidification of the alloy rod 20 from bottom to top;
[0109] In step seven, directional solidification is completed and the alloy rod 20 is unloaded: after the alloy rod 20 is completely solidified, the motion system and heating system of the ultrasonic directional solidification device are turned off. After the heating system is cooled to room temperature, the vacuum chamber of the ultrasonic directional solidification device is opened to take out the alloy after directional solidification.
[0110] The Al-4.5wt.%Cu alloy obtained by the method of the present invention has a growth rate of V=100μm / s. The longitudinal section EBSD structure analysis is as follows: Figure 3A As shown;
[0111] For comparison, when ultrasonic pretreatment of the solidification interface is not performed, other parameters are the same, and the Al-4.5wt.%Cu alloy has a growth rate of V=100μm / s. The longitudinal section EBSD microstructure analysis is shown as follows: Figure 3B As shown; the crystallographic orientation difference distribution statistics are as follows Figure 3C As shown;
[0112] from Figure 3A to Figure 3CIt can be seen that the maximum orientation difference of the crystal in directionally solidified under static conditions without ultrasonic application is 41°, and the maximum orientation difference of the crystal in directionally solidified after ultrasonic treatment with an amplitude of 44μm is only 7°, indicating that after ultrasonic treatment, the structure changes from polycrystalline plane distribution to single crystal plane distribution, and the orientation consistency is greatly improved.
[0113] In summary, the present invention applies an ultrasonic field before the directional solidification process and modulates the initial state of the interface so that after the growth starts, the crystal plane consistency of the columnar crystal growth is greatly improved, the efficiency of single crystal preparation is improved, and the cost is greatly reduced.
[0114] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing columnar oriented single crystals of alloy directional solidification by ultrasonic pre-modulation optimization. It is characterized in that The method comprises the following steps: Step 1, material loading: loading an alloy rod (20) for preparing a single crystal into a crucible (18) of an ultrasonic directional solidification device; the ultrasonic directional solidification device comprises a high temperature resistant pressure head (8) located at the top of the crucible (18) and an ultrasonic horn (2) located at the bottom of the crucible (18); the crucible (18) is clamped and fixed by the high temperature resistant pressure head (8) located at the top and the ultrasonic horn (2) located at the bottom; Step 2: preload adjustment: adjust the preload of the high temperature resistant pressure head (8) to a preset optimal preload; Step 3: Vacuuming: evacuate the directional solidification vacuum chamber of the ultrasonic directional solidification device to the daily working vacuum, and then fill it with protective gas; Step 4, heating initialization: start the heating system of the ultrasonic directional solidification device, make the heating temperature of the heating system reach the predetermined heating temperature T1, the alloy rod (20) is completely located in the heating system, melts evenly and keeps the temperature for a standing time t1, then stops heating; then, starts the motion system of the ultrasonic directional solidification device, makes the alloy rod (20) descend to the initial position of the alloy directional solidification, stops moving, and then stands for a standing time t2; Step 5: Ultrasonic pretreatment of the coagulation interface: adjust the output frequency and output voltage of the ultrasonic driving power supply (1) so that the end amplitude of the ultrasonic horn (2) is greater than the preset amplitude threshold As 0 , start the ultrasonic system of the ultrasonic directional solidification device, so that the ultrasonic wave acts on the solid-liquid initial interface of the alloy directional solidification, and make the ultrasonic system of the ultrasonic directional solidification device work continuously for at least a time longer than the preset ultrasonic pretreatment time threshold ts 0 After that, turn off the ultrasonic vibration; Step 6, directional solidification: starting the motion system and heating system of the ultrasonic directional solidification device to achieve directional solidification of the alloy rod (20) from bottom to top; Step 7, after the directional solidification is completed, the alloy rod (20) is unloaded: after the alloy rod (20) is completely solidified, the motion system and the heating system of the ultrasonic directional solidification device are turned off, and after the heating system is cooled to room temperature, the vacuum chamber of the ultrasonic directional solidification device is opened to take out the alloy after the directional solidification is completed.
2. The method for preparing columnar oriented single crystals by optimizing the ultrasonic pre-modulation of alloy directionally solidified according to claim 1, Features: The method for presetting the optimal preload force in step 2 is: Step B1, setting a heating temperature Th for single crystal preparation; Step B2: Look up the yield strength of the material used for the crucible (18) at the heating temperature Th and the yield strength of the material used for the ultrasonic horn (2) at the heating temperature Th in the material parameter table, compare the two, and record the smaller value as the yield strength σ s ; Step B3: Determine the value range of the preload force F as F min ~K F σ s ·S; Among them, F min is the minimum value of the preload force F, K F is the safety factor of the preload force, and S is the contact area between the ultrasonic horn (2) and the crucible (18); Step B4: Set the preload force F to F min The resonant frequency of the ultrasonic transducer is measured by an impedance analyzer and used as the operating frequency. The ultrasonic system of the ultrasonic directional coagulation device is started, and the output voltage of the ultrasonic driving power supply (1) is adjusted so that the end amplitude of the ultrasonic horn (2) is greater than A. min , and record the output voltage V of the ultrasonic driving power supply (1) at this time; where A min is the minimum value of the end amplitude of the ultrasonic horn (2); Step B5: Keep the output voltage V of the ultrasonic driving power supply (1) unchanged, and min ~K F σ s S, the value of the preload force F is changed multiple times. After each change of the preload force value, the resonance frequency of the ultrasonic transducer is measured with an impedance analyzer and used as the working frequency. The amplitude U of the wall of the crucible (18) is then measured with a laser vibrometer. The change of the amplitude U of the wall of the crucible (18) with the change of the preload force F is recorded, and a curve is drawn. The preload characteristic parameter f is obtained by curve fitting. 0 and the crucible (18) wall amplitude characteristic parameter U 0 ; Where, e is the natural logarithm; Step B6: Compare k f f 0 With K F σ s ·S size, the smaller value is determined as the optimal preload force; where k f is the characteristic coefficient of preload force.
3. The method for preparing columnar oriented single crystals by optimizing the ultrasonic pre-modulation of alloy directionally solidified according to claim 1, Features: The amplitude threshold As in step 5 0 and ultrasound pretreatment time threshold ts 0 The value of is: Step 501: Perform multiple experiments using the method of steps 1 to 7. During the multiple experiments, in step 5, multiple different amplitude values are selected within the maximum amplitude range at the end of the ultrasonic horn (2), and based on each amplitude value, the value of the amplitude is set at t min ~t max Select multiple different ultrasonic pretreatment times within the range, take longitudinal section samples after each alloy solidification, analyze the material crystal structure of a section of initial growth length L, check whether the longitudinal section is the same crystal plane, and take out the minimum effective ultrasonic pretreatment time for the longitudinal section to be the same crystal plane, and determine it as the ultrasonic pretreatment time threshold ts corresponding to the amplitude 0 , and obtain a set of amplitude As and ultrasonic pretreatment time threshold ts 0 The corresponding value of min is the minimum value of ultrasonic pretreatment time, t max is the maximum value of ultrasonic pretreatment time; Step 502: According to the formula Fitting is performed to obtain the formula The constant coefficient As 0 , Exponential term coefficient As 1 The value of the power coefficient τ gives the amplitude threshold As 0 The value of As is greater than the amplitude threshold As 0 When the value of Calculate the ultrasonic pretreatment time threshold ts corresponding to As 0 The value of ; where e is the natural logarithm and t is the time.
4. The method for preparing columnar oriented single crystals by optimizing the directional solidification of alloy by ultrasonic pre-modulation according to claim 3, Features: When checking whether the longitudinal section is the same crystal plane as described in step 501, an X-ray diffractometer is used to perform polycrystalline diffraction analysis. When the analysis result has only a single crystal plane diffraction peak, it is judged that the longitudinal section is the same crystal plane. Otherwise, it is judged that the longitudinal section is not the same crystal plane.
5. The method for preparing columnar oriented single crystals by optimizing the ultrasonic pre-modulation of alloy directionally solidified according to claim 3, Features: The min The value of is 1min, and the t max The value of is 2h; the value of L is 5mm~10mm.
6. The method for preparing columnar oriented single crystals by optimizing the ultrasonic pre-modulation of alloy directionally solidified according to claim 1, Features: In step 6, when the motion system and the heating system of the ultrasonic directional solidification device are started to realize the directional solidification of the alloy rod (20) from bottom to top, the motion system moves at a growth speed V. The value range of the growth speed V is determined by: When optimizing the cellular orientation of a material with a single-phase growth morphology, select Vc <V<Vd1; When optimizing the dendrite trunk crystal orientation of a material with a predominantly single-phase growth morphology, select Vd1 <V<Vd2; Among them, Vc is the transition speed from the flat interface to the cellular crystal of the material with a main single-phase growth morphology, Vd1 is the transition speed from the cellular crystal to the dendrite of the material with a main single-phase growth morphology, and Vd2 is the upper limit of the dendrite growth speed of the material with a main single-phase growth morphology.
7. The method for preparing columnar oriented single crystals by optimizing the ultrasonic pre-modulation of alloy directionally solidified according to claim 1, Features: The crucible (18) is a bottomless crucible with an open bottom, and the top end of the ultrasonic horn (2) is provided with a boss that protrudes upward and is used to be inserted into the bottom of the crucible (18).
8. The method for preparing columnar oriented single crystals by optimizing the ultrasonic pre-modulation of alloy directionally solidified according to claim 7, Features: The length of the boss is 1 mm to 5 mm, and the outer diameter of the boss is 0.2 mm to 0.5 mm smaller than the inner diameter of the crucible (18).
9. The method for preparing columnar oriented single crystals by optimizing the ultrasonic pre-modulation of alloy directionally solidified according to claim 7, Features: The top boss of the ultrasonic horn (2) is directly inserted into the crucible (18), the top boss of the ultrasonic horn (2) directly contacts the bottom of the alloy rod (20) loaded into the crucible (18), and the outer ring portion of the top boss of the ultrasonic horn (2) is in rigid contact with the crucible (18).
Citation Information
Patent Citations
Method and device for directionally solidifying liquid / solid interface based on ultrasonic wave modulation
CN102357654A
Monocrystal high-temperature alloy directional solidification growth device and method controlled by multi-mode static magnetic field and application of monocrystal high-temperature alloy directional solidification growth device
CN114164495A
Preparation method of multi-stage oriented growth metal material under multi-field action
CN114182352A
Method for making castings by directed solidification from a selected point of melt toward casting periphery
US20090242166A1