Water-based coating composition and coated article

By using melt-formed fluororesin particles and silica particles in the aqueous coating composition, combined with non-fluorine-based surfactant, the problem of warping of the fluororesin substrate in the high-frequency circuit is solved, and excellent electrical properties and surfaces are achieved The physical properties ensure the stability and performance of the high-frequency circuit substrate.

CN116390993BActive Publication Date: 2024-12-03DAIKIN INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180074931.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-06
Filing Date
2021-11-04
Publication Date
2024-12-03
Estimated Expiration
2041-11-04

AI Technical Summary

Technical Problem

In high-frequency circuit applications, fluororesin substrates are prone to warping during reflow soldering, resulting in unusability, and the prior art is difficult to effectively suppress this phenomenon.

Method used

Using an aqueous coating composition containing molten fluororesin particles and silica particles, and using a non-fluorine-based surfactant, a coating layer with excellent electrical properties and surface properties is formed by adjusting the particle size and specific surface area to suppress warping. The emergence of

Benefits of technology

It effectively suppresses warpage during reflow soldering, improves the matching and dispersion of the thermal expansion coefficient of the coating, ensures the smoothness and stability of the coating film, avoids hydrofluoric acid decomposition, and is suitable for high-frequency circuit substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004211715390000051
    Figure BDA0004211715390000051
  • Figure BDA0004211715390000052
    Figure BDA0004211715390000052
  • Figure BDA0004211715390000141
    Figure BDA0004211715390000141
Patent Text Reader

Abstract

The present invention provides an aqueous coating composition, which is an aqueous coating composition showing a low linear expansion coefficient, and can suppress the warping of a metal substrate such as copper foil by coating it. An aqueous coating composition, which is an aqueous coating composition containing fluororesin particles (A) that can be melt-formed, characterized in that the aqueous coating composition also contains silica particles (B), a non-fluorine-based surfactant (C) and water (D), the average particle size of the fluororesin particles (A) is 0.05 μm to 1000 μm, the average particle size of the silica particles (B) is 0.1 μm to 20 μm, the mixing ratio of the fluororesin particles (A) to the silica particles (B) is fluororesin particles (A): silica particles (B) = 10:90 to 90:10 (mass ratio), and the fluororesin particles (A) are contained in an amount of 15% to 80% by mass relative to 100% by mass of the coating solid content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to water-based coating compositions and coated articles. Background Art

[0002] Fluororesins are known to have various uses and various forms of use such as powders and films, taking advantage of their excellent heat resistance, weather resistance, oil resistance, solvent resistance, chemical resistance, and non-stickiness.

[0003] In printed wiring boards used in applications in the high-frequency region of several tens of GHz, laminates having an insulating layer formed thereon with a fluororesin are also mainly used from the viewpoints of dielectric properties and hygroscopicity.

[0004] Patent Document 1 discloses an aqueous coating composition for forming a coating layer composed of a fluororesin on a metal substrate.

[0005] Patent Document 2 discloses a coating composition for forming a coating layer composed of a fluororesin on a metal substrate, and further discloses that silica is blended therein.

[0006] Patent Documents 3 to 5 disclose aqueous coating compositions containing fluororesin particles.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 1994 / 05729

[0010] Patent Document 2: Japanese Patent Application Publication No. 2009-1767

[0011] Patent Document 3: Japanese Patent Application Laid-Open No. 5-301974

[0012] Patent Document 4: International Publication No. 2020 / 071382

[0013] Patent Document 5: International Publication No. 2018 / 016644 Summary of the invention

[0014] Problems to be solved by the invention

[0015] An object of the present disclosure is to provide an aqueous coating composition capable of suppressing warping of a metal substrate such as copper foil by applying the composition to the metal substrate.

[0016] Means for solving problems

[0017] The present disclosure relates to an aqueous coating composition, which is an aqueous coating composition containing melt-molded fluororesin particles (A), characterized in that:

[0018] The aqueous coating composition further comprises silica particles (B), a non-fluorinated surfactant (C) and water (D).

[0019] The average particle size of the fluororesin particles (A) is 0.05 μm to 1000 μm.

[0020] The average particle size of the silica particles (B) is 0.1 μm to 20 μm.

[0021] The mixing ratio of the fluororesin particles (A) and the silica particles (B) is fluororesin particles (A): silica particles (B) = 10:90 to 90:10 (mass ratio).

[0022] The fluororesin particles (A) are contained in an amount of 15 to 80% by mass based on 100% by mass of the coating solid content.

[0023] The aqueous coating composition preferably further contains a glycol solvent (E).

[0024] It is preferred that the diol solvent (E) does not remain after the fluororesin particles (A) are fired.

[0025] The maximum particle size of the silica particles (B) is preferably 10 μm or less.

[0026] The water dispersibility of the silica particles (B) is preferably 30% by mass or more.

[0027] The average particle size of the fluororesin particles (A) is preferably 0.1 to 100 angstroms.

[0028] The fluororesin particles (A) preferably have a volume-based cumulative 50% diameter of 0.05 μm to 40 μm.

[0029] The non-fluorine-based surfactant (C) is preferably a silicone-based surfactant.

[0030] The present disclosure also relates to a coated article, characterized in that the article has a coating layer formed by coating the above-mentioned aqueous coating composition.

[0031] The coated article may be a coated article having a coating layer formed by coating the aqueous coating composition on a metal substrate.

[0032] The coated article may be a printed circuit board, a dielectric material for a substrate, or a laminated circuit board.

[0033] Effects of the Invention

[0034] According to the present disclosure, it is possible to obtain an aqueous coating composition capable of forming a fluororesin coating layer having excellent electrical and surface properties and suppressed warpage without using a fluorine-based surfactant. DETAILED DESCRIPTION

[0035] If a fluororesin substrate is manufactured by laminating a fluororesin and a metal conductor, warping occurs during a reflow process at a temperature of about 260° C. A fluororesin substrate that has such warping cannot be used as a high-frequency circuit substrate.

[0036] Silicon dioxide has excellent fluorine corrosion resistance even at a reflow temperature of 260°C or above, and has a smaller thermal expansion coefficient than fluororesins. By forming a fluororesin coating layer mixed with the above-mentioned silicon dioxide, the difference between the thermal expansion coefficient of the coating layer and the thermal expansion coefficient of the metal substrate becomes smaller, and the generation of warping during reflow can be suppressed. Furthermore, in the water-based coating composition disclosed in the present invention, by using it in combination with a non-fluorine-based surfactant, the decomposition caused by hydrofluoric acid generated during reflow can be suppressed, and the effect brought by the mixed silicon dioxide can be effectively obtained.

[0037] The silica particles (B) preferably have a specific surface area of ​​1.0 m 2 / g~25.0m 2 / g, more preferably 1.0m 2 / g~10.0m 2 / g, more preferably 2.0m 2 / g~6.4m 2 When the specific surface area is within the above range, aggregation of silica in the film is reduced and the coating film surface is smooth, which is preferred.

[0038] The average particle size of the silica particles (B) is 0.1 μm to 20 μm. If the average particle size is within the above range, there is less aggregation and a good surface roughness can be obtained. The lower limit of the average particle size is preferably 0.1 μm, and more preferably 0.3 μm. The upper limit of the average particle size is preferably 5 μm, and more preferably 2 μm. The average particle size is a value measured by a laser diffraction / scattering method.

[0039] The maximum particle size of the silica particles (B) is preferably 10 μm or less. If the maximum particle size is 10 μm or less, there is less aggregation and the dispersion state is good. Furthermore, the surface roughness of the obtained coating can be reduced. The maximum particle size is more preferably 5 μm or less. For the maximum particle size, a SEM (scanning electron microscope) photo is taken and the image data of 200 randomly selected particles are obtained using SEM image analysis software.

[0040] The shape of the silica particles (B) is not particularly limited, and may be spherical, cylindrical, conical, truncated cone, polyhedral, hollow, etc. Spherical, cubic, basin-shaped, disc-shaped, octahedral, flaky, rod-shaped, plate-shaped, rod-shaped, quadrilateral, or hollow is particularly preferred, and spherical, cubic, octahedral, plate-shaped, or hollow is more preferred.

[0041] The water dispersibility of the silica particles (B) is preferably 30% by mass or more. If it is less than 30% by mass, the dispersibility becomes insufficient and the stability of the aqueous coating composition may be reduced.

[0042] Regarding the water dispersibility, silica and water were weighed in a container, and after sufficient shearing was applied to disperse the silica, stirring was stopped and it was confirmed that no precipitation occurred for several minutes.

[0043] The silica particles (B) may be surface-treated silica particles, for example, silica particles surface-treated with an organosilicon compound. The surface treatment with the organosilicon compound can reduce the dielectric constant of the silica particles (B).

[0044] The organosilicon compound is not particularly limited, and conventionally known organosilicon compounds can be used. For example, it is preferred that at least one selected from the group consisting of a silane coupling agent and an organosilazane is contained.

[0045] The surface treatment amount of the above-mentioned organic silicon compound is preferably 200 μg / cm2 per unit surface area (nm) 2 ) is 0.1 to 10, more preferably 0.3 to 7.

[0046] As the silica particles (B), one kind or two or more kinds of silica particles having different physical properties may be used.

[0047] The silica particles (B) may be used directly in the form of powder or in the form of powder dispersed in a resin.

[0048] The aqueous coating composition of the present disclosure is preferably blended with melt-moldable fluororesin particles (A). The use of such fluororesin particles (A) is preferred because the uniformity and film strength of the coating film after molding are improved, and the processability is improved.

[0049] The composition of the melt-moldable fluororesin particles (A) is not particularly limited, and examples thereof include tetrafluoroethylene [TFE] / hexafluoropropylene [HFP] copolymer [FEP], TFE / fluoroalkyl vinyl ether copolymer [PFA], TFE / HFP / fluoroalkyl vinyl ether copolymer [EPA], TFE / chlorotrifluoroethylene [CTFE] copolymer, TFE / ethylene copolymer [ETFE], polyvinylidene fluoride [PVdF], tetrafluoroethylene having a molecular weight of 300,000 or less [LMW-PTFE], etc. One kind may be used, or two or more kinds may be mixed.

[0050] As the fluoroalkyl vinyl ether, for example, at least one selected from the group consisting of the following substances is preferred:

[0051] General formula (110): CF 2 =CF-ORf 111

[0052] (Where Rf 111 represents a perfluorinated organic group. ) represents a fluorinated monomer;

[0053] General formula (120): CF 2 =CF-OCH 2 -Rf 121

[0054] (Where Rf 121 represents a fluorinated monomer represented by a perfluoroalkyl group having 1 to 5 carbon atoms;

[0055] General formula (130): CF 2 =CFOCF 2 O 131

[0056] (Where Rf 131 A fluorine-containing monomer represented by a linear or branched perfluoroalkyl group having 1 to 6 carbon atoms, a cyclic perfluoroalkyl group having 5 to 6 carbon atoms, or a linear or branched perfluorooxyalkyl group having 2 to 6 carbon atoms and containing 1 to 3 oxygen atoms;

[0057] General formula (140): CF 2 =CFO(CF 2 CF(Y 141 )O) m (CF 2 ) n F

[0058] (Where Y 141 represents a fluorine atom or a trifluoromethyl group. m is an integer from 1 to 4. n is an integer from 1 to 4. ) represents a fluorine-containing monomer; and

[0059] General formula (150): CF 2 =CF-O-(CF 2 CFY 151 -O) n -(CFY 152 ) m -A 151

[0060] (Where Y 151 Indicates fluorine atom, chlorine atom, -SO 2 F or perfluoroalkyl. The perfluoroalkyl group may contain ether oxygen and -SO 2 F group. n represents an integer of 0 to 3. n Y 151 Can be the same or different. 152 Represents a fluorine atom, a chlorine atom, or -SO 2 F group. m represents an integer of 1 to 5. m Y 152 Can be the same or different. 151 Indicates -SO 2 X 151 、-COZ 151 or-POZ 152 Z 153 .X 151 Indicates F, Cl, Br, I, -OR 151 or -NR 152 R 153 . Z 151 , Z 152 and Z 153 Same or different, indicates -NR 154 R 155 OR 156 . R 151 , R 152 , R 153 , R 154 , R 155 and R 156 are the same or different and represent H, ammonium, an alkali metal, an alkyl group which may contain a fluorine atom, an aryl group, or a sulfonyl group-containing group. ) is a fluorine-containing monomer.

[0061] In the present specification, the "perfluoroorganic group" refers to an organic group in which all hydrogen atoms bonded to carbon atoms are substituted with fluorine atoms. The perfluoroorganic group may have an ether oxygen.

[0062] Examples of the fluorinated monomer represented by the general formula (110) include Rf 111 A fluorine-containing monomer having a perfluoroalkyl group having 1 to 10 carbon atoms. The perfluoroalkyl group preferably has 1 to 5 carbon atoms.

[0063] Examples of the perfluoro organic group in the general formula (110) include a perfluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, a perfluorobutyl group, a perfluoropentyl group, and a perfluorohexyl group.

[0064] Examples of the fluorine-containing monomer represented by the general formula (110) include the following fluorine-containing monomers:

[0065] In the above general formula (110),

[0066] R 111 A fluorinated monomer which is a perfluoro(alkoxyalkyl) group having 4 to 9 carbon atoms;

[0067] R 111 Is the following formula:

[0068] [Chemistry 1]

[0069]

[0070] (wherein m represents 0 or an integer of 1 to 4.) a fluorine-containing monomer of a group represented by;

[0071] R 111 Is the following formula:

[0072] [Chemistry 2]

[0073]

[0074] (wherein n represents an integer of 1 to 4.) a fluorine-containing monomer having a group represented by the above; and the like.

[0075] As the fluorine-containing monomer represented by the general formula (110), among them, preferred are

[0076] General formula (160): CF 2 =CF-ORf 161

[0077] (Where Rf 161 represents a perfluoroalkyl group having 1 to 10 carbon atoms. ) is a fluorine-containing monomer. Rf 161 A perfluoroalkyl group having 1 to 5 carbon atoms is preferred.

[0078] The fluoroalkyl vinyl ether is preferably at least one selected from the group consisting of fluorinated monomers represented by general formulae (160), (130) and (140).

[0079] As the fluorinated monomer represented by the general formula (160), it is preferred to select at least one species from the group consisting of perfluoro(methyl vinyl ether), perfluoro(ethyl vinyl ether) and perfluoro(propyl vinyl ether), and it is more preferred to select at least one species from the group consisting of perfluoro(methyl vinyl ether) and perfluoro(propyl vinyl ether).

[0080] The fluorine-containing monomer represented by the general formula (130) is preferably selected from the group consisting of CF 2 =CFOCF 2 OCF 3 CF 2 =CFOCF 2 OCF 2 CF 3 and CF 2 =CFOCF 2 OCF 2 CF 2 OCF 3 At least one of the group consisting of.

[0081] The fluorinated monomer represented by the general formula (140) is preferably selected from the group consisting of CF 2 =CFOCF 2 CF(CF 3 )O(CF 2 ) 3 F. CF 2 =CFO(CF 2 CF(CF 3 )O) 2 (CF 2 ) 3 F and CF 2 =CFO(CF 2 CF(CF 3 )O) 2 (CF 2 ) 2 At least one of the group consisting of F.

[0082] The fluorine-containing monomer represented by the general formula (150) is preferably selected from the group consisting of CF 2 =CFOCF 2 CF 2 SO 2 F. CF 2 =CFOCF 2 CF(CF 3 )OCF 2 CF 2 SO 2 F. CF 2 =CFOCF 2 CF(CF 2 CF 2 SO 2 F)OCF 2 CF 2 SO 2 F and CF 2 =CFOCF 2 CF(SO 2 F)2 At least one of the group consisting of.

[0083] In the present specification, the "organic group" refers to a group containing one or more carbon atoms, or a group formed by removing one hydrogen atom from an organic compound.

[0084] Examples of the "organic group" include:

[0085] an alkyl group which may have one or more substituents,

[0086] an alkenyl group which may have one or more substituents,

[0087] an alkynyl group which may have one or more substituents,

[0088] a cycloalkyl group which may have one or more substituents,

[0089] a cycloalkenyl group which may have one or more substituents,

[0090] a cycloalkadienyl group which may have one or more substituents,

[0091] an aryl group which may have one or more substituents,

[0092] an aralkyl group which may have one or more substituents,

[0093] a non-aromatic heterocyclic group which may have one or more substituents,

[0094] a heteroaryl group which may have one or more substituents,

[0095] Cyano, formyl, RaO-, RaCO-, RaSO 2 -, RaCOO-, RaNRaCO-, RaCONRa-, RaOCO-, RaOSO 2 -、and RaNRbSO 2 -

[0096] (In these formulas, Ra is independently

[0097] an alkyl group which may have one or more substituents,

[0098] an alkenyl group which may have one or more substituents,

[0099] an alkynyl group which may have one or more substituents,

[0100] a cycloalkyl group which may have one or more substituents,

[0101] a cycloalkenyl group which may have one or more substituents,

[0102] a cycloalkadienyl group which may have one or more substituents,

[0103] an aryl group which may have one or more substituents,

[0104] an aralkyl group which may have one or more substituents,

[0105] A non-aromatic heterocyclic group which may have one or more substituents, or

[0106] a heteroaryl group which may have one or more substituents,

[0107] Rb is independently H or an alkyl group which may have one or more substituents).

[0108] As the organic group, an alkyl group which may have one or more substituents is preferred.

[0109] As the fluororesin particles (A), FEP, PFA or EPA is preferred from the viewpoint of non-stickiness and surface smoothness. PFA has a melting point of 300° C. or higher and is particularly preferred because it does not deform during brazing.

[0110] The average particle size of the fluororesin particles (A) is 0.05 to 1000 μm, preferably 0.1 to 100 μm, and more preferably 0.1 to 30 μm. When the average particle size is within the above range, a thin and smooth resin coating layer can be obtained, which is preferred.

[0111] The average particle size is, for example, a volume average particle size measured by a laser diffraction / scattering method. In order to adjust the fluororesin particles (A) to a desired particle size, classification using a sieve or wind force may be performed.

[0112] The volume-based cumulative 50% diameter of the fluororesin particles (A) is preferably 0.05 μm to 40 μm, and more preferably 7 μm to 40 μm. The volume-based cumulative 50% diameter is the particle diameter at the point where the cumulative volume becomes 50% on a cumulative curve obtained by measuring the particle size distribution by a laser diffraction / scattering method, with the total volume of the particle group being 100%. If the volume-based cumulative 50% diameter is within the above range, a thin and smooth coating resin layer can be formed, which is therefore preferred.

[0113] The method for producing the fluororesin particles (A) is not particularly limited, and specifically, for example, the fluororesin particles (A) can be produced by the method described in JP-A-2009-1767.

[0114] The polymerization method of the fluororesin constituting the fluororesin particles (A) is not particularly limited, and examples thereof include bulk polymerization, suspension polymerization, solution polymerization, emulsion polymerization, etc. In the above polymerization, various conditions such as temperature and pressure, polymerization initiator, and other additives can be appropriately set according to the desired composition and amount of the fluororesin.

[0115] The amount of the fluororesin particles (A) in the above-mentioned aqueous coating composition is 15% to 80% by mass of the total composition mass, preferably 15% to 75% by mass, and more preferably 20% to 50% by mass. If the amount of the fluororesin particles (A) is less than the above lower limit, the viscosity is too low, and even if it is applied to the surface of the article, it will immediately sag, and it is also impossible to apply thickly. On the other hand, if the amount of the fluororesin particles (A) is too much, the coating composition does not have fluidity and cannot be applied. The specific amount of mixing can be appropriately selected within the above range as long as the adjustment of the coating method and film thickness is considered, but in the case of spray coating, it is set to a relatively low concentration. On the other hand, in the case of press coating, it is set to more than 50% by mass to become a paste.

[0116] In the present disclosure, the solid content concentration of the aqueous coating composition is measured by a heating residual mass measurement method.

[0117] The aqueous coating composition disclosed in the present invention is fluororesin particles (A): silica particles (B) = 10:90 to 90:10 (mass ratio). By mixing fluororesin particles (A) and silica particles (B) in this ratio, effects such as preventing warping can be obtained. Regarding the above-mentioned mixing amount, the lower limit of the mixing amount of fluororesin particles (A) is more preferably 10, and more preferably 20. Regarding the above-mentioned mixing amount, the upper limit of the mixing amount of fluororesin particles (A) is more preferably 90, and more preferably 80. Regarding the above-mentioned mixing amount, the upper limit of the mixing amount of silica particles (B) is more preferably 60, and more preferably 50.

[0118] The aqueous coating composition of the present disclosure further contains a non-fluorine-based surfactant (C). Considering the cost, one of the reasons why the aqueous coating composition of the present disclosure is preferably containing a non-fluorine-based surfactant rather than a fluorine-based surfactant is one of the reasons.

[0119] Furthermore, when a fluorine-based surfactant is added, hydrofluoric acid is generated when the fluororesin particles (A) are calcined. This hydrofluoric acid promotes the degradation of the silica particles (B), so it is preferably not contained.

[0120] As the above-mentioned non-fluorine-based surfactant (C), there is no particular limitation as long as the fluororesin particles (A) can be stably dispersed in the composition, and any of anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants can be used. For example, anionic surfactants such as sodium alkyl sulfate, sodium alkyl ether sulfate, triethanolamine salt of alkyl sulfate, triethanolamine salt of alkyl ether sulfate, alkyl ammonium sulfate, alkyl ether ammonium sulfate, sodium alkyl ether phosphate, sodium fluoroalkyl carboxylate, etc.; cationic surfactants such as alkyl ammonium salts and alkyl benzyl ammonium salts; nonionic surfactants such as polyoxyethylene alkyl ether, polyoxyethylene phenyl ether, polyoxyethylene alkyl ester, propylene glycol-propylene oxide copolymer, perfluoroalkyl ethylene oxide adduct, 2-ethylhexanol ethylene oxide adduct; amphoteric surfactants such as alkylaminoacetic acid betaine, alkylamide acetic acid betaine, and imidazolium betaine. Among them, anionic and nonionic surfactants are preferred. Particularly preferred surfactants are nonionic surfactants with ethylene oxide chains with a small amount of thermal decomposition residues.

[0121] As the above-mentioned non-fluorine-based surfactant (C), hydrocarbon-based surfactants, silicone-based surfactants, acetylene-based surfactants such as acetylene glycols, etc. can also be used. In addition, one of these non-fluorine-based surfactants can be used or a combination of two or more can be used. It should be noted that it is preferred not to use nonylphenol-based surfactants.

[0122] As the above-mentioned non-fluorine-based surfactant (C), a silicone-based surfactant is particularly preferred. The above-mentioned silicone-based surfactant is not particularly limited, and examples thereof include polyoxyethylene (POE)-modified organopolysiloxane, polyoxyethylene·polyoxypropylene (POE·POP)-modified organopolysiloxane, POE sorbitan-modified organopolysiloxane, POE glycerin-modified organopolysiloxane and other organopolysiloxanes modified with a hydrophilic group.

[0123] Specific examples include DBE-712, DBE-821 (manufactured by AZmax), KP series, KF-6015, KF-6016, KF-6017, KF-6028 (manufactured by Shin-Etsu Chemical Co., Ltd.), ABIL-EM97 (manufactured by Goldschmidt Co., Ltd.), POLYFLOW KL-100, POLYFLOW KL-401, POLYFLOW KL-402, POLYFLOW KL-700 (manufactured by Kyoeisha Chemical), "FZ-77" (manufactured by Dow Corning Toray Co., Ltd.), and "BYK-333" (manufactured by BYK Japan KK).

[0124] The amount of the non-fluorine-based surfactant (C) is preferably 0.01% to 50% by mass, more preferably 0.1% to 30% by mass, and further preferably 0.2% to 20% by mass relative to 100% by mass of the fluororesin particles (A). If the amount of the surfactant added is too small, the dispersion of the fluororesin particles becomes uneven, and sometimes a part of them floats. On the other hand, if the amount of the surfactant added is too large, the decomposition residue of the surfactant caused by calcination becomes more and coloring occurs. In addition, the heat resistance and non-adhesiveness of the coating are reduced.

[0125] The aqueous coating composition disclosed herein contains water (D) as a solvent. Since the medium is water, it is preferred from the viewpoint of having little adverse effect on the environment.

[0126] Furthermore, the water-based coating composition disclosed herein preferably contains a water-soluble solvent in combination with water. The water-soluble solvent has the function of wetting the fluororesin particles (A), and the high-boiling-point solvent connects the resins to each other during drying after coating, and acts as a drying delay agent to prevent cracks. Even a high-boiling-point solvent will evaporate at the firing temperature of the fluororesin, so it will not have a negative effect on the coating film.

[0127] Specific examples of the water-soluble solvent include methanol, ethanol, isopropanol, sec-butyl alcohol, tert-butyl alcohol, acetone, methyl ethyl ketone, etc. as low-boiling point organic solvents with a boiling point of up to 100°C; methyl cellosolve, ethyl cellosolve, etc. as medium-boiling point organic solvents with a boiling point of 100°C to 150°C; N-methyl-2-pyrrolidone, N,N-dimethylacetamide, 3-butoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, N,N-dimethylformamide, ethylene glycol, propylene glycol, glycerin, dimethyl carbitol, butyl dicarbitol, butyl cellosolve, 1,4-butanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, etc. as high-boiling point organic solvents with a boiling point of more than 150°C. In addition, these water-soluble solvents can be used alone or in combination of two or more. As the water-soluble solvent, a high boiling point organic solvent is preferred, and among them, a glycol solvent (E) is more preferred from the viewpoint of dispersion stability and safety.

[0128] The mixing amount of the above-mentioned water-soluble solvent is preferably 0.5% to 50% by mass of the total water, and more preferably 1% to 30% by mass. In the case of a low-boiling point organic solvent, if the mixing amount is too little, it is easy to cause the mixing of bubbles, etc. If it is too much, the composition as a whole becomes flammable, which damages the advantages of the aqueous dispersion composition. In the case of a medium-boiling point organic solvent, if the mixing amount is too much, it sometimes remains in the coating film after firing and causes adverse effects. If it is too little, the fluororesin is restored to powder during drying after coating and cannot be fired. In the case of a high-boiling point organic solvent, if the mixing amount is too much, it sometimes remains in the coating film after firing and causes adverse effects. The above-mentioned water-soluble solvent preferably selects a solvent with a volatile property, or adjusts the mixing amount, etc., so that it will not remain in the coating film even after the firing of the above-mentioned fluororesin particles (A). The fact that the glycol solvent (E) does not remain after the calcination of the fluororesin particles (A) can be confirmed by scraping off the calcined coating film and determining by TG / DTA that there is no weight loss near the boiling point of the glycol solvent.

[0129] The aqueous coating composition disclosed herein may further contain a binder resin as required. However, in this case, it is preferred that the aqueous coating composition not contain 2 A resin having a weight loss of less than 55% at 400°C measured at 10°C / min. Even after heating for film formation, an aqueous coating composition containing such a resin may not completely decompose the binder resin and may remain, which may cause a decrease in the physical properties of the coating film.

[0130] The aqueous coating composition may be mixed with various additives commonly added to fluororesin compositions, such as pigments, stabilizers, thickeners, decomposition accelerators, rust inhibitors, preservatives, defoamers, etc. Examples of the pigments include inorganic pigments, composite oxide pigments, and white carbon, calcium carbonate, barium sulfate, talc, calcium silicate, etc.

[0131] The aqueous coating composition may be a clear coating containing no coloring pigment, or may be a colored coating containing a coloring pigment as required.

[0132] A coated article characterized by having a coating layer formed by coating the above-mentioned aqueous coating composition is also one of the present disclosures.

[0133] The above-mentioned aqueous coating composition can be applied by a coating method commonly used in coatings, and examples of the above-mentioned coating method include spray coating, roller coating, coating using a scraper, dipping (immersion) coating, infiltration coating, swirl coating, curtain flow coating, coating using a rod coater, gravure coating, micro gravure coating, etc.

[0134] After the above-mentioned coating, the coated article disclosed herein can be produced by drying and calcining. The above-mentioned drying is not particularly limited as long as the method can remove the aqueous medium. For example, a method of heating at room temperature to 130°C for 5 minutes to 30 minutes can be cited. The above-mentioned calcination is carried out at a temperature above the melting temperature of the fluororesin particles, and is usually preferably carried out at a range of 200°C to 400°C for 10 minutes to 60 minutes. In order to prevent oxidation of the coated metal foil, it is preferred to dry and calcine under an inert gas.

[0135] As the article substrate in the coated article disclosed in the present invention, the following can be used: metals such as iron, stainless steel, copper, aluminum, and brass; glass products such as glass plates, woven and non-woven fabrics of glass fibers; molded products and coverings of general-purpose and heat-resistant resins such as polypropylene, polyoxymethylene, polyimide, modified polyimide, polyamide-imide, polysulfone, polyethersulfone, polyetheretherketone, and liquid crystal polymers; molded products and coverings of general-purpose rubbers such as SBR, butyl rubber, NBR, and EPDM, and heat-resistant rubbers such as silicone rubber and fluororubber; woven and non-woven fabrics of natural fibers and synthetic fibers; or layered substrates formed by combining them, etc.

[0136] The article substrate may be a substrate that has been subjected to surface processing. Examples of the surface processing include surface processing roughened to a desired roughness by sandblasting, surface processing roughened by attaching particles, and surface processing subjected to metal anti-oxidation treatment.

[0137] The coated article disclosed herein can be used in fields requiring heat resistance, solvent resistance, lubricity, and non-adhesiveness, and can be used for films, fiber-reinforced films, prepregs, metal foils with resins, metal-clad laminates, printed circuit boards, dielectric materials for substrates, laminated circuit boards, and the like.

[0138] The coated article of the present disclosure preferably has a coating formed by the water-based coating composition of the present disclosure on copper foil. In recent years, in various fields, the communication in the high-frequency region becomes popular. In order to reduce the transmission loss when using in the high-frequency region, the dielectric layer containing fluoropolymer and the material formed by copper foil lamination are used. In such purposes, the water-based coating composition of the present disclosure can be used particularly suitably.

[0139] Example

[0140] Hereinafter, the present disclosure will be described by way of examples. In the examples, in the blending ratios, % and "parts" refer to mass % and mass parts unless otherwise specified. The present disclosure is not limited to the examples described below.

[0141] Example 1

[0142] Step 1. Pre-crushing (dry crushing)

[0143] Tetrafluoroethylene (TFE) / perfluorovinyl ether (PFVE) copolymer (PFA: melting point = 300°C, MFR = 25 g / 10 min) was produced by suspension polymerization, and the obtained dry powder was directly pulverized by a jet mill device (manufactured by IMMATERIAL) to obtain a fine powder with an average particle size of 10 μm.

[0144] Step 2. Premixing (predispersion)

[0145] Relative to 100 parts by mass of the PFA fine powder obtained in step 1., 10 parts by mass of an acetylene glycol dispersant (Surfynol 440, manufactured by Air Products Japan Co., Ltd.), 10 parts by mass of a silicone surfactant (KP-106, manufactured by Shin-Etsu Chemical Co., Ltd.) and 280 parts by mass of ion exchange water are thoroughly stirred and mixed with the PFA fine powder to obtain a PFA dispersion.

[0146] Step 3. Wet crushing

[0147] The PFA dispersion obtained in step 2 was filtered through a 100-mesh metal mesh and then passed through a high-pressure emulsifier (Nanomizer NMII, manufactured by Yoshida Machinery Co., Ltd., pulverization pressure = 200 MPa) to obtain a PFA fine powder dispersion (fluororesin particle (A-1) dispersion) having an average particle size of 0.20 μm (measured using CAPA700: manufactured by Horiba, Ltd.).

[0148] The volume-based cumulative 50% diameter of the obtained PFA fine powder was 0.20 μm.

[0149] Step 4. Coating

[0150] To 100 parts by mass of the PFA fine powder dispersion obtained in step 3., 2.5 parts by mass of a silicone surfactant (KP-106, manufactured by Shin-Etsu Chemical Co., Ltd.), 2.5 parts by mass of ethylene glycol (manufactured by Futaba Chemical Co., Ltd.), 58 parts by mass of silica particles, and 20 parts by mass of ion exchange water were added to form a coating.

[0151] It should be noted that the silica particles used were as follows.

[0152] B-1: Admafine SC2500-SQ manufactured by Admatechs, average particle size 0.5 μm, specific surface area 6.1 m 2 / g, maximum particle size 1.7μm

[0153] B-2: Admafine SC6500-SQ manufactured by Admatechs, average particle size 1.5 μm, specific surface area 4.0 m 2 / g, maximum particle size 4.2μm

[0154] It was confirmed that all silicas exhibited good water dispersibility at 70 mass %.

[0155] Embodiments 2 to 8

[0156] Except changing each compounding component as shown in Table 1, it carried out similarly to Example 1, and prepared the coating material.

[0157] Example 9

[0158] A coating (fluororesin particles (A-2) dispersion) was prepared in the same manner as in Example 1 except that PFA fine powder having an average particle size of 25 μm was used and the wet pulverization was omitted.

[0159] The volume-based cumulative 50% diameter of the obtained PFA fine powder was 22.9 μm.

[0160] Embodiments 10 to 16

[0161] Except changing each compounding component as shown in Table 2, it carried out similarly to Example 9, and prepared the coating material.

[0162] Examples 17 to 20

[0163] Coating was performed in the same manner as in Example 9 except that 10 parts by mass of a 10 wt % aqueous solution of polyvinyl alcohol (PVA, saponification degree: 78 to 82 mol % manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added as a binder resin and the respective blending components were changed as shown in Table 3.

[0164] Comparative Examples 1 to 4

[0165] Except changing each compounding component as shown in Table 4, the coating was prepared in the same manner as in Examples 1 and 9.

[0166] As a fluorine-based surfactant, 2.5 parts by mass of Ftergent 250 (manufactured by Neos Corporation) was added. In addition, in Comparative Example 4, ethylene glycol was not added and the coating was prepared.

[0167] The obtained coating composition was evaluated based on the following criteria.

[0168] The resin coating layer was obtained by the following method.

[0169] The coating was applied on copper foil (CF-V9S-SV-18 manufactured by Futian Metal Foil Powder Industry) using a rod coater (No. 40). The coated copper foil was dried at 130°C for 15 minutes and the powder falling was evaluated. Furthermore, the coating was fired at 350°C for 15 minutes in a nitrogen atmosphere to produce a coating film with a film thickness of 30 μm. No ethylene glycol remained in the fired coating film.

[0170] (Warp of copper-clad laminate)

[0171] The copper-clad laminate obtained was visually checked for the presence or absence of warping.

[0172] ×: Curled into a cylindrical shape.

[0173] △: Floating was observed.

[0174] ○: No floating was observed.

[0175] (falling powder)

[0176] When the sample was touched with a finger or pressed with a finger, the falling of the fluororesin powder was visually confirmed.

[0177] ×: Falling off was observed.

[0178] ○: No shedding was observed.

[0179] (Degradation of Silica)

[0180] The coated surface was examined by SEM to check whether the silica particles were deformed.

[0181] ×: There is deformation.

[0182] ○: No deformation.

[0183] [Table 1]

[0184]

[0185] [Table 2]

[0186]

[0187] [Table 3]

[0188]

[0189] [Table 4]

[0190]

[0191] From the results of Tables 1 to 4, it is understood that the aqueous coating composition of the present disclosure can form a good fluororesin coating layer that suppresses the warping of the copper foil and does not cause powder falling or deterioration of silica.

[0192] Industrial Applicability

[0193] According to the present disclosure, an aqueous coating composition can be obtained that can form a coating layer that suppresses warping of a substrate such as copper foil, and suppresses powder falling and degradation of silica particles. The aqueous coating composition is suitable for coating printed circuit boards, dielectric materials for substrates, laminated circuit boards, etc.

Claims

1. An aqueous coating composition comprising melt-molded fluororesin particles (A), characterized in that: The aqueous coating composition further comprises silica particles (B), a non-fluorinated surfactant (C) and water (D). The average particle size of the fluororesin particles (A) is 0.05 μm to 1000 μm, The average particle size of the silicon dioxide particles (B) is 0.1 μm to 20 μm, The mixing ratio of the fluororesin particles (A) to the silica particles (B) is fluororesin particles (A): silica particles (B) = 10:90 to 90:10 in terms of mass ratio. The fluororesin particles (A) are contained in an amount of 15 to 80% by mass based on 100% by mass of the coating solid content. 2 . The aqueous coating composition according to claim 1 , further comprising a glycol solvent (E).

3. The aqueous coating composition according to claim 2, wherein The glycol solvent (E) does not remain after the fluororesin particles (A) are fired.

4. The aqueous coating composition according to any one of claims 1 to 3, wherein The maximum particle size of the silica particles (B) is 10 μm or less.

5. The aqueous coating composition according to any one of claims 1 to 3, wherein The silica particles (B) are silica particles that can be uniformly dispersed when 70% by mass of silica particles and 30% by mass of water are mixed.

6. The aqueous coating composition according to any one of claims 1 to 3, wherein The average particle size of the fluororesin particles (A) is 0.1 μm to 100 μm.

7. The aqueous coating composition according to any one of claims 1 to 3, wherein The volume-based cumulative 50% diameter of the fluororesin particles (A) is from 0.05 μm to 40 μm.

8. The aqueous coating composition according to any one of claims 1 to 3, wherein The non-fluorine-based surfactant (C) is a silicone-based surfactant.

9. A coated article, characterized in that: The invention has a coating layer formed by coating the aqueous coating composition according to any one of claims 1 to 8.

10. The coated article according to claim 9, wherein A coating layer is provided on a metal substrate, which is formed by coating the aqueous coating composition according to any one of claims 1 to 8.

11. The coated article according to claim 9 or 10, which is a printed circuit board, a dielectric material for a substrate, or a laminated circuit board.