A method for preparing graphite for lithium ion battery

In the preparation of lithium-ion battery negative electrode materials, the low-temperature cross-linking reaction between gold salt and coke, combined with inert atmosphere and hydrochloric acid treatment, the safety hazards and cost problems of the high-temperature preparation process are solved, and the low temperature of high graphitization graphite is achieved Preparation and excellent electrochemical properties.

CN116395683BActive Publication Date: 2024-11-22WUXI HUARUI XINNENG BATTERY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310483309.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-22
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

The high-temperature preparation process of existing lithium-ion battery negative electrode materials consumes high energy and poses safety risks, making it difficult to achieve high graphitization at low temperatures, and cannot meet the safety and cost requirements of large-scale production.

Method used

The gold salt is annealed at high temperature in an inert atmosphere to form nano-gold particles and cross-link with coke at low temperatures. The graphitization is catalyzed by porous graphite coating, combined with the inert atmosphere and hydrochloric acid treatment, and the graphitization degree is higher than 90%. Graphite preparation.

Benefits of technology

It has achieved large-scale production of graphite with high graphitization under low temperature conditions, meets the requirements of negative electrode materials for lithium-ion batteries, shows excellent electrochemical performance, and has simple process and good repeatability, which can effectively recover and reuse gold salts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004208569730000011
    Figure HDA0004208569730000011
  • Figure HDA0004208569730000012
    Figure HDA0004208569730000012
  • Figure HDA0004208569730000013
    Figure HDA0004208569730000013
Patent Text Reader

Abstract

The present invention provides a method for preparing graphite for lithium ion batteries, comprising the following steps: (1) placing a gold salt in a tubular furnace, introducing a mixed gas of an inert gas and methane into the tubular furnace, annealing at 500-800°C for 1-10h, and obtaining a product A; (2) mixing product A and coke evenly, calcining under an inert atmosphere, crushing after cooling, soaking the crushed product in an N-methylpyrrolidone solution, filtering and drying to obtain a product B; (3) annealing product B under an inert atmosphere of 500-1100°C for 5-15h, washing the obtained product with hydrochloric acid, filtering and drying to obtain graphite for lithium ion batteries. The present invention can realize the low-temperature preparation of graphite, and the prepared graphite can meet the specification requirements of lithium battery negative electrode materials and show excellent electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of negative electrode materials for lithium ion batteries, and in particular to a method for preparing graphite for lithium ion batteries. Background Art

[0002] New energy vehicles have been increasing their market share in recent years, and they are mainly driven by lithium-ion batteries. The negative electrode material of lithium-ion batteries is artificial graphite. In 2022, the shipment volume of artificial graphite reached more than 500,000 tons. Artificial graphite is mainly made of needle coke derived from petroleum or coal. Graphite is obtained by thermally changing the soft carbon at a temperature above 2800°C. The degree of graphitization of the artificial graphite obtained in this way is higher than 90%, and the rate performance as a lithium-ion battery is good, such as CN112661149A and CN108550847B. These methods all use the principle of high-temperature phase change to make soft carbon spontaneously change to graphite crystals with high crystallinity from a kinetic point of view under an environment above 2800°C, but this process is a high-energy consumption process, and the production process is prone to thermal runaway, resulting in safety hazards. Therefore, finding a method for preparing a high degree of graphitization at low temperature can not only save costs, but also ensure safe production.

[0003] There are documents (Carbon 1979, 17, 131 and Carbon 2014, 75, 95) that proposed the idea of ​​low-temperature catalytic graphitization very early. However, from the intensity of the (002) peak in the XRD diagram of the product, it can be seen that the graphitization degree of the low-temperature graphite obtained is less than 50%, which is difficult to meet the parameter requirements of lithium-ion battery-grade graphite (graphitization degree is higher than 90%). CN108101043B uses magnesium metal as a catalyst to prepare low-temperature graphite with high graphitization at low temperature. Although it can meet the requirements of lithium-ion battery negative electrodes, its large-scale preparation process is still full of safety hazards. Because magnesium metal will release a lot of heat above 800°C, and for tons of graphite prepared, the heat released by this amount of magnesium metal will become a serious safety hazard. Therefore, it is necessary to find a method for preparing highly graphitized graphite at a gentle low temperature. Summary of the invention

[0004] In order to solve the above problems of the prior art, the present invention provides a method for preparing graphite for lithium-ion batteries, which can produce tons of graphite for lithium-ion batteries at a relatively low temperature without any safety hazards.

[0005] The present invention is achieved through the following technical solutions:

[0006] A method for preparing graphite for lithium-ion batteries comprises the following steps:

[0007] (1) placing a gold salt in a tube furnace, introducing a mixed gas of an inert gas and methane into the tube furnace, and annealing at 500 to 800° C. for 1 to 10 hours to obtain a product A;

[0008] (2) mixing product A and coke uniformly, calcining under an inert atmosphere, crushing after cooling, soaking the crushed product in an N-methylpyrrolidone solution, filtering and drying to obtain product B;

[0009] (3) annealing the product B at 500-1100° C. in an inert atmosphere for 5-15 h, washing the obtained product with hydrochloric acid, filtering and drying to obtain graphite for lithium-ion batteries.

[0010] Preferably, in step (1), the gold salt is potassium chloroaurate, gold hydroxide, gold iodide, sodium tetrachloroaurate or ammonium tetrachloroaurate.

[0011] Preferably, in step (1), the volume ratio of methane to inert gas in the mixed gas is (0.5-3):10.

[0012] Preferably, in step (1), the inert gas is argon.

[0013] Preferably, in step (2), the coke is calcined coke, calcined coke or needle coke.

[0014] Preferably, in step (2), the mass ratio of the product A to the coke is 1:(10-500).

[0015] Preferably, in step (2), the calcination conditions are: pressure 0.1-1 MPa, temperature 230° C., and time 5 h.

[0016] Preferably, in step (2) and step (3), the inert atmosphere is an argon atmosphere.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] In the method of the present invention, the gold salt is pyrolyzed into nano-gold particles under high temperature conditions in a methane atmosphere, and the surface of the nano-gold particles is coated with a thin layer of porous graphite; the nano-gold particle catalyst and the coke are in closer contact during low-temperature pyrolysis under pressure, and the thin-layer graphite and the coke are cross-linked; in the subsequent pyrolysis process, the gold catalyzes the coke to be low-temperature graphitized near the thin-layer graphite, and a low-temperature artificial graphite with a graphitization degree of more than 90% is obtained. The method of the present invention can realize the low-temperature preparation of graphite, and the prepared graphite can meet the specification requirements of lithium battery negative electrode materials and show excellent electrochemical properties. After button battery half-cell testing, it is found that it has lithium battery performance that is not inferior to high-end commercial artificial graphite. The process of the present invention is simple, reproducible, and can be mass-produced, and the gold salt obtained by impurity removal can be effectively recycled for secondary use. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The X-ray diffraction spectra of the graphite materials prepared in Examples 1 to 4 of the present invention are shown.

[0020] Figure 2 This is a SEM image of the graphite material prepared in Example 2 of the present invention.

[0021] Figure 3 This is the Raman spectrum of the graphite material prepared in Example 3 of the present invention.

[0022] Figure 4 This is a charge and discharge curve diagram of the graphite material prepared in Example 4 of the present invention as a lithium battery negative electrode material. DETAILED DESCRIPTION

[0023] In order to further understand the present invention, the present invention is described below in conjunction with embodiments. These descriptions are only to further explain the features and advantages of the present invention and are not intended to limit the claims of the present invention.

[0024] The method for preparing graphite for lithium-ion batteries according to the present invention comprises the following steps:

[0025] (1) The gold salt is placed in a tube furnace, and argon-loaded methane gas (the volume ratio of methane to argon is (0.5-3):10) is introduced, and annealing is performed at 500-800° C. for 1-10 h. The obtained product is recorded as product A.

[0026] (2) Product A and coke are uniformly mixed in a mass ratio of 1:(10-500), first calcined for 5 h at a pressure of 0.1-1 MPa and an argon atmosphere of 230°C, and then crushed after cooling. The crushed product is soaked in an N-methylpyrrolidone solution for 12 h, and the product obtained after filtering and drying is recorded as product B.

[0027] (3) annealing the product B at 500-1100° C. in an argon atmosphere for 5-15 h, washing the product with 1M hydrochloric acid to remove gold impurities, filtering and drying the product to obtain artificial low-temperature graphite for lithium-ion batteries with a graphitization degree of more than 90%.

[0028] The gold salt in step (1) is potassium chloroaurate, gold hydroxide, gold iodide, sodium tetrachloroaurate or ammonium tetrachloroaurate.

[0029] The coke in step (2) is calcined coke, calcined coke or needle coke.

[0030] Example 1

[0031] (1) 1 g of potassium chloroaurate was placed in a tubular furnace with a diameter of 60 mm, and argon-loaded methane gas (the volume ratio of methane to argon was 0.5:10) was introduced. The mixture was annealed at 500° C. for 10 h. The obtained product was recorded as product A.

[0032] (2) Product A and calcined coke were mixed uniformly in a mass ratio of 1:10, and calcined for 5 h at a pressure of 0.1 MPa and an argon atmosphere of 230° C. After cooling, the mixture was crushed. The crushed product was soaked in an N-methylpyrrolidone solution for 12 h, and the product obtained after filtration and drying was recorded as product B.

[0033] (3) The product B is annealed at 500° C. in an argon atmosphere for 15 h, and the product is pickled with 1M hydrochloric acid to remove gold impurities. After filtering and drying, artificial low-temperature graphite for lithium-ion batteries with a graphitization degree of more than 90% can be obtained.

[0034] Example 2

[0035] (1) 50 g of gold hydroxide was placed in a tubular furnace with a diameter of 60 mm, and argon-loaded methane gas (the volume ratio of methane to argon was 1:10) was introduced, and annealed at 600° C. for 8 h. The obtained product was recorded as product A.

[0036] (2) Product A and pre-calcined coke were uniformly mixed in a mass ratio of 1:100, and first calcined for 5 h under a pressure of 0.3 MPa and an argon atmosphere of 230° C., and then crushed after cooling. The crushed product was soaked in an N-methylpyrrolidone solution for 12 h, and the product obtained after filtering and drying was recorded as product B.

[0037] (3) The product B is annealed at 700° C. in an argon atmosphere for 10 h, and the product is pickled with 1M hydrochloric acid to remove gold impurities. After filtering and drying, artificial low-temperature graphite for lithium-ion batteries with a graphitization degree of more than 90% is obtained.

[0038] Example 3

[0039] (1) 100 g of gold salt was placed in a tubular furnace with a diameter of 60 mm, and argon-loaded methane gas (the volume ratio of methane to argon was 2:10) was introduced, and annealed at 700° C. for 4 h. The obtained product was recorded as product A.

[0040] (2) Product A and needle coke were mixed evenly in a mass ratio of 1:300, and calcined for 5 h at a pressure of 0.7 MPa and an argon atmosphere of 230° C. After cooling, the mixture was crushed. The crushed product was immersed in an N-methylpyrrolidone solution for 12 h, and the product obtained after filtration and drying was recorded as product B.

[0041] (3) The product B is annealed at 900° C. in an argon atmosphere for 9 h, and the product is pickled with 1M hydrochloric acid to remove gold impurities. After filtering and drying, lithium ion battery-grade artificial low-temperature graphite with a graphitization degree of more than 90% is obtained.

[0042] Example 4

[0043] (1) 200 g of gold salt was placed in a tubular furnace with a diameter of 60 mm, and argon-loaded methane gas (the volume ratio of methane to argon was 3:10) was introduced, and annealed at 800° C. for 1 h. The obtained product was recorded as product A.

[0044] (2) Product A and calcined coke were mixed evenly in a mass ratio of 1:500, and calcined for 5 h at a pressure of 1 MPa and an argon atmosphere of 230°C. After cooling, the mixture was crushed, and the crushed product was soaked in an N-methylpyrrolidone solution for 12 h. The product obtained after filtration and drying was recorded as product B.

[0045] (3) The product B is annealed at 1100° C. in an argon atmosphere for 5 h, and the product is pickled with 1M hydrochloric acid to remove gold impurities. After filtering and drying, lithium ion battery-grade artificial low-temperature graphite with a graphitization degree of more than 90% is obtained.

[0046] like Figure 1 The graphite X-ray diffraction spectra prepared in Examples 1 to 4 of the present invention are shown in FIG. 1 , wherein the horizontal axis is the angle, and the vertical axis is the relative intensity, using 30 wt% silicon as a reference standard. Figure 1 It can be seen that the present invention prepares a graphite material, the highest peak of which corresponds to the (002) diffraction plane of graphite. It is calculated that the graphitization degree of the graphite of the present invention is 92.3%.

[0047] like Figure 2 , which is a scanning electron microscope image of the graphite prepared in Example 2 of the present invention, it can be found from the image that the obtained graphite is in the form of flakes.

[0048] like Figure 3 , which is the Raman spectrum of the graphite prepared in Example 3 of the present invention. It can be seen from the figure that the intensity of the G peak is much greater than the intensity of the D peak, proving that the obtained graphite has a high degree of graphitization.

[0049] like Figure 4 As shown, it is a charge and discharge curve diagram of the graphite prepared in Example 4 of the present invention as a negative electrode material for a lithium ion battery. It can be seen from the figure that it exhibits good electrochemical properties when used as a negative electrode material for a lithium ion battery.

[0050] The present invention is not limited to the specific embodiments listed above. Those skilled in the art can make various equivalent modifications, equivalent replacements, component additions and subtractions, and recombinations based on the working principle of the present invention and the specific embodiments given above, so as to form more new embodiments.

Claims

1. A method for preparing graphite for lithium ion batteries, characterized in that: The steps include: (1) placing a gold salt in a tube furnace, introducing a mixture of inert gas and methane into the tube furnace, and annealing at 500-800°C for 1-10 hours to obtain product A; (2) Product A and coke are uniformly mixed, calcined under an inert atmosphere, and crushed after cooling. The crushed product is immersed in an N-methylpyrrolidone solution, filtered, and dried to obtain Product B; (3) Annealing the product B at 500-1100° C. in an inert atmosphere for 5-15 h, washing the obtained product with hydrochloric acid, filtering and drying the obtained product to obtain graphite for lithium-ion batteries.

2. The method for preparing graphite for lithium ion batteries according to claim 1, wherein In step (1), the gold salt is potassium chloroaurate, gold hydroxide, gold iodide, sodium tetrachloroaurate or ammonium tetrachloroaurate.

3. The method for preparing graphite for lithium ion batteries according to claim 1, wherein In step (1), the volume ratio of methane to inert gas in the mixed gas is (0.5-3):

10.

4. The method for preparing graphite for lithium ion batteries according to claim 1, wherein In step (1), the inert gas is argon.

5. The method for preparing graphite for lithium ion batteries according to claim 1, wherein In step (2), the coke is calcined coke, pre-calcined coke or needle coke.

6. The method for preparing graphite for lithium ion batteries according to claim 1, wherein In step (2), the mass ratio of the product A to the coke is 1:(10-500).

7. The method for preparing graphite for lithium ion batteries according to claim 1, wherein In step (2), the calcination conditions are: pressure 0.1-1 MPa, temperature 230° C., and time 5 h.