A method for softening and finishing linen fabric
Through two rounds of liquid nitrogen and alkaline water treatment and tyrosin enzymatic reaction, polypolyphenol compounds are formed to be embedded on the surface of linen fabric, solving the problem of poor softness of linen fabric and significantly improving its softness and wrinkle resistance.
Patent Information
- Application Number
- CN202310432844.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-04-21
AI Technical Summary
Linen fabrics have poor softness and wrinkle resistance, which affects their performance.
After two rounds of liquid nitrogen and alkaline water bath, the reaction was carried out using buffer solutions of tyrosine, acid cellulase, laccase and horseradish peroxidase, and oxygen was introduced to form polypolyphenol compound embedded fibers. The surface destroys the large crystalline region, forms covalent bonds, and improves softness and wrinkle resistance.
The softness and wrinkle resistance of linen fabrics are significantly improved, and the internal crystallization zone of the fiber is destroyed by repeated emergency freezing and alkali cooking, and the surfactant is formed through enzymatic oxidation, enhancing the frictional properties of the fibers.
Smart Images

Figure BDA0004190890720000031 
Figure BDA0004190890720000032
Abstract
Description
Technical Field
[0001] The invention belongs to the field of textile engineering, and in particular relates to a linen fabric softening and finishing method. Background Art
[0002] Flax is an important raw material for clothing fabrics in the linen textile industry. Its fibers are strong, soft, and have good color. Flax fibers are strong, not easy to rot in water, and have waterproof properties. In addition, they have unique advantages such as friction resistance, high temperature resistance, fast heat dissipation, low dust absorption rate, not easy to tear, not easy to burn, no static electricity, and high acid and alkali resistance. It is the preferred textile raw material for the pursuit of green and environmental protection and is known as the "Queen" of natural fibers. However, this type of fabric has poor softness, feels rough, is easy to wrinkle, and has a tingling feeling, which to a certain extent affects its wearing performance. Summary of the invention
[0003] In view of this, the object of the present invention is to provide a method for softening and finishing linen fabrics, which can significantly increase the softness and wrinkle resistance of linen fabrics after finishing.
[0004] In order to solve the above technical problems, the technical solutions provided by the present invention are as follows:
[0005] A linen fabric softening and finishing method comprises the following steps:
[0006] S1: washing and drying the linen fabric, and then successively immersing it in liquid nitrogen and alkaline water for two rounds, and then washing and drying it; the two rounds of immersing in liquid nitrogen and alkaline water are specifically immersing in alkaline water after liquid nitrogen treatment, and then immersing in liquid nitrogen and alkaline water in sequence;
[0007] S2: Put the linen fabric in step S1 into a NaAc-HAc buffer solution containing tyrosine and a mixed enzyme preparation, and after the first stage reaction, add 2,2,6,6-tetramethyl-1-piperidinyloxy free radical, continue to introduce oxygen into the solution, and carry out the second stage reaction, and then wash with water and dry.
[0008] Preferably, in step S1, the alkaline water is sodium hydroxide or potassium hydroxide solution with a concentration of 50-60 g / L and a temperature of 85-95°C.
[0009] Preferably, in step S2, the mixed enzyme preparation is mixed with acid cellulase, laccase and horseradish peroxidase in a mass ratio of 1:2:(0.01-0.05).
[0010] The preferred activities of the acid cellulase, laccase and horseradish peroxidase in the mixed enzyme preparation are 80000-100000 U / g, 10000-20000 U / g and 240000-300000 U / g respectively.
[0011] Preferably, in step S2, the pH value of the NaAc-HAc buffer solution is in the range of 4.0-5.0, and the concentration is 0.1-0.12 mol / L.
[0012] Preferably, in step S2, the dosage of tyrosine and the mixed enzyme preparation is 0.065-0.074 g / g of linen fabric and 0.23-0.45 g / g of linen fabric, respectively.
[0013] Preferably, in step S2, the amount of 2,2,6,6-tetramethyl-1-piperidinyloxy free radical used is 0.05-0.08 g / g of linen fabric.
[0014] Preferably, in step S2, the oxygen ventilation rate is 0.5-0.8 V / (V·min).
[0015] Preferably, in step S2, the first stage reaction temperature is 30-37° C., and the reaction time is 12-24 h.
[0016] Preferably, in step S2, the second stage reaction temperature is 35-40°C, and the reaction time is 6-12h.
[0017] Compared with the prior art, the finishing method of the present invention combines repeated quick freezing and alkali boiling to crush the large crystal area inside the cellulose by the generated ice crystals to generate small crystal areas, and then utilizes tyrosine to be oxidized by the mono-oxygenation and di-oxygenation of laccase and horseradish peroxidase to form polyphenol compounds as grafted polymer groups to be embedded in the cracks on the surface of the linen fabric and the gaps in the small crystal areas, so that the friction between the fibers is reduced, resulting in significantly improved softness and wrinkle resistance. In addition, the covalent bonding of the polyphenol compounds to the cellulose is through the cellulose oxidation of laccase / TEMPO to generate aldehyde groups that react with the amino groups on the polyphenol compounds to generate Schiff bases. Since the polyphenol compounds are formed by tyrosine and retain a large number of amino groups and carboxyl groups, they also show the properties of polyphenol amphoteric surfactants on the surface of the linen fibers, further improving the softening finishing effect. DETAILED DESCRIPTION
[0018] The present invention can be better understood according to the following examples. However, it is easy for those skilled in the art to understand that the contents described in the examples are only used to illustrate the present invention, and should not and will not limit the present invention described in detail in the claims.
[0019] Example 1
[0020] A linen fabric softening and finishing method comprises the following steps:
[0021] 1. Wash and dry the linen fabric, treat it with liquid nitrogen, and then soak it in a 92°C 54g / L sodium hydroxide solution, then soak it in liquid nitrogen and a 92°C 54g / L sodium hydroxide solution in sequence, then wash and dry it;
[0022] 2. A mixed enzyme preparation was prepared by mixing acid cellulase with an activity of 92000 U / g, laccase with an activity of 16000 U / g and horseradish peroxidase with an activity of 280000 U / g in a mass ratio of 1:2:0.04;
[0023] 3. The linen fabric of step 1 is put into a 0.11 mol / L NaAc-HAc buffer solution of pH 4.5 containing tyrosine and a mixed enzyme preparation, wherein the amounts of tyrosine and the mixed enzyme preparation are 0.07 g / g linen fabric and 0.4 g / g linen fabric, respectively, and the first stage reaction is carried out at a temperature of 32° C. and a reaction time of 18 h. Then, 0.07 g / g linen fabric of 2,2,6,6-tetramethyl-1-piperidinyloxy free radical is added, and oxygen is continuously introduced into the solution at a ventilation rate of 0.6 V / (V·min). The second stage reaction is carried out at a temperature of 37° C. and a reaction time of 10 h. Finally, the reaction is washed with water and dried.
[0024] Example 2
[0025] A linen fabric softening and finishing method comprises the following steps:
[0026] 1. After washing and drying the linen fabric, it is immersed in liquid nitrogen and 85℃ 60g / L potassium hydroxide solution for two rounds, and then washed and dried;
[0027] 2. A mixed enzyme preparation was prepared by mixing acid cellulase with an activity of 100000 U / g, laccase with an activity of 10000 U / g, and horseradish peroxidase with an activity of 300000 U / g in a mass ratio of 1:2:0.01;
[0028] 3. The linen fabric of step 1 is placed in a 0.1 mol / L NaAc-HAc buffer solution of pH 4.0 containing tyrosine and a mixed enzyme preparation, wherein the amounts of tyrosine and the mixed enzyme preparation are 0.065 g / g of linen fabric and 0.45 g / g of linen fabric, respectively, and a first-stage reaction is carried out at a temperature of 30° C. for a reaction time of 24 h. Subsequently, 0.05 g / g of 2,2,6,6-tetramethyl-1-piperidinyloxy free radical is added to the linen fabric, and oxygen is continuously introduced into the solution at a ventilation rate of 0.5 V / (V·min). A second-stage reaction is carried out at a temperature of 40° C. for a reaction time of 6 h, and finally the reaction is washed with water and dried.
[0029] Example 3
[0030] A linen fabric softening and finishing method comprises the following steps:
[0031] 1. After washing and drying the linen fabric, it is immersed in liquid nitrogen and 95℃ 50g / L sodium hydroxide solution for two rounds, and then washed and dried;
[0032] 2. A mixed enzyme preparation was prepared by mixing acid cellulase with an activity of 80,000 U / g, laccase with an activity of 20,000 U / g, and horseradish peroxidase with an activity of 240,000 U / g in a mass ratio of 1:2:0.05;
[0033] 3. The linen fabric of step 1 is put into a 0.12 mol / L NaAc-HAc buffer solution of pH 5.0 containing tyrosine and a mixed enzyme preparation, wherein the amounts of tyrosine and the mixed enzyme preparation are 0.074 g / g linen fabric and 0.23 g / g linen fabric, respectively, and the first stage reaction is carried out at a temperature of 37° C. for a reaction time of 12 h. Thereafter, 0.08 g / g linen fabric of 2,2,6,6-tetramethyl-1-piperidinyloxy free radical is added, and oxygen is continuously introduced into the solution at a ventilation rate of 0.8 V / (V·min). The second stage reaction is carried out at a temperature of 35° C. for a reaction time of 12 h, and finally the product is washed with water and dried.
[0034] Comparative Example 1 (no freeze-thaw)
[0035] A linen fabric softening and finishing method comprises the following steps:
[0036] 1. A mixed enzyme preparation was prepared by mixing acid cellulase with an activity of 92000U / g, laccase with an activity of 16000U / g and horseradish peroxidase with an activity of 280000U / g in a mass ratio of 1:2:0.04;
[0037] 2. After washing and drying the linen fabric, put it into a 0.11 mol / L NaAc-HAc buffer solution with a pH of 4.5 containing tyrosine and a mixed enzyme preparation, the dosage of tyrosine and the mixed enzyme preparation are 0.07 g / g linen fabric and 0.4 g / g linen fabric respectively, and carry out the first stage reaction at a temperature of 32°C for 18 hours. Then, 0.07 g / g linen fabric of 2,2,6,6-tetramethyl-1-piperidinyloxy free radical is added, and oxygen is continuously introduced into the solution at a ventilation volume of 0.6 V / (V·min). The second stage reaction is carried out at a temperature of 37°C for 10 hours. Finally, wash with water and dry.
[0038] Comparative Example 2 (without TEMPO)
[0039] A linen fabric softening and finishing method comprises the following steps:
[0040] 1. After washing and drying the linen fabric, it is immersed in liquid nitrogen and 92℃ 54g / L sodium hydroxide solution for two rounds, and then washed and dried;
[0041] 2. A mixed enzyme preparation was prepared by mixing acid cellulase with an activity of 92000 U / g, laccase with an activity of 16000 U / g and horseradish peroxidase with an activity of 280000 U / g in a mass ratio of 1:2:0.04;
[0042] 3. The linen fabric of step 1 was placed in a 0.11 mol / L NaAc-HAc buffer solution of pH 4.5 containing tyrosine and a mixed enzyme preparation, wherein the amounts of tyrosine and the mixed enzyme preparation were 0.07 g / g of linen fabric and 0.4 g / g of linen fabric, respectively, and the first stage reaction was carried out at a temperature of 32° C. for 18 h, and then oxygen was continuously introduced into the solution at a ventilation rate of 0.6 V / (V·min), and the second stage reaction was carried out at a temperature of 37° C. for 10 h, and finally washed with water and dried.
[0043] Comparative Example 3 (without tyrosine)
[0044] A linen fabric softening and finishing method comprises the following steps:
[0045] 1. After washing and drying the linen fabric, it is immersed in liquid nitrogen and 92℃ 54g / L sodium hydroxide solution for two rounds, and then washed and dried;
[0046] 2. A mixed enzyme preparation was prepared by mixing acid cellulase with an activity of 92000 U / g, laccase with an activity of 16000 U / g and horseradish peroxidase with an activity of 280000 U / g in a mass ratio of 1:2:0.04;
[0047] 3. The linen fabric of step 1 is put into a 0.11 mol / L NaAc-HAc buffer solution of pH 4.5 containing a mixed enzyme preparation, the amount of the mixed enzyme preparation is 0.4 g / g of linen fabric, and the first stage reaction is carried out at a temperature of 32° C. and a reaction time of 18 h. Then, 0.07 g / g of 2,2,6,6-tetramethyl-1-piperidinyloxy free radical is added to the linen fabric, and oxygen is continuously introduced into the solution at a ventilation rate of 0.6 V / (V·min). The second stage reaction is carried out at a temperature of 37° C. and a reaction time of 10 h. Finally, the reaction is washed with water and dried.
[0048] Wrinkle recovery angle test
[0049] According to GB / T 3819-1997 “Determination of Crease Recovery of Textile Fabrics - Recovery Angle Method”, the YG(B)541E intelligent fabric wrinkle elasticity tester was used to test the wrinkle recovery angle of linen fabrics before and after finishing. The results are shown in Table 1.
[0050] Table 1
[0051]
[0052] As can be seen from Table 1, the wrinkle recovery angle of the linen fabric treated by the finishing method of the present invention is significantly reduced. Comparative Example 1 does not destroy the large crystal area, and the enzyme preparation and the surface modified molecules cannot penetrate into the fiber core. Comparative Example 2 does not oxidize the free hydroxyl groups of cellulose and cannot form Schiff bases with polyphenols. Although polyphenols can penetrate into the fiber core during the finishing process, there is no covalent bonding and a stable finishing effect cannot be obtained. Comparative Example 3 does not have tyrosine and cannot form polyphenol compounds. Only when tyrosine is present can laccase and horseradish peroxidase catalyze the synthesis of polyphenol zwitterionic compounds, which are the key molecules for surface modification. The key molecule cannot be formed in Comparative Example 3, so a significant softening effect cannot be obtained.
[0053] Stiffness test
[0054] According to GB / T 18318-2001 “Determination of bending length of textile fabrics”, HD207N automatic fabric stiffness tester was used to take 5 samples in warp and weft directions for testing. The results are shown in Table 2.
[0055] Table 2
[0056]
[0057] As can be seen from Table 2, the stiffness of the linen fabric treated by the finishing method of the present invention is significantly reduced, that is, the softness is significantly improved. This is mainly because the crystal area of the linen fabric is destroyed by repeated quick freezing and alkali boiling and the action of acid cellulase, and a part of the glycosidic bonds are also broken, which provides good conditions for the subsequent oxidation of the free hydroxyl groups of cellulose by the laccase / TEMPO system. Comparative Examples 1 and 2 cannot form effective active aldehyde groups for the grafting of polyphenol amphiphilic compounds. Comparative Example 3 cannot form polyphenol amphiphilic compounds and their active amino groups, so the softening finishing effect of the embodiment cannot be obtained.
[0058] The present invention provides a linen fabric softening finishing method and method. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. A method for softening and finishing linen fabric, characterized in that: The steps include: S1. After washing and drying the linen fabric, two rounds of liquid nitrogen and alkaline water immersion were carried out, followed by washing and drying, wherein the alkaline water immersion temperature was 85-95°C; S2. Put the linen fabric treated in step S1 into a NaAc-HAc buffer solution containing tyrosine and a mixed enzyme preparation, and after the first stage reaction, add 2,2,6,6-tetramethyl-1-piperidinyloxy free radical, continue to introduce oxygen into the solution, and carry out the second stage reaction, and then wash with water and dry; the mixed enzyme preparation is a mixture of acid cellulase, laccase, and horseradish peroxidase in a mass ratio of 1:2:(0.01-0.05).
2. A linen fabric softening and finishing method according to claim 1, characterized in that: In step S1, the alkaline water is a sodium hydroxide solution or a potassium hydroxide solution with a concentration of 50-60 g / L.
3. A linen fabric softening and finishing method according to claim 1, characterized in that: The activity of the acid cellulase is 80000-100000 U / g, the activity of the laccase is 10000-20000 U / g, and the activity of the horseradish peroxidase is 240000-300000 U / g.
4. A linen fabric softening and finishing method according to claim 1, characterized in that: In step S2, the pH value of the NaAc-HAc buffer solution ranges from 4.0 to 5.0, and the concentration ranges from 0.1 to 0.12 mol / L.
5. A linen fabric softening and finishing method according to claim 1, characterized in that: In step S2, the dosage of tyrosine and the mixed enzyme preparation is 0.065-0.074 g / g of linen fabric and 0.23-0.45 g / g of linen fabric, respectively.
6. A linen fabric softening and finishing method according to claim 1, characterized in that: In step S2, the amount of 2,2,6,6-tetramethyl-1-piperidinyloxy free radical used is 0.05-0.08 g / g of linen fabric.
7. A linen fabric softening and finishing method according to claim 1, characterized in that: In step S2, the first stage reaction temperature is 30-37°C, and the reaction time is 12-24h.
8. A linen fabric softening and finishing method according to claim 1, characterized in that: In step S2, the second stage reaction temperature is 35-40°C, and the reaction time is 6-12h.