A catalyst for catalytic conversion of cellulose to prepare ethyl levulinate, and its preparation method and application
By using catalysts with phosphorus, tungsten and sulfonic acid groups in the cellulose depolymerization process, the corrosion and efficiency problems caused by the addition of acid are solved, and efficient and selective conversion of cellulose into ethyl levulinate is achieved. , suitable for industrial applications.
Patent Information
- Application Number
- CN202310364308.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-04-03
AI Technical Summary
During the depolymerization process of cellulose, the existing technology requires the addition of acid, which leads to corrosion, environmental pollution and equipment damage. Moreover, the conversion efficiency and selectivity are insufficient, making it difficult to achieve efficient conversion of cellulose to ethyl levulinate.
It uses a nitrogen-containing carbon-based carrier made of polyaniline as a carbon material precursor, and a catalyst loaded with phosphorus, tungsten and sulfonic acid groups. It is formed by combining citric acid gel with phosphorus and tungsten precursors, calcining and sulfonation. Efficient catalyst for the conversion of cellulose to ethyl levulinate in water-ethanol biphasic solvents.
Efficient conversion without adding acid is achieved, with 100% cellulose conversion rate and ethyl levulinate selectivity exceeding 80%. Each gram of cellulose can produce more than 400mg ethyl levulinate, with long catalyst life and low economic cost. Suitable for industrial applications.
Smart Images

Figure CN116408125B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a catalyst for catalytically converting cellulose to prepare ethyl levulinate, and a preparation method and application thereof. Background Art
[0002] Compared with fossil energy, biomass energy has the characteristics of less pollution, renewable, low cost, carbon neutrality, relatively short growth cycle and abundant raw materials. Among various biomass, cellulose is the most abundant. Efficient use of lignocellulosic biomass to produce biofuels is an effective way to solve the energy crisis and environmental pollution.
[0003] Cellulose is the most abundant component of biomass. In the past, the depolymerization process of cellulose often involves the addition of acid, which inevitably forms humus, an unwanted product, which affects the selectivity and yield of the target product, and also causes equipment corrosion and environmental problems. The subsequent separation also increases its cost. Therefore, it is necessary to develop a mild and efficient catalytic system to achieve efficient conversion of cellulose to ethyl levulinate. Summary of the invention
[0004] The main purpose of the present invention is to provide a catalyst for catalytically converting cellulose to ethyl levulinate, which does not require acid addition, has a high conversion rate and high selectivity for ethyl levulinate, and a preparation method and application thereof.
[0005] To achieve the above-mentioned purpose, the present invention provides a catalyst for catalytic conversion of cellulose to ethyl levulinate, comprising a carrier and an active component loaded on the carrier, wherein the carrier is a nitrogen-containing carbon-based carrier made with polyaniline as a carbon material precursor, and the active components are phosphorus, tungsten and sulfonic acid groups.
[0006] Furthermore, the content of phosphorus is 0.04-0.15wt%, the content of tungsten is 1-10wt%, and the content of sulfur is 1-5wt%.
[0007] The present invention also provides a method for preparing the catalyst for catalytic conversion of cellulose to ethyl levulinate, comprising the following steps:
[0008] S1, adding citric acid to deionized water, heating to form citric acid gel, dispersing polyaniline in deionized water to form a polyaniline solution, mixing the citric acid gel and the polyaniline solution, stirring, adding a phosphorus precursor salt and a tungsten precursor salt, stirring again, evaporating water, and finally drying to obtain a catalyst precursor;
[0009] S2. The catalyst precursor is placed in a nitrogen atmosphere for calcination treatment, and then sulfonated with concentrated sulfuric acid to obtain the catalyst for catalytic conversion of cellulose to ethyl levulinate.
[0010] Furthermore, in step S1, the mass ratio of citric acid to polyaniline is 1:1-2.
[0011] Furthermore, in step S1, the stirring treatment conditions for the two times are: temperature 20-60° C., and time 6-24 h.
[0012] Furthermore, the precursor salt of phosphorus and the precursor salt of tungsten are both phosphotungstic acid, or the precursor salt of phosphorus is diammonium hydrogen phosphate, and the precursor salt of tungsten is ammonium tungstate.
[0013] Furthermore, in step S1, the drying treatment conditions are: temperature 105° C., time 8 to 12 hours.
[0014] Furthermore, in step S2, the calcination treatment conditions are: heating to 600-800° C. at a heating rate of 2-6° C. / min and calcining for 4 hours in a nitrogen atmosphere.
[0015] Furthermore, in step S2, the sulfonation treatment conditions are: sulfonation reflux reaction with 98% concentrated sulfuric acid for 6 to 12 hours, sulfonation temperature of 120 to 180° C., and the volume mass ratio of concentrated sulfuric acid to calcined product is 10 to 20 mL: 1 g.
[0016] The invention also provides application of the catalyst in catalytic conversion of cellulose to prepare ethyl levulinate.
[0017] The present invention also provides a method for preparing ethyl levulinate by catalytic conversion of cellulose, comprising the following steps: taking cellulose as raw material, adding the above catalyst to carry out reaction, the reaction conditions are: catalyst dosage 0.10-0.25g, cellulose dosage 0.5g, reaction temperature 180-260°C, reaction time 1-5h, and the reaction solvent is a water-ethanol bicompatible agent.
[0018] The beneficial effects of the present invention are embodied in:
[0019] The catalyst of the present invention uses phosphorus, tungsten, and sulfonic acid groups as active components, which can enhance the ability of the catalyst to crack cellulose; phosphorus and metal tungsten form a transition metal interstitial compound structure, which not only causes an interfacial charge transfer mechanism on the catalyst surface, increasing the accessibility of metal tungsten to electron-rich groups, but also enhances the Lewis acid strength; at the same time, sulfonic acid groups are introduced on the carbon carrier to increase its Bronsted acid strength, thereby enhancing the catalyst's depolymerization ability. Compared with other carbon-based catalysts, the catalyst of the present invention can anchor the phosphorus and tungsten active components on the polyaniline carbon carrier by impregnating and complexing the polyaniline-citric acid colloid with phosphorus and tungsten precursors and then calcining in an inert gas atmosphere, thereby weakening the leaching of the active components and increasing the life of the catalyst. The calcined sample is treated with sulfonation to obtain the catalyst.
[0020] The catalyst of the present invention is applied to the field of catalytic conversion of cellulose to ethyl levulinate. In a water-ethanol biphasic solvent, a 100% conversion rate of cellulose, a selectivity of ethyl levulinate exceeding 80%, and production of more than 400 mg of ethyl levulinate per gram of cellulose can be achieved.
[0021] When the catalyst of the present invention is used to catalyze the conversion of cellulose to produce ethyl levulinate in a water-ethanol biphasic solvent, the complete conversion of cellulose can be achieved, the selectivity of ethyl levulinate in the liquid product exceeds 80%, and more than 400 mg of ethyl levulinate can be produced per gram of cellulose. The catalyst has the advantages of low economic cost, low metal loading, and high cycle number, can improve the depolymerization ability of the catalyst on cellulose, meet the industrialization requirements of catalyzing the conversion of cellulose to produce ethyl levulinate, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a high-resolution image of catalyst #1 prepared in Example 1 of the present invention;
[0023] Figure 2 This is an EDS layered image of catalyst #1 prepared in Example 1 of the present invention;
[0024] Figure 3 This is a high-resolution image of the 3# catalyst prepared in Example 3 of the present invention;
[0025] Figure 4 This is an EDS layered image of the 3# catalyst prepared in Example 3 of the present invention;
[0026] Figure 5 XRD spectra of catalyst #1 and catalyst #3 prepared in the examples of the present invention;
[0027] Figure 6 FTIR spectra of catalyst #1 and catalyst #3 prepared in the examples of the present invention;
[0028] Figure 7 NH3-TPD spectra of catalyst #1 and catalyst #3 prepared in the examples of the present invention;
[0029] Figure 8 The Raman spectra of catalyst #1 and catalyst #3 prepared in the examples of the present invention are shown. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Unless otherwise specified, all raw materials used in the following examples are commercially available products known in the art.
[0032] Example 1
[0033] Preparation of a catalyst for catalytic conversion of cellulose to ethyl levulinate, the preparation method is as follows:
[0034] S1. Weigh 5g of citric acid and disperse it evenly in 10mL of deionized water, heat it at 120℃ to form sol solution I, weigh 5g of polyaniline and disperse it in 40mL of deionized water to form solution II. Slowly add solution II to solution I to form solution III, and stir at 30℃ for 12h. Weigh 0.55g of phosphotungstic acid and slowly add it to solution III, stir at 30℃ for 12h, and then evaporate to dryness at 90℃, then put the obtained product in an oven and dry it for 12h to obtain the phosphorus and tungsten precursors loaded on the carbon material.
[0035] S2. After sufficient grinding, the temperature was raised to 700°C at a heating rate of 4°C / min in a nitrogen atmosphere and maintained for 4 hours to obtain the phosphorus and tungsten samples supported by the carbon material. Subsequently, 3.7g of the phosphorus and tungsten samples supported by the carbon material and 50mL of concentrated sulfuric acid with a mass fraction of 98% were taken in a 100mL Teflon liner, sulfonated and refluxed at 150°C for 6 hours, and then cooled to room temperature, filtered and washed with deionized water until neutral, and dried for 12 hours to obtain the catalyst for catalytic conversion of cellulose to ethyl levulinate, numbered 1#.
[0036] Example 2
[0037] Preparation of a catalyst for catalytic conversion of cellulose to ethyl levulinate, the preparation method is as follows:
[0038] S1. Weigh 4.5g of citric acid and disperse it evenly in 20mL of deionized water, heat it at 120℃ to form sol solution I, weigh 4.5g of polyaniline and disperse it in 30mL of deionized water to form solution II. Slowly add solution II to solution I to form solution III, and stir at 25℃ for 6h. Weigh 0.50g of phosphotungstic acid and slowly add it to solution III, stir at 25℃ for 12h, and then evaporate to dryness at 90℃, then put the obtained product in an oven and dry it for 12h to obtain the phosphorus and tungsten precursors supported by the carbon material.
[0039] S2. After sufficient grinding, the temperature was raised to 600°C at a heating rate of 5°C / min in a nitrogen atmosphere and maintained for 4 hours to obtain the phosphorus and tungsten samples supported by the carbon material. Subsequently, 4.0g of the phosphorus and tungsten samples supported by the carbon material and 60mL of concentrated sulfuric acid with a mass fraction of 98% were taken in a 100mL Teflon liner, sulfonated and refluxed at 120°C for 8 hours, and then cooled to room temperature, filtered and washed with deionized water until neutral, and dried for 12 hours to obtain the catalyst for catalytic conversion of cellulose to ethyl levulinate, numbered 2#.
[0040] Example 3
[0041] Preparation of a catalyst for catalytic conversion of cellulose to ethyl levulinate, the preparation method is as follows:
[0042] S1. Weigh 9g of citric acid and disperse it evenly in 20mL of deionized water, heat it at 120℃ to form sol solution I, weigh 4.5g of polyaniline and disperse it in 30mL of deionized water to form solution II. Slowly add solution II to solution I to form solution III, and stir at 50℃ for 12h. Weigh 0.50g of ammonium tungstate and 0.05g of diammonium hydrogen phosphate and slowly add them to solution III, stir at 50℃ for 12h, and then evaporate to dryness at 90℃, then put the obtained product in an oven and dry it for 12h to obtain phosphorus and tungsten precursors loaded on carbon materials.
[0043] S2. After sufficient grinding, the temperature was raised to 750°C at a heating rate of 6°C / min in a nitrogen atmosphere and maintained for 4 hours to obtain the phosphorus and tungsten samples supported by the carbon material. Subsequently, 3.5 g of the phosphorus and tungsten samples supported by the carbon material and 70 mL of concentrated sulfuric acid with a mass fraction of 98% were taken in a 100 mL Teflon liner, sulfonated and refluxed at 160°C for 10 hours, and then cooled to room temperature, filtered and washed with deionized water until neutral, and dried for 12 hours to obtain the catalytic conversion of cellulose to ethyl levulinate catalyst, No. 3#.
[0044] Example 4
[0045] Preparation of a catalyst for catalytic conversion of cellulose to ethyl levulinate, the preparation method is as follows:
[0046] S1. Weigh 10g of citric acid and disperse it evenly in 30mL of deionized water, heat it at 120℃ to form sol solution I, weigh 6g of polyaniline and disperse it in 30mL of deionized water to form solution II. Slowly add solution II into solution I to form solution III, and stir at 60℃ for 12h. Weigh 0.68g of ammonium tungstate and 0.07g of diammonium hydrogen phosphate and slowly add them into solution III, stir at 60℃ for 24h, and then evaporate to dryness at 90℃, then put the obtained product in an oven and dry it for 12h to obtain phosphorus and tungsten precursors loaded on carbon materials.
[0047] S2. After sufficient grinding, the temperature was raised to 700°C at a heating rate of 6°C / min in a nitrogen atmosphere and maintained for 4 hours to obtain the phosphorus and tungsten samples supported by the carbon material. Subsequently, 5.0 g of the phosphorus and tungsten samples supported by the carbon material and 75 mL of concentrated sulfuric acid with a mass fraction of 98% were taken in a 100 mL Teflon liner, sulfonated and refluxed at 180°C for 12 hours, and then cooled to room temperature, filtered and washed with deionized water until neutral, and dried for 12 hours to obtain the catalyst for catalytic conversion of cellulose to ethyl levulinate, numbered 4#.
[0048] Example 5
[0049] Preparation of a catalyst for catalytic conversion of cellulose to ethyl levulinate, the preparation method is as follows:
[0050] S1. Weigh 10g of citric acid and disperse it evenly in 30mL of deionized water, heat it at 120℃ to form sol solution I, weigh 5g of polyaniline and disperse it in 30mL of deionized water to form solution II. Slowly add solution II into solution I to form solution III, and stir at 60℃ for 24h. Weigh 0.58g of ammonium tungstate and 0.09g of diammonium hydrogen phosphate and slowly add them into solution III, stir at 60℃ for 24h, and then evaporate to dryness at 90℃, then put the obtained product in an oven and dry it for 12h to obtain the phosphorus and tungsten precursors loaded on the carbon material.
[0051] S2. After fully grinding, the temperature was raised to 700°C at a heating rate of 4°C / min in a nitrogen atmosphere and maintained for 4 hours to obtain the phosphorus and tungsten samples supported by the carbon material. Subsequently, 5.0 g of the phosphorus and tungsten samples supported by the carbon material and 75 mL of concentrated sulfuric acid with a mass fraction of 98% were taken in a 100 mL Teflon liner, sulfonated and refluxed at 150°C for 6 hours, and then cooled to room temperature, filtered and washed with deionized water until neutral, and dried for 12 hours to obtain the catalyst for catalytic conversion of cellulose to ethyl levulinate, No. 5#
[0052] Example 6
[0053] Structure determination of the catalyst
[0054] The structural characteristics of the catalysts prepared in the above examples were studied by various characterizations, and the results are as follows:
[0055] The contents of phosphorus (P), tungsten (W) and sulfur (S) in the catalysts and raw material polyaniline prepared in the above examples were analyzed by ICP analysis. The results are shown in Table 1 below.
[0056] Table 1 Catalyst composition
[0057]
[0058]
[0059] ICP results confirmed the presence of P, W, and S in the catalyst. The image of the catalyst is shown in Figures 1 to 4 .
[0060] See also Figure 5 , polyaniline has two weak characteristic peaks at 2θ=20.2°(020) and 2θ=25.5°(200), which are broad diffraction peaks of the amorphous non-crystalline nature of polyaniline. After the catalyst is sulfonated, the relevant characteristic peaks disappear because the concentrated sulfuric acid washes away a large number of oxide clusters formed after the load calcination, while the retained P and W species are difficult to form a highly crystalline structure due to their low content and high dispersion.
[0061] See also Figure 6 , for polyaniline, 1575cm -1 and 1484cm -1 The characteristic peaks correspond to the C=C stretching vibrations of the quinone ring and the benzene ring, appearing at 1304 cm -1 The absorption peaks are from the stretching vibration of CN in the secondary aromatic amine, 1142-1114 cm -1 Corresponds to CH bending vibration in the plane of the aromatic ring. 814cm -1 It is the CH bending vibration of the aromatic ring in the backbone of polyaniline. For catalysts 1# and 3#, after sulfonation with concentrated sulfuric acid, 1032 and 1174 cm -1 The peak intensity at 1032cm -1 Related to the symmetric stretching vibration of (O=S=O bond), 1174cm -1 This corresponds to the antisymmetric vibration of the sulfonic acid group. The combination of the two indicates the successful introduction of the sulfonic acid group.
[0062] See also Figure 7 It is not difficult to see that the amount of weak acid and medium-strong acid in catalysts 1# and 3# are significantly increased compared with polyaniline, which is very beneficial to cellulose.
[0063] See also Figure 8 The Raman spectrum results are shown in the figure. -1 and 1590cm -1 The two specific diffraction peaks correspond to the D band and the G band. The D band is generally considered to be disordered, edge, and sp 3 hybridized carbon atoms. The G band is related to sp 2 Hybridized carbon atom E 2g The intensity ratio of the D band and the G band (I D :I G ) is used to measure the degree of graphitization and disorder of the material. The existence of D and G bands proves that the material we prepared is a carbonized material with polycyclic aromatic carbon sheets. The results are consistent with XRD.
[0064] Example 7
[0065] Performance test of catalyst for converting cellulose into ethyl levulinate
[0066] 0.10-0.25g of the above 1#-5# catalysts were taken to perform performance tests in a micro high temperature and high pressure reactor, wherein the amount of cellulose was 0.5g, the reaction temperature was 180-260°C, the reaction time was 1-5h, and the reaction solvent was a water-ethanol biphasic solvent (water: 10mL, ethanol: 20mL). Specific reaction conditions and results are shown in Table 2.
[0067] Table 2 Performance test of catalytic conversion of cellulose into ethyl levulinate
[0068]
[0069] From the above results, it can be concluded that the catalyst of the present invention can achieve full conversion of cellulose under the condition of water-ethanol dual compatibilizer, the selectivity of ethyl levulinate in the liquid product exceeds 80%, more than 400 mg of ethyl levulinate can be produced per gram of cellulose, and the service life is more than 15 times.
[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A catalyst for catalytic conversion of cellulose to ethyl levulinate, It is characterized in that It comprises a carrier and an active component loaded on the carrier, wherein the carrier is a nitrogen-containing carbon-based carrier made of polyaniline as a carbon material precursor, and the active component is phosphorus, tungsten and sulfonic acid groups; The method for preparing the catalyst for catalytic conversion of cellulose to ethyl levulinate comprises the following steps: S1, adding citric acid to deionized water, heating to form citric acid gel, dispersing polyaniline in deionized water to form a polyaniline solution, mixing the citric acid gel and the polyaniline solution, stirring, adding a phosphorus precursor salt and a tungsten precursor salt, stirring again, evaporating water, and finally drying to obtain a catalyst precursor; S2. The catalyst precursor is placed in a nitrogen atmosphere for calcination treatment, and then sulfonated with concentrated sulfuric acid to obtain the catalyst for catalytic conversion of cellulose to ethyl levulinate.
2. The catalyst for catalytic conversion of cellulose to ethyl levulinate according to claim 1, It is characterized in that The content of phosphorus is 0.04-0.15wt%, the content of tungsten is 1-10wt%, and the content of sulfur is 1-5wt%.
3. The catalyst for catalytic conversion of cellulose to ethyl levulinate according to claim 1, It is characterized in that In step S1, the mass ratio of citric acid to polyaniline is 1:1-2.
4. The catalyst for catalytic conversion of cellulose to ethyl levulinate according to claim 1, It is characterized in that In step S1, the stirring treatment conditions for the two times are: temperature 20-60° C., and time 6-24 h.
5. The catalyst for catalytic conversion of cellulose to ethyl levulinate according to claim 1, It is characterized in that In step S1, the drying treatment conditions are: temperature 105° C., time 8 to 12 hours.
6. The catalyst for catalytic conversion of cellulose to ethyl levulinate according to claim 1, It is characterized in that In step S2, the calcination treatment conditions are: heating to 600-800°C at a heating rate of 2-6°C / min and calcining for 4 hours in a nitrogen atmosphere.
7. The catalyst for catalytic conversion of cellulose to ethyl levulinate according to claim 1, It is characterized in that In step S2, the sulfonation treatment conditions are: sulfonation reflux reaction with 98% concentrated sulfuric acid for 6 to 12 hours, sulfonation temperature of 120 to 180° C., and the volume mass ratio of concentrated sulfuric acid to calcined product is 10 to 20 mL: 1 g.
8. Use of the catalyst according to any one of claims 1 to 7 in catalytic conversion of cellulose to produce ethyl levulinate.
9. A method for preparing ethyl levulinate by catalytic conversion of cellulose, It is characterized in that The following steps are involved: Cellulose is used as a raw material, and a catalyst as described in any one of claims 1 to 7 is added to react. The reaction conditions are: 0.10-0.25 g of catalyst, 0.5 g of cellulose, a reaction temperature of 180-260° C., a reaction time of 1-5 h, and a reaction solvent of a water-ethanol bicompatible agent.