A diesel hydrogenation reforming catalyst and its preparation method and application
By using Group VIB and Group VIII active metals, mesoporous amorphous silicon aluminum and alumina and composite mesoporous molecular sieve in diesel hydrogenation modification catalysts, the mesoporous structure and acid properties of the catalyst are optimized, and the octanoplasmic properties of the high aromatic diesel is solved. The problems of low alkylene number and high sulfur content have achieved the effect of efficient production of high octane gasoline and ultra-low sulfur diesel.
Patent Information
- Application Number
- CN202111681472.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-12-31
AI Technical Summary
When the existing diesel hydrogenation modification catalysts treat high aromatic inferior diesel, the product has low octane number and high sulfur content, which cannot meet the needs of producing high octane gasoline and ultra-low sulfur diesel.
Compounds containing 10 to 30 wt% of Group VIB active metal, 1 to 5 wt% of Group VIII active metal, 15 to 40 wt% of Mesoporous amorphous silicon aluminum, 5 to 30 wt% of Mesoporous alumina and 20 to 25 wt% were used. The catalyst of mesoporous molecular sieve improves the hydrogenation and modification performance of the catalyst by optimizing the mesoporous structure and acid properties.
In inferior high aromatic diesel, it improves naphtha yield and diesel hexadecane number, reduces hydrogen consumption, and produces high octane gasoline and ultra-low sulfur diesel, helping to reduce the diesel-to-gasoline ratio, suitable for refining and chemical integration Industrial applications of enterprises.
Smart Images

Figure BDA0003453531870000131 
Figure BDA0003453531870000141 
Figure BDA0003453531870000151
Abstract
Description
Technical Field
[0001] The invention relates to the field of diesel fuel hydro-modification, and in particular to a diesel fuel hydro-modification catalyst and a preparation method and application thereof. Background Art
[0002] Catalytic cracking is one of the main means of heavy oil processing. In my country, the catalytic cracking processing capacity accounts for about one-third of the crude oil primary processing capacity, resulting in catalytic cracking gasoline accounting for more than 75% and catalytic diesel accounting for more than 30% in the composition of gasoline and diesel products. Catalytic diesel contains more heteroatom compounds, aromatics and olefins, poor stability and low cetane number. With the increasing deterioration of crude oil quality, and many companies have modified or increased the severity of catalytic cracking units in order to improve gasoline quality or increase propylene production, resulting in a further deterioration of the quality of catalytic diesel. The aromatic content of catalytic diesel produced by some companies even reaches more than 80%, and the cetane number is usually less than 20. Due to increasingly stringent environmental regulations, this part of catalytic diesel with special properties is increasingly difficult to meet market demand through traditional processing methods. Traditional catalytic diesel processing methods mainly include hydrofining and hydrocracking. Hydrofining can reduce the sulfur and nitrogen content of the product, but due to the limitation of aromatic saturation thermodynamic equilibrium, the cetane number is limited. Hydrocracking can partially crack diesel fractions into naphtha and light components, but the gasoline produced by cracking is high-cycloalkane, low-octane naphtha, which must be reformed to reach the octane number required for product blending, thereby increasing processing costs.
[0003] With the decline in demand for oil products, my country's diesel consumption has basically reached its peak, and diesel consumption will decrease year by year. In 2020, the total apparent consumption of diesel was 140.48 million tons, down 3.7% year-on-year. It is expected that by 2025, the diesel-to-gasoline ratio will drop to 0.75. Therefore, refining companies are in urgent need of technologies to reduce the diesel-to-gasoline ratio. Therefore, in response to the high aromatic content of catalytic diesel and the technical needs of refining companies to reduce the diesel-to-gasoline ratio, various research institutions have begun to study the technology of producing high-octane gasoline using catalytic diesel as raw material.
[0004] CN106140279 B discloses a method for preparing a diesel hydrogenation reforming catalyst. The method includes the preparation of a carrier and the loading of a hydrogenation active metal component, wherein the carrier is prepared by mixing β molecular sieve, macroporous alumina and a binder, and the reforming catalyst is suitable for inferior diesel raw materials. Under medium pressure conditions of 10MPa, the hydrogen-oil ratio is 800:1, and the air velocity is 1.5h -1, reaction temperature 370 ℃, treatment of inferior catalytic diesel, its naphtha yield is about 2wt%, aromatics potential content can reach 53-54wt%, diesel yield is greater than 96wt%, cetane number is increased by about 30%. This method has the disadvantages of high reaction temperature and low naphtha yield, and cannot meet the technical requirements of reducing diesel-to-gasoline ratio and transformation of oil refining to chemical industry.
[0005] CN101619235 B discloses a catalyst for hydrogenation reforming of inferior diesel. The catalyst contains a carrier containing silicon oxide-alumina, aluminum oxide, and Y molecular sieve and a hydrogenation active metal component loaded on the carrier. The catalyst is heated to 360°C, 6.4 MPa, and 1.3 h / min at a reaction temperature of 1.30 °C. -1 Under the process conditions of a hydrogen-to-oil ratio of 600:1, the desulfurization rate is greater than 95wt%, and the denitrification rate is greater than 98wt%. It has high desulfurization and denitrification activity and diesel yield, and the diesel cetane number is increased by about 10 units. This technology can meet the production needs of clean oil products, but cannot meet the technical needs of reducing the diesel-to-gasoline ratio and the transformation of refining to chemical industry.
[0006] CN101463271A discloses a catalyst for hydrogenation and reforming of inferior diesel and a preparation method thereof. The method mainly uses silicon oxide-alumina, alumina and / or alumina precursor and Y-type molecular sieve to mix, shape and roast, and then introduces an effective amount of hydrogenation metal into the shape. The catalyst has high desulfurization and denitrification activity, but the yield of the product is low.
[0007] CN101724454 discloses a hydrocracking method for producing high-octane gasoline. The method adopts a series process flow, the raw material is a diesel fraction with an aromatic mass fraction of more than 70%, the raw material is treated with hydrorefining, and then directly hydrocracking. The catalyst used in this technology is a light oil-type hydrocracking catalyst, and the Y molecular sieve used is an SSY molecular sieve or a Y molecular sieve further modified by SSY. The unconverted diesel fraction adopts a partial circulation operation mode, the single-pass conversion rate is controlled to 30-60%, the total conversion rate is controlled to 50-95%, the gasoline yield is 51.8-58.1wt%, the octane number RON is 92.7-93.9, the reaction temperature is 406-415°C, and the product yield is 91.6-92.0%. Although this method can produce gasoline products with an octane number RON higher than 90, it has the disadvantages of too high a reaction temperature and too low a liquid product yield, and cannot meet the needs of long-term operation and maximum efficiency of the refinery.
[0008] CN101987971 discloses a method for producing high-octane gasoline from inferior diesel. The raw material of the method is a diesel fraction with a total aromatic mass fraction of more than 65wt% and a content of dicyclic and higher aromatics higher than 40wt%. The raw material is directly hydrocracking after being treated with hydrofining. The method requires controlling the saturation depth of aromatics in the hydrofining process. Compared with the diesel raw material, the saturation rate of dicyclic and higher aromatics in the refined oil is more than 50wt%, and the content of monocyclic aromatics is increased to more than 40wt%. The loading ratio of the hydrofining catalyst and the hydrocracking catalyst is between 5:1 and 1:5, which is determined according to the nitrogen content of the diesel raw material oil. The gasoline yield of the method is 38.8-49.0wt%, the octane number RON is 89.4-92.0, the reaction temperature is 390-410℃, the diesel cetane number is increased by 10.0-10.8 units, and the sulfur content is less than 50μ / g. Although this method can also produce gasoline products with an octane number RON higher than 90, it also has disadvantages such as a relatively high reaction temperature, a small increase in the cetane number of the diesel product, and a relatively high sulfur content.
[0009] UOP announced a new LCO upgrading technology with high added value and high return on investment at the 2005 NPRA Annual Meeting (AM-05-53), the LCO UnicrackingTM process, which converts LCO into ultra-low sulfur diesel and high-octane gasoline that can be directly blended economically and effectively. The technology is characterized by selective hydrogenation, focusing on the hydrodesulfurization of diesel products, while reducing naphtha aromatic saturation to a minimum. This technology uses a highly active HC190 catalyst to process LCO feedstock with an aromatic content of 65-80wt%. By optimizing the operating conditions, the heavy naphtha yield is 35-37wt%, and the octane number (RON) is 90-95; the diesel yield is 46-51wt%, and the diesel cetane number increases by 6-8 units. This method can produce gasoline products with an octane number RON higher than 90, but there is also a disadvantage that the cetane number of the diesel product is not increased much.
[0010] US6241876B1 and US6500329B2 disclose a catalytic diesel hydrogenation reforming technology. Their common feature is that they use a two-stage countercurrent process to treat catalytic diesel. The first stage is hydrogenation desulfurization, nitrogen and other impurities, and the second stage uses a precious metal catalyst containing a Y-type molecular sieve for deep hydrogenation and dearomatization, which can greatly improve the cetane number of the diesel product. Their disadvantages are that the operating conditions are harsh, and a countercurrent process and precious metal catalysts are required. Therefore, the operation and investment costs are very high, and it is difficult to apply them industrially. Summary of the invention
[0011] Based on the above, the purpose of the present invention is to provide a diesel hydro-modification catalyst and its preparation method and application. The diesel hydro-modification catalyst is used for the hydro-modification of inferior high-aromatic diesel feedstock, which can overcome the defects of low octane number and high sulfur content of the product when the existing hydrogenation catalyst is used for the modification of high-aromatic inferior diesel, and can produce high-octane gasoline and ultra-low sulfur diesel.
[0012] To this end, the present invention provides a diesel hydrogenation reforming catalyst, which comprises, based on the total weight of the catalyst: 10-30wt% of Group VIB active metals calculated by weight of oxides, 1-5wt% of Group VIII active metals calculated by weight of oxides, 15-40wt% of mesoporous amorphous silica-alumina, 5-30wt% of mesoporous alumina, and 20-25wt% of a composite mesoporous molecular sieve; the composite mesoporous molecular sieve is composed of USY molecular sieve and MSU-1 molecular sieve; the mesoporous amorphous silica-alumina refers to amorphous silica-alumina in which pores with a pore size of 2-50nm account for more than 85%, and the mesoporous alumina refers to alumina in which pores with a pore size of 2-50nm account for more than 85%.
[0013] Specifically, the hydrogenation reforming catalyst of the present invention uses 15-40wt% mesoporous amorphous silica-alumina and 5-30wt% mesoporous alumina as carriers, which increases the mesoporous structure of the catalyst, and optimizes the acid properties of the catalyst by using 20-25wt% composite mesoporous molecular sieve as the acidic component.
[0014] The diesel hydro-reforming catalyst of the present invention is preferably that the VIB group active metal is Mo and / or W, and the VIII group active metal is Co and / or Ni; the content of the VIB group active metal is 10-20wt%, and the content of the VIII group active metal is 1-3wt%.
[0015] The diesel hydro-reforming catalyst of the present invention is preferably that in the composite mesoporous molecular sieve, the mass ratio of USY molecular sieve to MSU-1 molecular sieve is 80:20 to 40:60, and the mass ratio of USY molecular sieve to MSU-1 molecular sieve can be 80:20, 70:30, 60:40, 50:50 or 40:60, and 60:40 is more preferred.
[0016] The diesel hydro-reforming catalyst of the present invention is preferably a method for preparing the composite mesoporous molecular sieve comprising the following steps: adding USY molecular sieve and MSU-1 molecular sieve to an alkaline solution, stirring, standing, filtering, washing, drying and calcining to prepare the composite mesoporous molecular sieve; further preferably, stirring in an alkaline solution for 2 to 6 hours, standing for 0.5 to 3 hours, filtering, washing, drying at 100 to 150° C. for 2 to 6 hours, and calcining at 500 to 550° C. for 4 to 6 hours.
[0017] The diesel hydro-reforming catalyst of the present invention is preferably such that the alkaline solution is selected from the group consisting of potassium hydroxide solution, hexamethylenediamine solution, ammonium bicarbonate solution and ammonia water.
[0018] The diesel hydro-reforming catalyst of the present invention is preferably characterized in that the volume of the pores with a pore diameter of 2-50 nm in the mesoporous amorphous silica-alumina is 1.20-1.90 mL / g, and the specific surface area is 380-550 m 2 / g, the bulk density is 0.15-0.40g / mL; the volume of the pores with a pore diameter of 2-50nm in the mesoporous alumina is 0.80-1.60mL / g, and the specific surface area is 220-380m 2 / g, and the bulk density is 0.35-0.55g / mL.
[0019] To this end, the present invention also provides a method for preparing the above-mentioned diesel hydro-reforming catalyst, comprising the following steps:
[0020] (1) mixing mesoporous amorphous silica-alumina, mesoporous alumina, composite mesoporous molecular sieve, a binder and an extrusion aid, extruding into strips, and drying and calcining the obtained shaped product to prepare a carrier; the carrier is preferably in the shape of a cylindrical or shaped strip, and the shaped strip is in the shape of a three-leaf clover or a four-leaf clover;
[0021] (2) The carrier is impregnated with an impregnation solution containing active metals, dried and calcined to obtain a catalyst.
[0022] The catalyst of the present invention is formed and loaded with metal mainly by extrusion followed by metal impregnation, and various conventional techniques such as tableting or spheroidization can also be used. The loading of metal can be carried out by coprecipitation, kneading and impregnation.
[0023] The preparation method of the diesel hydro-reforming catalyst of the present invention is preferably that the binder is made of an inorganic acid and / or an organic acid, the inorganic acid is selected from one or two of hydrochloric acid, nitric acid, phosphoric acid and sulfuric acid, and the organic acid is selected from one or two of formic acid, acetic acid, citric acid and tartaric acid; the extrusion aid is selected from one or more of starch, sesbania powder, polyethanol and methyl cellulose, and its content is 1.0 to 5.0 wt%, and more preferably 2 to 4 wt%.
[0024] To this end, the present invention also provides a diesel hydrogenation reforming method, using the above-mentioned diesel hydrogenation reforming catalyst as a catalyst, the diesel is a low-quality high-aromatic diesel fraction with a distillation range of 150 to 420° C., preferably a distillation range of 150 to 390° C., and the total aromatic content is preferably greater than 60wt%, and the low-quality high-aromatic diesel fraction includes at least one of catalytic cracking diesel, coal tar, and coal direct liquefaction oil.
[0025] The diesel hydro-reforming method of the present invention is preferably that the diesel hydro-reforming catalyst needs to be pre-sulfurized when treating low-quality high-aromatic diesel feedstock, and the pre-sulfurization conditions are: reaction temperature 200-400°C, reaction pressure 6-12MPa, hydrogen-oil volume ratio 350-800:1, volume space velocity 1.0-3.0h -1 ; The reaction conditions of hydrogenation reforming are: reaction temperature 320~420℃, pressure 6~12MPa, hydrogen-oil volume ratio 350~800:1, volume space velocity 0.5~3.0h -1 .
[0026] The diesel hydro-reforming catalyst provided by the present invention is particularly suitable for the process of hydro-reforming inferior diesel to produce high-octane gasoline and ultra-low sulfur diesel. In addition, it is preferably operated under the conditions of a series hydrogenation process, and the hydro-refining catalyst is first used to remove most of the nitrogen compounds in the raw materials and partially saturate the polycyclic aromatic hydrocarbons, thereby ensuring that the activity of the hydro-reforming catalyst is fully exerted.
[0027] The advantages of the present invention are: by optimizing the composition of the catalyst carrier material, amorphous silicon aluminum and aluminum oxide with high mesopore content are used as the main carrier, and the (USY+MSU-1) composite mesoporous molecular sieve is used as the acidic component. Therefore, in the process of hydrogenation conversion of inferior high-aromatic diesel, the catalyst of the present invention has a low bulk density, a high naphtha yield, and a high aromatic potential; and the obtained diesel cetane number has a high improvement value, that is, when the catalyst treats inferior diesel raw materials, it has excellent hydrogenation and upgrading performance, and can produce high-quality diesel blending components while producing more high-aromatic potential naphtha, which is helpful to reduce the diesel-to-gasoline ratio; and the hydrogen consumption is less than 1.5wt%. DETAILED DESCRIPTION
[0028] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments that do not specify specific conditions are usually based on conventional conditions. The technical solution of the present invention is described in detail below through specific embodiments.
[0029] The diesel hydrogenation reforming catalyst provided by the present invention comprises, based on the total weight of the catalyst, 10-30wt% of Group VIB active metals calculated by weight of oxides, 1-5wt% of Group VIII active metals calculated by weight of oxides, 15-40wt% of mesoporous amorphous silica-alumina, 5-30wt% of mesoporous alumina, and 20-25wt% of a composite mesoporous molecular sieve; the composite mesoporous molecular sieve is composed of USY molecular sieve and MSU-1 molecular sieve; the mesoporous amorphous silica-alumina refers to amorphous silica-alumina in which pores with a pore size of 2-50nm account for more than 85%, and the mesoporous alumina refers to alumina in which pores with a pore size of 2-50nm account for more than 85%.
[0030] Specifically, the hydrogenation reforming catalyst of the present invention uses 15-40wt% mesoporous amorphous silica-alumina and 5-30wt% mesoporous alumina as carriers, which increases the mesoporous structure of the catalyst, and optimizes the acid properties of the catalyst by using 20-25wt% composite mesoporous molecular sieve as the acidic component.
[0031] Specifically, the properties of the mesoporous amorphous silica-alumina and mesoporous alumina used in some embodiments are shown in Table 2.
[0032] Table 2 Properties of mesoporous amorphous silica-alumina and mesoporous alumina
[0033] project Highly mesoporous amorphous silicon-alumina Highly mesoporous alumina Pore volume, mL / g 2-10nm 0.50-0.80 0.20-0.50 10-20nm 0.35-0.65 0.45-0.75 20-50nm 0.15-0.35 0.10-0.30 Total mesopore (2-50nm) volume, mL / g 1.20-1.90 0.80-1.60 <![CDATA[Specific surface area, m 2 / g]]> 380-550 220-380 Bulk density, g / mL 0.15-0.40 0.35-0.55
[0034] In some embodiments, preferably, the Group VIB active metal is Mo and / or W, and the Group VIII active metal is Co and / or Ni; the content of the Group VIB active metal is 10-20wt%, and the content of the Group VIII active metal is 1-3wt%.
[0035] In some embodiments, preferably, in the composite mesoporous molecular sieve, the mass ratio of USY molecular sieve to MSU-1 molecular sieve is 80:20 to 40:60, and the mass ratio of USY molecular sieve to MSU-1 molecular sieve can be 80:20, 70:30, 60:40, 50:50 or 40:60, and 60:40 is further preferred.
[0036] In some embodiments, preferably, the preparation method of the composite mesoporous molecular sieve comprises the following steps: adding USY molecular sieve and MSU-1 molecular sieve to an alkaline solution, stirring, standing, filtering, washing, drying, and calcining to prepare a composite mesoporous molecular sieve; further preferably, fully stirring in an alkaline solution for 2 to 6 hours, standing for 0.5 to 3 hours, filtering, washing, drying at 100 to 150°C for 2 to 6 hours, and calcining at 500 to 550°C for 4 to 6 hours.
[0037] The properties of the composite mesoporous molecular sieve prepared by the above method are shown in Table 1.
[0038] Table 1 Properties of the mesoporous molecular sieve used in the present invention and the prepared composite molecular sieve
[0039] project USY molecular sieve MSU-1 molecular sieve (USY+MSU-1) composite mesoporous molecular sieve B acid content, μmole / g 10-90 - 5-80 Silicon to aluminum ratio 20-60 - 30-80 <![CDATA[Specific surface area, m 2 / g]]> 500-900 500-900 500-900 Mesopore volume, mL / g 0.30-0.40 0.30-0.90 0.30-0.80 Total pore volume, mL / g 0.55-0.70 0.35-0.10 0.45-0.90
[0040] In some embodiments, preferably, the alkaline solution is selected from potassium hydroxide solution, hexamethylenediamine solution, ammonium bicarbonate solution, and ammonia water.
[0041] In some embodiments, preferably, the volume of the pores with a pore size of 2-50 nm in the mesoporous amorphous silica-alumina is 1.20-1.90 mL / g, and the specific surface area is 380-550 m 2 / g, the bulk density is 0.15-0.40g / mL; the volume of the pores with a pore diameter of 2-50nm in the mesoporous alumina is 0.80-1.60mL / g, and the specific surface area is 220-380m 2 / g, and the bulk density is 0.35-0.55g / mL.
[0042] The preparation method of the diesel hydro-reforming catalyst provided by the present invention comprises the following steps:
[0043] (1) mixing mesoporous amorphous silica-alumina, mesoporous alumina, composite mesoporous molecular sieve, a binder and an extrusion aid, extruding into strips, and drying and calcining the obtained shaped product to prepare a carrier; the carrier is preferably in the shape of a cylindrical or shaped strip, and the shaped strip is in the shape of a three-leaf clover or a four-leaf clover;
[0044] (2) The carrier is impregnated with an impregnation solution containing active metals, dried and calcined to obtain a catalyst.
[0045] The catalyst of the present invention is formed and loaded with metal mainly by extrusion followed by metal impregnation, and various conventional techniques such as tableting or spheroidization can also be used. The loading of metal can be carried out by coprecipitation, kneading and impregnation.
[0046] In some embodiments, preferably, the adhesive is made of an inorganic acid and / or an organic acid, the inorganic acid is selected from one or two of hydrochloric acid, nitric acid, phosphoric acid and sulfuric acid, and the organic acid is selected from one or two of formic acid, acetic acid, citric acid and tartaric acid; the extrusion aid is selected from one or more of starch, sesbania powder, polyethanol and methyl cellulose, and its content is 1.0 to 5.0 wt%, and more preferably 2 to 4 wt%.
[0047] The diesel hydro-reforming method provided by the present invention uses the above-mentioned diesel hydro-reforming catalyst as a catalyst, the diesel is an inferior high-aromatic diesel fraction with a distillation range of 150 to 420° C., preferably a distillation range of 150 to 390° C., and the total aromatic content is preferably greater than 60wt%. The inferior high-aromatic diesel fraction includes at least one of catalytic cracking diesel, coal tar, and coal direct liquefaction oil.
[0048] In some embodiments, it is preferred that the diesel hydro-reforming catalyst needs to be pre-sulfurized when treating low-quality high-aromatic diesel feedstock, and the pre-sulfurization conditions are: reaction temperature 200-400°C, reaction pressure 6-12MPa, hydrogen-oil volume ratio 350-800:1, volume space velocity 1.0-3.0h -1 ; The reaction conditions of hydrogenation reforming are: reaction temperature 320~420℃, pressure 6~12MPa, hydrogen-oil volume ratio 350~800:1, volume space velocity 0.5~3.0h -1 .
[0049] The diesel hydro-reforming catalyst provided by the present invention is particularly suitable for the process of hydro-reforming inferior diesel to produce high-octane gasoline and ultra-low sulfur diesel. In addition, it is preferably operated under the conditions of a series hydrogenation process, and the hydro-refining catalyst is first used to remove most of the nitrogen compounds in the raw materials and partially saturate the polycyclic aromatic hydrocarbons, thereby ensuring that the activity of the hydro-reforming catalyst is fully exerted.
[0050] Preparation of composite mesoporous molecular sieves
[0051] The preparation method of the composite mesoporous molecular sieve in the following embodiment includes the following steps: adding USY molecular sieve and MSU-1 molecular sieve to an alkaline solution, stirring for 4 hours, standing for 2 hours, filtering, washing with deionized water, drying at 120°C for 4 hours, and calcining at 500°C for 4 hours to prepare a composite mesoporous molecular sieve.
[0052] Example 1
[0053] The compound ratio of 20g is m USY :m MSU-1 =60:40 (USY+MSU-1) composite mesoporous molecular sieve (B acid content 54μmole / g, specific surface area 782m 2 / g, mesopore volume 0.46mL / g, total pore volume 0.68mL / g), 57g mesoporous alumina (mesopore (pores with pore diameters of 2-50nm) volume 1.24mL / g, specific surface area 281m 2 / g, bulk density 0.40g / mL), 70g mesoporous amorphous silica-alumina (total mesopore (pores with pore diameters of 2-50nm) volume 1.72mL / g, specific surface area 503m 2 / g, bulk density 0.30g / mL), 3.0g of sesbania powder, after mixing, add dropwise a mixed solution of 3.5g concentrated nitric acid (96wt%), 3.2g of citric acid and 81g of water, extrude into 1.5mm cylinders, dry at 110℃ for 2h, and calcine at 550℃ in air atmosphere for 4h to make a carrier.
[0054] Then, the catalyst was impregnated with an impregnation solution prepared with nickel nitrate and ammonium metatungstate, dried at 120°C for 4 hours, and calcined at 500°C in air atmosphere for 4 hours to obtain catalyst A. According to specific requirements, the catalyst was crushed or cut into the required particle size or length, and the hydrogenation reaction could be carried out after sulfurization.
[0055] Example 2
[0056] Compound 25g in proportion to m USY :m MSU-1 =60:40 (USY+MSU-1) composite mesoporous molecular sieve (B acid content 54μmole / g, specific surface area 782m 2 / g, average crystal size of 186nm, mesopore volume of 0.46mL / g, total pore volume of 0.68mL / g), 53g mesoporous alumina (mesopore (2-50nm) volume of 1.24mL / g, specific surface area of 281m 2 / g, bulk density 0.40g / mL), 66g mesoporous amorphous silica-alumina (total mesopore (2-50nm) volume 1.72mL / g, specific surface area 503m 2 / g, bulk density 0.30g / mL), 3.0g of sesbania powder, after mixing, add dropwise a mixed solution of 3.5g concentrated nitric acid (96wt%), 3.2g of citric acid and 81g of water, extrude into 1.5mm cylinders, dry at 110℃ for 2h, and calcine at 550℃ in air atmosphere for 4h to make a carrier.
[0057] Then, the catalyst was impregnated with an impregnation solution prepared with nickel nitrate and ammonium metatungstate, dried at 120°C for 4 hours, and calcined at 500°C in air atmosphere for 4 hours to obtain catalyst B. According to specific requirements, the catalyst was crushed or cut into the required particle size or length, and the hydrogenation reaction could be carried out after sulfurization.
[0058] Example 3
[0059] Compound 25g in proportion to m USY :m MSU-1 =80:20 (USY+MSU-1) composite mesoporous molecular sieve (B acid content 65μmole / g, specific surface area 774m 2 / g, mesopore volume 0.42mL / g, total pore volume 0.61mL / g), 53g mesoporous alumina (mesopore (2-50nm) volume 1.24mL / g, specific surface area 281m 2 / g, bulk density 0.40g / mL), 66g mesoporous amorphous silica-alumina (total mesopore (2-50nm) volume 1.72mL / g, specific surface area 503m 2 / g, bulk density 0.30g / mL), 3.0g of sesbania powder, after mixing, add dropwise a mixed solution of 3.5g concentrated nitric acid (96wt%), 3.2g of citric acid and 81g of water, extrude into 1.5mm cylinders, dry at 110℃ for 2h, and calcine at 550℃ in air atmosphere for 4h to make a carrier.
[0060] Then, the catalyst was impregnated with an impregnation solution prepared with nickel nitrate and ammonium metatungstate, dried at 120°C for 4 hours, and calcined at 500°C in air atmosphere for 4 hours to obtain catalyst C. According to specific requirements, the catalyst was crushed or cut into the required particle size or length, and the hydrogenation reaction could be carried out after sulfurization.
[0061] Example 4
[0062] Compound 25g in proportion to m USY :m MSU-1 =40:60 (USY+MSU-1) composite mesoporous molecular sieve (B acid content 43μmole / g, specific surface area 794m 2 / g, mesopore volume 0.49mL / g, total pore volume 0.71mL / g), 53g mesoporous alumina (mesopore (2-50nm) volume 1.24mL / g, specific surface area 281m 2 / g, bulk density 0.40g / mL), 66g mesoporous amorphous silica-alumina (total mesopore (2-50nm) volume 1.72mL / g, specific surface area 503m 2 / g, bulk density 0.30g / mL), 3.0g of sesbania powder, after mixing, add dropwise a mixed solution of 3.5g concentrated nitric acid (96wt%), 3.2g of citric acid and 81g of water, extrude into 1.5mm cylinders, dry at 110℃ for 2h, and calcine at 550℃ in air atmosphere for 4h to make a carrier.
[0063] Then, the catalyst was impregnated with an impregnation solution prepared with nickel nitrate and ammonium metatungstate, dried at 120°C for 4 hours, and calcined at 500°C in air atmosphere for 4 hours to obtain catalyst D. According to specific requirements, the catalyst was crushed or cut into the required particle size or length, and the hydrogenation reaction could be carried out after sulfurization.
[0064] Comparative Example 1
[0065] 20g of conventional Y molecular sieve (B acid content 63μmole / g, specific surface area 593m 2 / g, mesopore volume 0.19mL / g, total pore volume 0.43mL / g), 57g conventional alumina (mesopore (2-50nm) volume 0.62mL / g, specific surface area 258m 2 / g, bulk density 0.73g / mL), 70g conventional amorphous silica-alumina (total mesopore (2-50nm) volume 0.65mL / g, specific surface area 311m 2 / g, bulk density 0.53g / mL), 3.0g sesbania powder, after mixing, add dropwise 3.5g concentrated nitric acid (96wt%), 3.2g citric acid and 79g water mixed solution, squeeze into 1.5mm cylinder, dry at 110℃ for 2h, calcine at 550℃ air atmosphere for 4h to make a carrier. Then impregnate with impregnation solution prepared by nickel nitrate and ammonium metatungstate, dry at 120℃ for 4h, calcine at 500℃ air atmosphere for 4h to make catalyst E. According to specific requirements, crush or cut into the required particle size or length, and carry out hydrogenation reaction after sulfurization.
[0066] Comparative Example 2
[0067] 25g of conventional Y molecular sieve (B acid content 63μmole / g, specific surface area 593m 2 / g, mesopore volume 0.19mL / g, total pore volume 0.43mL / g), 53g conventional alumina (mesopore (2-50nm) volume 0.62mL / g, specific surface area 258m 2 / g, bulk density 0.73g / mL), 66g conventional amorphous silica-alumina (total mesopore (2-50nm) volume 0.65mL / g, specific surface area 311m 2 / g, bulk density 0.53g / mL), 3.0g sesbania powder, after mixing, add dropwise 3.5g concentrated nitric acid (96wt%), 3.0g citric acid and 79g water mixed solution, squeeze into 1.5mm cylinder, dry at 110℃ for 2h, calcine at 550℃ air atmosphere for 4h to make a carrier. Then impregnate with impregnation solution prepared by nickel nitrate and ammonium metatungstate, dry at 120℃ for 4h, calcine at 500℃ air atmosphere for 4h to make catalyst F. According to specific requirements, crush or cut into the required particle size or length, and carry out hydrogenation reaction after sulfurization.
[0068] The physicochemical properties of catalysts A, B, C, D, E, and F prepared in the above examples and comparative examples are shown in Table 3:
[0069] Table 3 Physicochemical properties of catalysts A, B, C, D, E, and F
[0070]
[0071] Example 5
[0072] Catalyst A, Catalyst B, Catalyst C, Catalyst D, Catalyst E, and Catalyst F in Examples 1, 2, 3, 4 and Comparative Examples 1 and 2 were evaluated on a 200 ml small fixed bed hydrogenation evaluation device using high aromatic diesel as raw material (properties shown in Table 4). The specific steps are as follows:
[0073] (1) The high aromatic diesel (LCO) feedstock is passed through a pretreatment catalyst bed under hydrogenation pretreatment conditions to remove impurities such as sulfur and nitrogen, and to perform partial saturation of aromatics; the hydrogenation pretreatment conditions in this embodiment are: reaction pressure 8.0 MPa, reaction temperature 382°C, hydrogen-to-oil volume ratio 800:1, volume space velocity 1.2 h -1 .
[0074] (2) the reaction product obtained in step (1) is subjected to hydrogenation reforming through a hydrogenation reforming catalyst bed (catalyst A, catalyst B, catalyst C, catalyst D, catalyst E or catalyst F) without undergoing gas-liquid separation;
[0075] (3) Separating the reaction product obtained in step (2) to obtain gasoline and diesel components.
[0076] Table 3 Raw oil properties
[0077] Crude oil LCO <![CDATA[Density (20 °C), g / cm 3 > 0.9291 Distillation range (ASTM D-86), ℃ Initial distillation point 165 10% 234 50% 298 Final distillation point 387 Sulfur content, μg / g 2110 Nitrogen content, μg / g 1070 Cetane number ~20 Total aromatic content, wt% 77.8 Content of two-ring or higher aromatic hydrocarbons, wt% 51.6
[0078] Table 4 Catalyst evaluation results
[0079]
[0080]
[0081] It can be seen from Table 4 that, under the same evaluation process conditions, compared with the catalyst of the comparative example, the catalysts A, B, C and D prepared in the embodiment of the present invention have high gasoline fraction yield, large increase in the cetane number of the diesel fraction, and low hydrogen consumption, that is, the catalyst has excellent hydrogenation and upgrading performance when treating high aromatic diesel, and can produce high-aromatic potential naphtha while producing high-aromatic potential naphtha, and can produce high-quality diesel blending components, which is helpful to reduce the diesel-gasoline ratio; the developed catalyst can effectively and efficiently convert inferior diesel into high value-added products, and has great industrial application value in refining and chemical integration enterprises.
[0082] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.
Claims
1. A diesel hydro-reforming catalyst, characterized in that: The catalyst comprises, based on the total weight, 10-30 wt% of active metals of Group VIB calculated by weight of oxides, 1-5 wt% of active metals of Group VIII calculated by weight of oxides, 15-40 wt% of mesoporous amorphous silica-alumina, 5-30 wt% of mesoporous alumina, and 20-25 wt% of composite mesoporous molecular sieves; the composite mesoporous molecular sieves are composed of USY molecular sieves and MSU-1 molecular sieves; the mesoporous amorphous silica-alumina refers to amorphous silica-alumina in which pores with a pore size of 2-50 nm account for more than 85%, and the mesoporous alumina refers to alumina in which pores with a pore size of 2-50 nm account for more than 85%.
2. The diesel hydro-reforming catalyst according to claim 1, characterized in that The VIB group active metal is Mo and / or W, and the VIII group active metal is Co and / or Ni; the content of the VIB group active metal is 10-20wt%, and the content of the VIII group active metal is 1-3wt%.
3. The diesel hydro-reforming catalyst according to claim 1, characterized in that In the composite mesoporous molecular sieve, the mass ratio of USY molecular sieve to MSU-1 molecular sieve is 80:20 to 40:
60.
4. The diesel hydro-reforming catalyst according to claim 3, characterized in that In the composite mesoporous molecular sieve, the mass ratio of USY molecular sieve to MSU-1 molecular sieve is 60:
40.
5. The diesel hydro-reforming catalyst according to claim 1, characterized in that The preparation method of the composite mesoporous molecular sieve comprises the following steps: adding USY molecular sieve and MSU-1 molecular sieve into an alkaline solution, stirring, standing, filtering, washing, drying and calcining to prepare the composite mesoporous molecular sieve.
6. The diesel hydro-reforming catalyst according to claim 5, characterized in that: Stir thoroughly in an alkaline solution for 2 to 6 hours, let stand for 0.5 to 3 hours, filter, wash, dry at 100 to 150°C for 2 to 6 hours, and calcine at 500 to 550°C for 4 to 6 hours.
7. The diesel hydro-reforming catalyst according to claim 5 or 6, characterized in that: The alkaline solution is selected from potassium hydroxide solution, hexamethylenediamine solution, ammonium bicarbonate solution and ammonia water.
8. The diesel hydro-reforming catalyst according to claim 1, characterized in that The volume of the pores with a pore diameter of 2-50 nm in the mesoporous amorphous silica-alumina is 1.20-1.90 mL / g, and the specific surface area is 380-550 m 2 / g, the bulk density is 0.15-0.40g / mL; the volume of the pores with a pore diameter of 2-50nm in the mesoporous alumina is 0.80-1.60mL / g, and the specific surface area is 220-380m 2 / g, and the bulk density is 0.35-0.55g / mL.
9. A method for preparing a diesel hydro-reforming catalyst according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) mixing mesoporous amorphous silica-alumina, mesoporous alumina, composite mesoporous molecular sieve, binder and extrusion aid uniformly, extruding into strips, and drying and calcining the obtained shaped product to prepare a carrier; (2) The carrier is impregnated with an impregnation solution containing active metals, dried and calcined to obtain a catalyst.
10. The preparation method according to claim 9, characterized in that: The adhesive is made of inorganic acid and / or organic acid, the inorganic acid is selected from one or two of hydrochloric acid, nitric acid, phosphoric acid and sulfuric acid, and the organic acid is selected from one or two of formic acid, acetic acid, citric acid and tartaric acid; the extrusion aid is selected from one or more of starch, sesbania powder, polyethanol and methyl cellulose, and its content is 1.0-5.0wt%.
11. The preparation method according to claim 9, characterized in that: The content of the extrusion aid is 2-4 wt%.
12. The preparation method according to claim 9, characterized in that: The carrier is cylindrical or a special-shaped bar.
13. The preparation method according to claim 12, characterized in that: The special-shaped strip is in the shape of a three-leaf clover or a four-leaf clover.
14. A diesel hydro-reforming method, characterized in that: The diesel hydro-reforming catalyst according to any one of claims 1 to 8 is used as a catalyst, the diesel is an inferior high-aromatic diesel fraction with a distillation range of 150 to 420° C., and the inferior high-aromatic diesel fraction includes at least one of catalytic cracking diesel, coal tar, and coal direct liquefaction oil.
15. The diesel hydro-upgrading method according to claim 14, characterized in that: The distillation range of the diesel is 150-390°C.
16. The diesel hydro-upgrading method according to claim 14, characterized in that: The total aromatic content of the diesel is greater than 60 wt%.
17. The diesel hydro-upgrading method according to claim 14, characterized in that: The diesel hydro-reforming catalyst needs to be pre-sulfurized when treating low-quality high-aromatic diesel raw materials. The pre-sulfurization conditions are: reaction temperature 200-400°C, reaction pressure 6-12MPa, hydrogen-oil volume ratio 350-800:1, volume space velocity 1.0-3.0h -1 ; The reaction conditions of hydrogenation reforming are: reaction temperature 320~420℃, pressure 6~12MPa, hydrogen-oil volume ratio 350~800:1, volume space velocity 0.5~3.0h -1 .