Electromagnetic heat-melting tin alloy solder and its preparation and soldering method

Through the combination of electromagnetic heat-melting tin alloy solder and electromagnetic wave heating equipment, the problems of oxidation and environmental pollution of tin alloy solder during the welding process are solved, high-quality welding and low-cost production are achieved, and product life is extended.

CN116441786BActive Publication Date: 2024-10-29SHENZHEN QIANHAI ZHENBAIYI TECHNOLOGY CO LT +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310459147.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-10-29
Estimated Expiration
2043-04-26

AI Technical Summary

Technical Problem

Existing tin alloy solders are prone to oxidation, impurity formation, leakage and environmental pollution due to high temperatures during the welding process, and the welding quality is difficult to control, resulting in high failure rates of electronic products and high cost and quality control costs.

Method used

Using electromagnetic heat-melting tin alloy solder, through a specific proportion of particulate metal laminated materials and special electromagnetic wave heating equipment, welding is quickly heated from the inside out, reducing the amount of flux and power loss, avoiding high temperature damage to components, and achieving seamless Contact heating.

Benefits of technology

It improves solder quality, reduces solder oxidation and residues, reduces environmental pollution and costs, extends product service life, and avoids welding quality problems and high temperature damage to components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116441786B_ABST
    Figure CN116441786B_ABST
Patent Text Reader

Abstract

The present invention discloses an electromagnetic hot-melting tin alloy solder and its preparation and soldering method, including high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials, high-purity copper or other highly conductive metal materials and synthetic materials, high-purity zinc or other metal materials that easily form eutectic alloys with tin, and tin alloys. The present invention contains a specific proportion of microparticle-shaped metal laminated materials that can be heated by a specific electromagnetic field. The soldering process is completed by using a special electromagnetic wave heating device to quickly heat and fuse the invented tin alloy solder from the inside out, which can improve the quality of the solder, significantly reduce the amount of tin alloy and flux used and the loss of electric energy, and can also eliminate the cleaning link after the soldering is completed, thereby reducing costs and reducing pollution to the environment, especially avoiding damage to components caused by high temperature and increasing the service life of the product. It is inevitable to completely replace the existing tin alloy solder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electronic product manufacturing, and in particular to an electromagnetic hot-melting tin alloy solder and a preparation method thereof and a soldering method. Background Art

[0002] Tin alloy solder is a fusible metal with a lower melting point than the metal being welded. When the solder melts, it can wet the surface of the metal being welded without melting the metal, and form an alloy layer at the contact surface to connect the metal to the metal being welded. In general electronic product assembly, it is commonly known as solder.

[0003] Tin alloy solder is often processed and shaped according to specified sizes when used, and there are many forms such as sheets, blocks, pastes, strips, balls and wires;

[0004] 1) Filamentary solder - usually called solder wire, with rosin wrapped in the center, called rosin core welding wire, commonly used in manual soldering. The outer diameter of rosin core welding wire usually has specifications such as 0.5mm, 0.6mm, 0.8mm, 1.Omm, 1.2mm, 1.6mm, 2.Omm, 2.3mm, 3.Omm, etc.

[0005] 2) Flake solder-commonly used for welding silicon wafers and other sheet welded parts;

[0006] 3) Strip solder - commonly used in automatic assembly production lines, using an automatic welding machine to punch out a section of the strip solder for welding to improve production efficiency;

[0007] 4) Solder paste - solder and flux are mixed together. When welding, the solder paste is first applied to the printed circuit board, and then soldering is performed. It has been widely used in automatic patch processes;

[0008] The existing tin alloy solder is composed of solder resist and tin alloy in a certain proportion. The existing tin alloy is mainly composed of tin-lead, tin-bismuth, tin-silver-copper alloy, and the general proportions are SN63 / PB37, SN42BI58, SN96.5CU0.5AG3.0 and SN99CU0.7AG0.3. Before there was a lead-free requirement, the most commonly used alloy was Sn63 / Pb37. The tin alloy solder with lead-free requirements is mainly composed of tin / silver / copper SN96.5CU0.5AG3.0 and SN99CU0.7AG0.3. Silver and copper replace the original lead component and a small amount of antioxidant elements. Elements that reduce the melting point are added for low temperature requirements.

[0009] Soldering with tin alloy solder is called tin soldering. The soldering temperature of tin soldering is low and it can be achieved with simple tools and the method is simple. It is easy to repair solder joints and replace components, so it is the most common soldering method used in the assembly of complete machines in the electronics industry.

[0010] The existing tin alloy solder is currently mainly heated from the surface to the inside by heating tools such as electric soldering irons and flat soldering tables, or non-contact heating such as laser heating or air heating such as reflow soldering to melt the solder paste. After the alloy components cool and solidify, a solder joint is formed between the two objects to be soldered to achieve the purpose of metallurgical connection. The existing tin alloy solder using the existing hot melt soldering process has the following disadvantages:

[0011] 1. When the existing soldering adopts the direct contact heating method of electric soldering iron and flat soldering table, it is easy to cause soldering quality problems such as false soldering and cold soldering due to the influence of factors such as the power and temperature of the electric soldering iron or flat soldering table, the type of tin alloy material, the amount of tin alloy material, the heat dissipation of the object to be welded, the ambient temperature, the degree of air flow, the type of soldering iron tip, the contact pressure when transferring heat to the welded part, the contact area and contact angle, and the proficiency of the operator. In particular, when the soldering iron is used for contact heating, since the soldering iron tip is in a high temperature state for a long time and contacts weak acidic substances such as flux, its surface is easily oxidized and stained with a layer of black impurities. These impurities form a heat insulation layer, which will hinder the heat conduction between the soldering iron tip and the solder weldment if it is not cleaned in time, thereby affecting the welding quality. In addition, the carbonized material on the surface of the soldering iron tip will remain between the solder joints, affecting the appearance and even causing leakage and affecting the product quality. If the temperature of the electric soldering iron or flat soldering table is too high, it is very easy to damage the components or PCB. Even using the soldering iron tip to directly heat and melt the tin, once the soldering iron tip leaks electricity, it will damage static-sensitive components and cause significant economic losses. If the performance of the components is degraded, it will trigger large-scale after-sales incidents, which will have a huge negative impact on the product's brand image.

[0012] 2. Existing tin alloy solder is used in the form of solder paste in the surface mount soldering process (SMT) of electronic products. The solder paste is printed and coated on the pads of the printed circuit board, and the surface mount components are accurately placed on the pads coated with solder paste, and then placed in the reflow soldering equipment (hot air heating equipment) to heat the circuit board according to a specific reflow temperature curve to melt the solder paste. After its alloy components cool and solidify, solder joints are formed between the components and the printed circuit board to achieve welding. There are also many factors that affect the quality of SMT solder: for example, the mismatch between the reflow temperature setting and the type of solder paste will cause over-temperature oxidation or cold welding due to insufficient temperature or insufficient melting time; uneven hot air in the reflow soldering equipment will cause the solder quality problem of tombstone (different degrees of melting of solder paste on both sides of the surface mount component cause the component to stand up); the preheating zone of the reflow temperature curve is used to raise the temperature of the PCB from the ambient temperature to the required active temperature. In this zone, the temperature of the product rises continuously at a rate of no more than 2-5℃ per second. If the temperature rises too fast, it will cause certain defects, such as fine cracks in ceramic capacitors. If the temperature rises too slowly, the solder paste will be over-sensitive to the temperature, and there will not be enough time for the PCB to reach the active temperature, resulting in poor solder quality. The setting of the preheating zone is affected by factors such as ambient temperature, type of solder, density of mounted components, size of PCB, thickness of PCB copper foil, etc., so it is difficult to avoid the problem of poor soldering. The SMT process is a continuous high-temperature process, and the temperature resistance requirements for PCB and surface mount components are very high. If you are not careful, it will cause damage to surface mount components, and the high temperature resistance requirements for PCB and surface mount components will increase a lot of costs. In addition, the reflow soldering equipment must maintain a continuous high temperature during operation and needs to discharge the high-temperature evaporation gas of the flux. The production process consumes a lot of energy and is very costly.

[0013] 3. Existing tin alloy solder is used in the form of high-temperature liquid tin alloy in the wave soldering and dip soldering processes of circuit boards. Most PCB solders with more plug-in materials use this production process. The tin alloy solder is placed in the tin melting tank of the tin furnace and heated to a liquid state with an electric heating tube. After the PCB with the plug-in is sprayed with flux and in contact with the solder liquid surface, the tin alloy adheres to the PCB pad and the pins of the plug-in material to complete the soldering work. Since this process is affected by factors such as the heat dissipation of the object to be welded, the ambient temperature, the quality of the flux, the amount of solder resist, the quality of the tin alloy solder, and the proficiency of the operator, it is easy to cause solder quality problems such as false soldering and cold soldering. Since the solder needs to maintain a continuous high temperature, the tin surface is very easy to oxidize and needs to be cleaned in time to form a large amount of tin slag, causing a large loss of solder. Since the residues produced by the high temperature of the flux and solder adhere to the surface of the PCB, it is not only unsightly but may also cause leakage. Therefore, most PCBs need to be washed with a cleaning agent or ultrasonic board after the wave soldering or dip soldering process, which not only increases the process cost but also causes environmental pollution.

[0014] According to statistics, nearly half of the failures of electronic complete products are caused by poor welding. An electronic product has tens of thousands of solder joints. It is common for the entire product to not work properly due to quality problems of one, two or several solder joints. However, it is not easy to find the solder joints that cause failures in an electronic device with tens of thousands of solder joints, especially the false solder joints. Sometimes it is normal when just soldered, but after a period of time, the machine fails due to increased oxidation. Especially for high-frequency and high-voltage equipment, if there are burrs, sand holes and bubbles on the solder joints, tip discharge may occur or the internal resistance of the welding joint is too large, causing overheating and fire. Due to the limitations of existing tin alloy solders and the process of heating and welding solder from the outside to the inside, although a large amount of quality control costs have been invested, it has not been possible to effectively eliminate the quality problems of products caused by solder quality. In addition, the use of existing tin alloy solders and soldering processes has a relatively large loss of solder and electric energy, causing relatively large environmental pollution and high costs. Summary of the invention

[0015] In order to solve the above problems, the present invention provides an electromagnetic heat-melting tin alloy solder and its preparation and soldering method, which contains a specific proportion of microparticle-shaped metal laminated materials that can be heated by a specific electromagnetic field. The tin alloy solder of the invention is quickly heated and melted from the inside out by using a special electromagnetic wave heating device to complete the soldering process, which can improve the solder quality, significantly reduce the amount of tin alloy and flux and the loss of electric energy, and can also eliminate the cleaning link after the soldering is completed, thereby reducing costs and reducing pollution to the environment, especially avoiding damage to components by high temperature and increasing the service life of the product. It has the inevitability of completely replacing the existing tin alloy solder.

[0016] The present invention is realized by the following technical scheme: an electromagnetically heated tin alloy solder, comprising:

[0017] High-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials, high-purity copper or other highly conductive metal materials and synthetic materials, high-purity zinc or other metal materials that easily form eutectic alloys with tin, and tin alloys constitute electromagnetic hot-melt tin alloy solder, which is a microparticle-shaped metal laminate material.

[0018] As a preferred technical solution, the mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 28-40%.

[0019] As a preferred technical solution, the mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 38.8%.

[0020] As a preferred technical solution, the mass percentage of high-purity copper or other high-conductivity metal materials and synthetic materials is 5-15%.

[0021] As a preferred technical solution, the mass percentage of high-purity copper or other highly conductive metal materials and synthetic materials is 8.73%.

[0022] As a preferred technical solution, the mass percentage of high-purity zinc or other metal materials that can easily form a eutectic alloy with tin is 10-22%.

[0023] As a preferred technical solution, the mass percentage of high-purity zinc or other metal materials that can easily form a eutectic alloy with tin is 17.68%.

[0024] A method for preparing an electromagnetically molten tin alloy solder of the present invention comprises the following steps:

[0025] S1. Prepare iron with a purity of 99.5% or more and a mass percentage of 38.8%, copper with a purity of 99.5% or more and a mass percentage of 8.73%, and zinc with a purity of 99.5% or more and a mass percentage of 17.68;

[0026] S2. Prepare an appropriate amount of tin alloy;

[0027] S3, copper with a purity of 99.5% or more and 8.73% by mass, zinc with a purity of 99.5% or more and 17.68% by mass, and an appropriate amount of tin alloy are plated on the outside of the high-purity iron in sequence;

[0028] S4, preparing electromagnetically heated molten tin alloy solder.

[0029] The invention discloses a method for soldering by using electromagnetic heat to melt tin alloy solder. The tin alloy solder is melted by electromagnetic heat and a special electromagnetic wave heating device is used to quickly heat and fuse the solder from the inside out to complete the soldering process.

[0030] The beneficial effects of the present invention are as follows: 1. Since the surface heating time is short and the probability of oxidation is small, the tin alloy solder of the present invention can reduce the content of the flux, thereby reducing the harmful gas and residue generated by the flux after high temperature, thereby reducing the risk of air pollution and PCB leakage;

[0031] 2. The tin alloy solder powder of the present invention can be heated by a non-contact specific electromagnetic field soldering process, and the electric heating element does not need to directly contact the solder to avoid damage to electrostatic sensitive components due to leakage of the electric heating element;

[0032] 3. The tin alloy solder powder of the present invention uses a dedicated electromagnetic wave heating device to heat and fuse the inside and outside of the tin alloy solder of the present invention synchronously, which is almost unaffected by factors such as the heat dissipation of the object to be welded, the ambient temperature, and the proficiency of the operator. There is almost no residue generated by the high temperature of the solder, which can greatly improve the quality of the solder and reduce the cost of solder quality control. In particular, it avoids the large loss of electricity and solder in hand dip soldering and wave soldering due to oxidation to form tin slag and the need to replace the solder due to pollution;

[0033] 4. The tin alloy solder powder of the present invention can also be used in the form of solder paste in the surface mount soldering process (SMT) of electronic products. The tin alloy solder of the present invention is quickly heated and melted from the inside out using a dedicated electromagnetic wave heating device to complete the soldering process, thereby avoiding the welding quality problems, high energy consumption and large air pollution problems caused by the existing tin alloy solder using reflow soldering equipment (hot air heating equipment). In addition, the tin alloy solder of the present invention does not need to be refrigerated to maintain surface activity because it is heated and melted as a whole inside and outside at the same time, which reduces the production links and the quality problems caused by the links, and reduces the production cost and loss;

[0034] 5. The tin alloy solder of the present invention reduces the content of tin alloy and greatly reduces the cost of using solder. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 It is a schematic cross-sectional view of a single particle axis of Type 6 tin alloy solder powder of the present invention;

[0037] Figure 2 It is a schematic diagram of the axis single-layer atomic sequence structure of a single particle of type 6 tin alloy solder powder of the present invention. DETAILED DESCRIPTION

[0038] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.

[0039] Any feature disclosed in this specification (including any additional claims, abstract and drawings), unless otherwise stated, may be replaced by other equivalent or alternative features with similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.

[0040] In the description of the present invention, it is necessary to understand that the terms "one end", "the other end", "outside", "upper", "inside", "horizontal", "coaxial", "center", "end", "length", "outer end" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0041] In addition, in the description of the present invention, “plurality” means at least two, for example, two, three, etc., unless otherwise clearly and specifically defined.

[0042] Terms such as "upper", "above", "lower", "below", etc. used in the present invention to indicate spatial relative positions are used for the purpose of convenience to describe the relationship of one unit or feature relative to another unit or feature as shown in the accompanying drawings. Terms of spatial relative position may be intended to include different orientations of the device in use or operation in addition to the orientation shown in the drawings. For example, if the device in the figure is turned over, the unit described as being "below" or "beneath" other units or features will be located "above" the other units or features. Therefore, the exemplary term "below" can encompass both the above and below orientations. The device may be oriented in other ways (rotated 90 degrees or other orientations), and the spatially related descriptors used herein interpreted accordingly.

[0043] In the present invention, unless otherwise clearly specified and limited, the terms "disposed", "socketed", "connected", "through", "plugged" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0044] Example 1

[0045] The electromagnetic hot-melt tin alloy solder of the present invention comprises high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials, high-purity copper or other highly conductive metal materials and synthetic materials, high-purity zinc or other metal materials that can easily form eutectic alloys with tin, and tin alloys, which constitute the electromagnetic hot-melt tin alloy solder. The electromagnetic hot-melt tin alloy solder is a microparticle-shaped metal laminated material.

[0046] In this embodiment, the mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 28-40%. Specifically, in this embodiment, high-purity iron is used, and its mass percentage is 28%.

[0047] The mass percentage of high-purity copper or other high-conductivity metal materials and synthetic materials is 5-15%. Specifically, in this embodiment, high-purity copper is used, and its mass percentage is 5%.

[0048] The mass percentage of high-purity zinc or other metal materials that can easily form a eutectic alloy with tin is 10-22%. Specifically, in this embodiment, high-purity zinc is used, and its mass percentage is 10%.

[0049] Example 2

[0050] The electromagnetic hot-melt tin alloy solder of the present invention comprises high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials, high-purity copper or other highly conductive metal materials and synthetic materials, high-purity zinc or other metal materials that can easily form eutectic alloys with tin, and tin alloys, which constitute the electromagnetic hot-melt tin alloy solder. The electromagnetic hot-melt tin alloy solder is a microparticle-shaped metal laminated material.

[0051] In this embodiment, the mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 28-40%. Specifically, in this embodiment, high-purity iron is used, and its mass percentage is 38.8%.

[0052] The mass percentage of high-purity copper or other high-conductivity metal materials and synthetic materials is 5-15%. Specifically, in this embodiment, high-purity copper is used, and its mass percentage is 8.73%.

[0053] The mass percentage of high-purity zinc or other metal materials that can easily form a eutectic alloy with tin is 10-22%. Specifically, in this embodiment, high-purity zinc is used, and its mass percentage is 17.68%.

[0054] The mass percentage in this embodiment is the optimal configuration.

[0055] Example 3

[0056] The electromagnetic hot-melt tin alloy solder of the present invention comprises high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials, high-purity copper or other highly conductive metal materials and synthetic materials, high-purity zinc or other metal materials that can easily form eutectic alloys with tin, and tin alloys, which constitute the electromagnetic hot-melt tin alloy solder. The electromagnetic hot-melt tin alloy solder is a microparticle-shaped metal laminated material.

[0057] In this embodiment, the mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 28-40%. Specifically, in this embodiment, high-purity iron is used, and its mass percentage is 40%.

[0058] The mass percentage of high-purity copper or other high-conductivity metal materials and synthetic materials is 5-15%. Specifically, in this embodiment, high-purity copper is used, and its mass percentage is 15%.

[0059] The mass percentage of high-purity zinc or other metal materials that can easily form a eutectic alloy with tin is 10-22%. Specifically, in this embodiment, high-purity zinc is used, and its mass percentage is 22%.

[0060] The invention discloses a method for preparing an electromagnetic hot-melt tin alloy solder, taking iron, copper, zinc and tin alloy as examples, comprising the following steps: (i) preparing iron with a purity of 99.5% or more and a mass percentage of 38.8%, copper with a purity of 99.5% or more and a mass percentage of 8.73%, and zinc with a purity of 99.5% or more and a mass percentage of 17.68; (ii) preparing an appropriate amount of tin alloy; (iii) sequentially plating copper with a purity of 99.5% or more and a mass percentage of 8.73%, zinc with a purity of 99.5% or more and a mass percentage of 17.68, and an appropriate amount of tin alloy on the outside of the high-purity iron; and (iv) obtaining the electromagnetic hot-melt tin alloy solder.

[0061] Taking type 6 tin alloy solder powder as an example, its single particle is prepared by plating spherical pure iron particles with a diameter of about 4.14um with 128nm thick pure copper, 270nm thick pure zinc, and 400nm thick tin alloy (various commercial tin alloys such as SN63 / PB37, SN42BI58, SN96.5CU0.5AG3.0 and SN99CU0.7AG0.3 can be selected according to actual needs). Figure 1 and Figure 2 As shown in the figure, the width of an iron atom is about 4.14um, the width of a copper atom is about 128nm, the width of a zinc atom is about 270nm, and the width of a tin alloy atom is about 400nm.

[0062] The present invention relates to an invented tin alloy solder powder, which contains a specific proportion of metal laminated materials that can be heated by a specific electromagnetic field. The invented tin alloy solder is quickly heated and welded from the inside out by using a special electromagnetic wave heating device to complete the soldering process, which can improve the solder quality, significantly reduce the amount of tin alloy and flux used and the loss of electric energy. In addition, the cleaning link after the soldering is completed can be eliminated, thereby reducing costs and reducing pollution to the environment, especially avoiding damage to components by high temperature and increasing the service life of the product. It has the inevitability of completely replacing the existing tin alloy solder.

[0063] The invention of tin alloy solder can use special electromagnetic wave heating equipment to quickly heat and fuse from the inside out to complete the soldering process, which has the following advantages:

[0064] 1. Since the surface heating time is short and the probability of oxidation is small, the invention of tin alloy solder can reduce the content of flux, so that the harmful gas and residue generated by the flux at high temperature can be reduced, thereby reducing the risk of air pollution and PCB leakage;

[0065] 2. The tin alloy solder powder of the present invention can be heated by a non-contact specific electromagnetic field soldering process, and the electric heating element does not need to directly contact the solder to avoid damage to electrostatic sensitive components due to leakage of the electric heating element;

[0066] 3. The tin alloy solder powder of the present invention uses a dedicated electromagnetic wave heating device to heat and fuse the inside and outside of the tin alloy solder of the present invention synchronously, which is almost unaffected by factors such as the heat dissipation of the object to be welded, the ambient temperature, and the proficiency of the operator. There is almost no residue generated by the high temperature of the solder, which can greatly improve the quality of the solder and reduce the cost of solder quality control. In particular, it avoids the large loss of electricity and solder in hand dip soldering and wave soldering due to oxidation to form tin slag and the need to replace the solder due to pollution;

[0067] 4. The tin alloy solder powder of the present invention can also be used in the form of solder paste in the surface mount soldering process (SMT) of electronic products. The tin alloy solder of the present invention is quickly heated and melted from the inside out using a dedicated electromagnetic wave heating device to complete the soldering process, thereby avoiding the welding quality problems, high energy consumption and large air pollution problems caused by the existing tin alloy solder using reflow soldering equipment (hot air heating equipment). In addition, the tin alloy solder of the present invention does not need to be refrigerated to maintain surface activity because it is heated and melted as a whole inside and outside at the same time, which reduces the production links and the quality problems caused by the links, and reduces the production cost and loss;

[0068] 5. The tin alloy solder of the present invention reduces the content of tin alloy and greatly reduces the cost of using solder.

[0069] The above is only a specific implementation of the present invention and only a preferred embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any similar replacement and change made according to the principle described in the scope of the patent application of the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope defined in the claims.

Claims

1. A method for soldering by using electromagnetic heat to melt tin alloy solder, characterized in that: Use electromagnetic heat to melt tin alloy solder, and use special electromagnetic wave heating equipment to quickly heat and fuse from the inside out to complete the soldering process; The electromagnetically heated tin alloy solder comprises: High-purity iron, high-purity copper, high-purity zinc and tin alloy form electromagnetic hot-melting tin alloy solder, and the electromagnetic hot-melting tin alloy solder is a microparticle-shaped metal laminated material; The mass percentage of the high-purity iron is 28-40%; The mass percentage of the high-purity copper is 5-15%; The mass percentage of the high-purity zinc is 10-22%; The diameter of the electromagnetically heated tin alloy solder is 5.74 μm, wherein the width of an iron atom is 4.14 μm, the width of a copper atom is 128 nm, the width of a zinc atom is 270 nm, and the width of a tin alloy atom is 400 nm.

2. The method according to claim 1, characterized in that: The mass percentage of high-purity iron is 38.8%.

3. The method according to claim 1, characterized in that: The mass percentage of high-purity copper is 8.73%.

4. The method according to claim 1, characterized in that: The mass percentage of high-purity zinc is 17.68%.

5. The method according to claim 1, characterized in that: The method for preparing the electromagnetically molten tin alloy solder comprises the following steps: S1. Prepare iron with a purity of 99.5% or more and a mass percentage of 38.8%, copper with a purity of 99.5% or more and a mass percentage of 8.73%, and zinc with a purity of 99.5% or more and a mass percentage of 17.68; S2. Prepare an appropriate amount of tin alloy; S3, copper with a purity of 99.5% or more and 8.73% by mass, zinc with a purity of 99.5% or more and 17.68% by mass, and an appropriate amount of tin alloy are plated on the outside of the high-purity iron in sequence; S4, preparing electromagnetically heated molten tin alloy solder.

Citation Information

Patent Citations

  • Solder ball and manufacturing method thereof

    CN102672365A