Conductive aggregate, intelligent cement composite material and preparation method and application thereof
By using graphene and other materials in smart cement-based composite materials to form conductive aggregates and three-dimensional conductive networks, the problem of conductive phase agglomeration affecting performance is solved, and the effects of efficiently reducing resistivity and improving sensor sensitivity are achieved.
Patent Information
- Application Number
- CN202310436768.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-21
AI Technical Summary
When the resistivity of existing smart cement-based composite materials is reduced, the agglomeration of the conductive phase affects the working performance of the mixture, and traditional methods limit the sensitivity and conductivity of cement-based sensors.
Graphene, polystyrene sulfonic acid and PVDF emulsion are mixed to form a conductive polymer dispersion. River sand is soaked, stirred and dried to prepare conductive aggregate, which is then dry-mixed with cement, fly ash and carbon fiber to form a smart cement composite material. Construct conductive skeletons and three-dimensional conductive networks.
It significantly reduces the resistivity of cement mortar, improves the sensitivity and conductivity of the sensor, hardly damages the working performance and mechanical strength, and reduces energy consumption and carbon emissions.
Smart Images

Figure CN116462436B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a conductive aggregate, an intelligent cement composite material, a preparation method and application thereof, and application of the conductive aggregate in preparing a cement-based piezoresistive sensor, and belongs to the technical field of conductive cement-based composite materials. Background Art
[0002] As civil engineering gradually develops towards intelligence, smart cement-based composites have received great attention in recent years and can be applied to fields such as structural health monitoring, road deicing / snow melting, and electromagnetic interference shielding. The premise of these potential application areas is to give cement-based materials conductivity, which can be achieved by directly introducing conductive phases (such as carbon black, carbon nanotubes, graphene, and carbon fibers) into the cement matrix. Studies have shown that directly adding the above conductive phases to the cement matrix can reduce the resistivity of the original cement-based material (105-107Ω·cm) by about 3 orders of magnitude, and the reduction mainly depends on the concentration and dispersion quality of the conductive phase. However, in general, the direct introduction of conductive phases into the cement matrix will cause the conductive phase to agglomerate, seriously affecting the working performance of the mixture, and then affecting the mechanical and durability properties of cement-based materials. In addition, the agglomerated conductive phase cannot form a complete conductive path inside the cement-based material; therefore, in order to further reduce the resistivity of the specimen, the only way is to increase the amount of conductive phase or use a more complicated dispersion process, which undoubtedly increases the cost of smart cement-based composites and limits their practical application.
[0003] More importantly, the traditional strategy for preparing smart cement composites is to directly add the conductive phase to cement and make it conductive, and then mix it with aggregate. Considering the low volume proportion of cement in mortar / concrete (30-40% and 10-25%, respectively), the conductivity of the smart mortar / concrete prepared by this process will be greatly limited. In addition, this method limits the weakest interface transition zone in cement-based materials to the periphery of the conductive network, thereby limiting the sensitivity of cement-based sensors. Summary of the invention
[0004] The purpose of the present invention is to provide a conductive aggregate, an intelligent cement composite material and a preparation method and application thereof, so as to overcome the deficiencies in the prior art.
[0005] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0006] The main purpose of the present invention is to provide a method for preparing a conductive aggregate, comprising:
[0007] Mixing a mixed system of graphene, polystyrene sulfonic acid and water with a PVDF emulsion to form a conductive polymer dispersion;
[0008] The river sand is immersed in the conductive polymer dispersion, and after stirring and drying, an aggregate with a dense conductive polymer film deposited on the surface is obtained, namely, conductive aggregate.
[0009] The invention also provides conductive aggregate prepared by the preparation method.
[0010] Another object of the present invention is to provide a method for preparing a smart cement composite material, which comprises:
[0011] Cement, fly ash, the conductive aggregate and carbon fiber are dry-mixed, and then water is added to mix to obtain an intelligent cement composite material containing the conductive aggregate.
[0012] The invention also provides an intelligent cement composite material containing conductive aggregate prepared by the preparation method.
[0013] In addition, the present invention also provides a cement-based piezoresistive sensor, which is made of the intelligent cement composite material.
[0014] The present invention also provides the application of the cement-based piezoresistive sensor in the field of structural health monitoring of buildings, bridges, tunnels and the like.
[0015] Compared with the prior art, the beneficial effects of the present invention are at least:
[0016] 1) The present invention provides a new type of conductive aggregate. The introduction of the conductive aggregate forms a "conductive skeleton" structure inside the cement mortar, and is linked by randomly distributed conductive carbon fibers to form a "three-dimensional conductive network structure", which greatly increases the electrical conductivity of the conductive cement mortar.
[0017] 2) The weakest interface transition zone (aggregate-cement paste interface) in the smart cement composite material containing conductive aggregate provided by the present invention is embedded inside the conductive network, thereby increasing the sensitivity of the cement-based sensor. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 Schematic diagram of the preparation process of the conductive polymer in an embodiment of the present invention.
[0020] Figure 2 This is the appearance of natural aggregate.
[0021] Figure 3This is the appearance of the conductive aggregate prepared in Example 1 of the present invention.
[0022] Figure 4 This is a schematic diagram of the electrode distribution and resistivity test of the smart cement composite material containing conductive aggregate prepared in Example 1 of the present invention.
[0023] Figure 5 This is a schematic diagram of testing the piezoresistive performance of the smart cement composite material sensor containing conductive aggregate prepared in Example 1 of the present invention.
[0024] Figure 6 Schematic diagram of the distribution of the internal circuit of the smart cement composite material containing conductive aggregate prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be clearly and completely described below. It mainly provides a conductive aggregate, an intelligent cement composite material and its preparation method and application. The preparation method of the intelligent cement composite material is based on the interface coating design to greatly reduce the resistivity of the intelligent cement-based composite material while hardly damaging its working performance and mechanical strength.
[0026] One aspect of an embodiment of the present invention provides a method for preparing a conductive aggregate, comprising:
[0027] Mixing a mixed system of graphene, polystyrene sulfonic acid and water with a PVDF emulsion to form a conductive polymer dispersion;
[0028] The river sand is immersed in the conductive polymer dispersion, and after stirring and drying, an aggregate with a dense conductive polymer film deposited on the surface is obtained, namely, conductive aggregate.
[0029] In some specific embodiments, graphene and water are mixed for 1-3 minutes, a surfactant is used to modify the surface of the graphene, and ultrasonic dispersion is performed under ice bath conditions to obtain a graphene dispersion;
[0030] The mixed system of graphene, polystyrene sulfonic acid and water in the graphene oxide dispersion is mixed with the PVDF emulsion to form a conductive polymer dispersion.
[0031] Furthermore, the graphene includes highly conductive graphene, and the graphene is preferably KY HE-1 highly conductive graphene produced by Sichuan Kenye Technology Development Co., Ltd., with a carbon-oxygen ratio of 26, a sheet size of 5-15 μm, and a film conductivity of 660 S / cm (tested by four-probe method).
[0032] Furthermore, the surfactant includes melamine.
[0033] Furthermore, the mass ratio of the surfactant to graphene is 0.50-0.55:1.
[0034] In some specific embodiments, the PVDF emulsion includes Arkema Kynar Flex 2751 copolymer emulsion, with a melting point of 135° C. and a melt viscosity of 22 KP.
[0035] Furthermore, the solid content of the polystyrene sulfonic acid is 2%, and the density at 25° C. is 1.11 g / mL.
[0036] Furthermore, the particle size of the river sand is 0.075-4.75 mm, and the water absorption rate within 24 hours is 0.9%.
[0037] Furthermore, the stirring speed is 20-30 r / min, and the stirring time is 5-7 min.
[0038] Furthermore, the drying temperature is 70-80° C., and the drying time is 48-72 hours.
[0039] In some more specific embodiments, the graphene surface is first modified with an aqueous melamine solution, and then treated with an ultrasonic cell disperser (power 60-70 W, ultrasonic time 460-500 min) under ice bath conditions to obtain a high-quality graphene dispersion.
[0040] Furthermore, the graphene dispersion and the polystyrene sulfonic acid aqueous solution are treated with an industrial ultrasonic instrument at an ultrasonic power of 160-180 W for 30-40 minutes.
[0041] Furthermore, the dispersion process of the mixture and the PVDF emulsion is: firstly manually mixing for 1 minute, then using an industrial ultrasonic instrument to treat for 30-40 minutes at an ultrasonic power of 160-180W, and finally obtaining a well-dispersed conductive polymer dispersion.
[0042] Furthermore, river sand and the conductive polymer dispersion are mixed in a wide-mouthed basin and manually stirred at a speed of about 20-30 r / min for 5 minutes; then placed in an oven and dried at a temperature of 70-80° C. for 48 hours, and stirred evenly every about 1-2 hours during the drying process to prevent the conductive aggregates from sticking to each other.
[0043] Another aspect of the embodiments of the present invention further provides a conductive aggregate produced by the preparation method.
[0044] Another aspect of the embodiments of the present invention further provides a method for preparing a smart cement composite material, comprising:
[0045] Cement, fly ash, the conductive aggregate and carbon fiber are dry-mixed, and then water is added to mix to obtain an intelligent cement composite material containing the conductive aggregate.
[0046] Among them, graphene is coated on the surface of river sand in the form of a coating instead of being directly mixed with cement, avoiding the technical bottleneck of uneven dispersion (agglomeration) of graphene (carbon-based nanomaterials) in the cement matrix.
[0047] In some specific embodiments, a mixed system including cement, fly ash, the conductive aggregate and carbon fiber is dry-mixed, and then water is added to mix, and then stirred at a low speed and then at a high speed to obtain a smart cement composite material containing conductive aggregate.
[0048] Furthermore, the rotation speed of the low-speed stirring is 57-67 r / min, and the stirring time is 3-5 min.
[0049] Furthermore, the rotation speed of the high-speed stirring is 115-135 r / min, and the stirring time is 1-3 min.
[0050] In some specific embodiments, the water-to-binder ratio of the mixed system is 0.4-0.6.
[0051] In some specific embodiments, the cement includes silicate cement, and the cement is preferably ordinary silicate cement (P·O42.5).
[0052] In some specific embodiments, the fly ash includes ultrafine fly ash, the fly ash includes ultrafine fly ash, the average particle size is 5-10μm, and the strength activity index is greater than 80%. The introduction of ultrafine fly ash can not only reduce the amount of cement (reduce energy consumption and carbon emissions), optimize the system microstructure, but also improve the fluidity of the system.
[0053] Furthermore, the mass ratio of fly ash to cement is 10-15:100.
[0054] In some specific embodiments, the carbon fiber includes any one of 3 mm, 6 mm, and 10 mm chopped carbon fibers or a combination of two or more thereof, preferably 3 mm chopped carbon fibers, the diameter of the carbon fiber is 7-9 μm, the Young's modulus is 240 GPa, and the resistivity is 1.5×10 -3 Ω·cm, preferably chopped carbon fiber produced by Japan Tenax Company.
[0055] The length of carbon fiber has a significant effect on the electrical properties of smart mortar. At the same dosage, 3mm, 6mm and 10mm carbon fibers can all connect conductive aggregates (the theoretical spacing of conductive aggregates is about 100μm). The shorter the carbon fiber, the greater the number at the same dosage. The electrical properties of smart mortar with 3mm carbon fiber are better.
[0056] In some specific embodiments, the mass of graphene in the conductive aggregate is 0.1-1.0% of the mass of cement and fly ash.
[0057] Furthermore, the mass of the surfactant in the conductive aggregate is 0.05-0.50% of the mass of the cement and fly ash.
[0058] Furthermore, the mass of the carbon fiber is 0.1-0.2% of the mass of the cement and fly ash.
[0059] In some more specific embodiments, cement, fly ash, conductive aggregate and carbon fiber are mechanically stirred at an orbital speed of 57-67 r / min for 1 min, and then water is added and stirred at a low speed (57-67 r / min) for 3 min, and then stirred at a high speed (115-135 r / min) for 1 min. The resulting mixture (i.e., smart cement composite material containing conductive aggregate) is poured into an oiled mold, subjected to 30 s of high-frequency vibration (60-80 Hz) for vibration compaction, and then placed in a standard curing room for curing. The specimen curing age is 28 days. When testing electrical indicators, four electrode sheets are inserted in parallel when the fresh mixture is just poured into the mold.
[0060] In some more specific embodiments, the preparation method of the conductive aggregate and the smart cement composite material containing the conductive aggregate includes:
[0061] Step 1: Preparation of Conductive Polymer Dispersion
[0062] The graphene and deionized water were manually mixed for 1 minute and then subjected to a "chemical combined with physical" dispersion process to obtain a highly dispersed graphene dispersion; then the graphene was evenly mixed with a polystyrene sulfonic acid aqueous solution under ultrasonic conditions; finally, the above mixture was mixed with a PVDF emulsion to obtain a conductive polymer dispersion.
[0063] Step 2: Conductive aggregate preparation
[0064] The river sand is immersed in the above conductive polymer dispersion, and after simple stirring and drying, an aggregate having a layer of dense conductive polymer film deposited on the surface, namely, conductive aggregate, can be obtained.
[0065] Step 3: Preparation of conductive cement mortar (i.e., smart cement composite material containing conductive aggregate)
[0066] The dry materials such as cement, fly ash, conductive aggregate and carbon fiber are dry mixed, and then mixing water is added, and the mixture is stirred at a low speed and then at a high speed to finally obtain the conductive water-jet mortar.
[0067] In addition, an embodiment of the present invention further provides a cement-based piezoresistive sensor, which is made of the intelligent cement composite material containing conductive aggregate. Specifically, the cement and conductive aggregate are mechanically stirred at an orbital speed of 57r / min for 1min, and then a mixture of water and surfactant is added, first stirred at a low speed (57r / min) for 3min, and then stirred at a high speed (115r / min) for 1min. The resulting mixture is poured into an oiled mold, and then four parallel electrode sheets are inserted. After 30s of high-frequency vibration (60Hz) for vibration compaction, it is placed in a standard curing room for curing.
[0068] The embodiment of the present invention further provides a smart cement composite material prepared by the preparation method, wherein the thickness of the conductive film coating containing the conductive aggregate is 6-8 nm.
[0069] Furthermore, the resistivity of the smart cement composite material containing conductive aggregate decreased by 4 orders of magnitude, and the resistance change rate increased by 167 times.
[0070] The technical principles of the present invention are as follows:
[0071] The present invention proposes a unique "chemical combined with physical" dispersion process to prepare high-quality graphene dispersion liquid; and then evenly mixes with polystyrene sulfonic acid and PVDF emulsion to obtain a low-viscosity conductive polymer glue, which can well wrap aggregates (river sand and stone, etc.). In the process of mixing river sand and conductive polymer glue, continuous hand mixing can promote the conductive polymer to be evenly coated on the surface of river sand, and then after drying treatment, the water in the conductive polymer coated on the surface of river sand is evaporated, and an ultra-thin conductive film (about 6-8nm) is obtained by solid phase deposition, and the bonding strength between the conductive film and the aggregate is very good, that is, a high-quality conductive aggregate is obtained. The introduction of conductive aggregate forms a "conductive skeleton" in the cement mortar system, and at the same time introduces a small amount of carbon fiber (the amount added is lower than its seepage threshold, generally its seepage threshold is 0.5-1.0wt%) to form a "three-dimensional conductive network channel", which greatly improves the conductivity of the cement mortar; in addition, the introduction of fly ash can not only reduce the amount of cement, reduce energy consumption and carbon emissions; at the same time, the "micro-aggregate filling" and "volcanic ash" effects of ultrafine fly ash can optimize the mortar microstructure, improve strength and durability; more importantly, ultrafine fly ash has a good "ball / lubrication effect", which can improve the fluidity of the mixture and make the mixture more densely filled.
[0072] In addition, an embodiment of the present invention further provides a cement-based piezoresistive sensor, which is made of the smart cement composite material.
[0073] The embodiment of the present invention also provides the application of the cement-based piezoresistive sensor in the field of structural health monitoring.
[0074] In summary, the present invention uses a synthetic conductive polymer to deposit a 6-8nm conductive film (i.e., conductive aggregate) on the surface of river sand, introduces the conductive aggregate into the mortar system to construct a "conductive skeleton", and then connects the conductive aggregate through a small amount of randomly distributed carbon fibers to construct a "three-dimensional conductive network channel" inside the smart mortar, which can reduce the mortar resistivity by 4 orders of magnitude, and increase the resistance change rate by 167 times, and basically has no adverse effect on the fluidity and mechanical properties of the mortar. The cement-based piezoresistive sensor of the present invention can be used in the field of structural health monitoring.
[0075] The technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention, and do not have any limiting effect on them. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are usually carried out under conventional conditions or according to the conditions recommended by the manufacturer.
[0076] Example 1
[0077] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, comprising the following steps:
[0078] Step 1: Preparation of Conductive Polymer Dispersion
[0079] The graphene and deionized water were manually mixed for 1 minute and then subjected to a "chemical combined with physical" dispersion process to obtain a highly dispersed graphene dispersion; then the graphene was evenly mixed with a polystyrene sulfonic acid aqueous solution under ultrasonic conditions; finally, the above mixture was mixed with a PVDF emulsion to obtain a conductive polymer dispersion.
[0080] Step 2: Conductive aggregate preparation
[0081] The river sand is soaked in the above conductive polymer dispersion, and after simple stirring and drying, an aggregate with a dense conductive polymer film deposited on the surface can be obtained, that is, the conductive aggregate.
[0082] Step 3: Preparation of conductive cement mortar
[0083] The dry materials such as cement, fly ash, conductive aggregate and carbon fiber are dry mixed, and then mixing water is added, and then stirred at a low speed and then at a high speed to finally obtain a conductive cement mortar. Finally, four parallel electrode sheets are inserted into the conductive cement mortar to obtain a cement-based piezoresistive sensor.
[0084] The graphene is KY HE-1 type highly conductive graphene. The surfactant is a melamine aqueous solution, the dosage of which is 0.5 times that of the graphene. The solid content of the polystyrene sulfonic acid aqueous solution is 2%. The PVDF emulsion is Arkema PVDF Kynar Flex 2751 copolymer emulsion.
[0085] The dispersion process of "chemistry combined with physics" is as follows: firstly, the graphene surface is modified by using a melamine aqueous solution, and then treated by an ultrasonic cell disperser (power of 60W, ultrasonic time of 460min) under ice bath conditions to obtain a high-quality graphene dispersion. The graphene dispersion and polystyrene sulfonic acid aqueous solution are treated by an industrial ultrasonic instrument at an ultrasonic power of 180W for 40min. The dispersion process of the mixture and PVDF emulsion is as follows: first, hand-mix for 1min, then treat with an industrial ultrasonic instrument at an ultrasonic power of 180W for 40min, and finally obtain a well-dispersed conductive polymer dispersion.
[0086] The river sand has a particle size of 0.075-4.75 mm and a 24-hour water absorption rate of 0.9%. The river sand and the conductive polymer dispersion are mixed in a wide-mouthed basin and stirred by hand at a speed of about 30 r / min for 5 minutes; then placed in an oven and dried at 80°C for 48 hours. During the drying process, the sand is evenly stir-fried every 1-2 hours to prevent the conductive aggregates from sticking to each other.
[0087] The cement is preferably ordinary Portland cement (PO 42.5), the fly ash is used in an amount of 15% of the cement mass, and the carbon fiber is preferably chopped carbon fiber (3 mm) produced by Japan Tenax Company.
[0088] Among them, cement, fly ash, conductive aggregate and carbon fiber are stirred at an orbital speed of 57r / min for 1min, then water is added and stirred at a low speed (57r / min) for 3min, and then stirred at a high speed (115r / min) for 1min. The resulting mixture is poured into an oiled mold, subjected to 30s of high-frequency vibration (60Hz) for vibration compaction, and then placed in a standard curing room for curing. In addition, the water-cement ratio of the mixture is 0.40, the amount of graphene is 0.1% of the mass of the cementitious material (cement and fly ash), the amount of surfactant (melamine) is 0.05% of the mass of the cementitious material, and the amount of carbon fiber is 0.1% of the mass of the cementitious material. The specimen curing age is 28 days. When testing the electrical indicators, four electrode sheets are inserted in parallel when the fresh mixture is just poured into the mold.
[0089] Example 2
[0090] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, and the steps are basically the same as those in Embodiment 1, except that:
[0091] The amount of graphene used is 0.3% of the mass of the cementitious material (cement and fly ash), and the amount of the surfactant (melamine) used is 0.15% of the mass of the cementitious material.
[0092] Example 3
[0093] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, and the steps are basically the same as those in Embodiment 1, except that:
[0094] The amount of graphene used is 0.5% of the mass of the cementitious material (cement and fly ash), and the amount of the surfactant (melamine) used is 0.25% of the mass of the cementitious material.
[0095] Example 4
[0096] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, and the steps are basically the same as those in Embodiment 1, except that:
[0097] The amount of graphene used is 0.7% of the mass of the cementitious material (cement and fly ash), and the amount of the surfactant (melamine) used is 0.35% of the mass of the cementitious material.
[0098] Example 5
[0099] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, and the steps are basically the same as those in Embodiment 1, except that:
[0100] The amount of graphene used is 1.0% of the mass of the cementitious material (cement and fly ash), and the amount of the surfactant (melamine) used is 0.50% of the mass of the cementitious material.
[0101] Example 6
[0102] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, and the steps are basically the same as those in Embodiment 1, except that:
[0103] The length of the chopped carbon fiber is 6 mm.
[0104] Example 7
[0105] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, and the steps are basically the same as those in Embodiment 1, except that:
[0106] The length of the chopped carbon fiber is 10 mm.
[0107] Example 8
[0108] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, and the steps are basically the same as those in Embodiment 1, except that:
[0109] The amount of chopped carbon fiber added is 0.15% of the cementitious material.
[0110] Example 9
[0111] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, and the steps are basically the same as those in Embodiment 1, except that:
[0112] The amount of chopped carbon fiber added is 0.20% of the cementitious material.
[0113] Example 10
[0114] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, comprising the following steps:
[0115] Step 1: Preparation of Conductive Polymer Dispersion
[0116] The graphene and deionized water were manually mixed for 3 minutes and then dispersed by a "chemical combined with physical" process to obtain a highly dispersed graphene dispersion; then the graphene was evenly mixed with a polystyrene sulfonic acid aqueous solution under ultrasonic conditions; finally, the above mixture was mixed with a PVDF emulsion to obtain a conductive polymer dispersion.
[0117] Step 2: Conductive aggregate preparation
[0118] The river sand is soaked in the above conductive polymer dispersion, and after simple stirring and drying, an aggregate with a dense conductive polymer film deposited on the surface can be obtained, that is, the conductive aggregate.
[0119] Step 3: Preparation of conductive cement mortar
[0120] The dry materials such as cement, fly ash, conductive aggregate and carbon fiber are dry mixed, and then mixing water is added, and then stirred at a low speed and then at a high speed to finally obtain a conductive cement mortar. Finally, four parallel electrode sheets are inserted into the conductive cement mortar to obtain a cement-based piezoresistive sensor.
[0121] The graphene is KY HE-1 type highly conductive graphene. The surfactant is a melamine aqueous solution, the amount of which is 0.55 times the amount of graphene. The solid content of the polystyrene sulfonic acid aqueous solution is 2%. The PVDF emulsion is Arkema PVDF Kynar Flex 2751 copolymer emulsion.
[0122] The dispersion process of "chemistry combined with physics" is as follows: firstly, the graphene surface is modified by using a melamine aqueous solution, and then treated by an ultrasonic cell disperser (power of 60W, ultrasonic time of 460min) under ice bath conditions to obtain a high-quality graphene dispersion. The graphene dispersion and polystyrene sulfonic acid aqueous solution are treated by an industrial ultrasonic instrument at an ultrasonic power of 180W for 40min. The dispersion process of the mixture and PVDF emulsion is as follows: first, hand-mix for 1min, then treat with an industrial ultrasonic instrument at an ultrasonic power of 180w for 40min, and finally obtain a well-dispersed conductive polymer dispersion.
[0123] The river sand has a particle size of 0.075-4.75 mm and a 24-hour water absorption rate of 0.9%. The river sand and the conductive polymer dispersion are mixed in a wide-mouthed basin and stirred by hand at a speed of about 20 r / min for 7 minutes; then placed in an oven and dried at 70°C for 72 hours. During the drying process, the sand is evenly stir-fried every 1-2 hours to prevent the conductive aggregates from sticking to each other.
[0124] The cement is preferably ordinary Portland cement (PO 42.5), the fly ash is used in an amount of 15% of the cement mass, and the carbon fiber is preferably chopped carbon fiber (3 mm) produced by Japan Tenax Company.
[0125] Among them, cement, fly ash, conductive aggregate and carbon fiber are stirred at an orbital speed of 67r / min for 1min, then water is added and stirred at a low speed (67r / min) for 5min, and then stirred at a high speed (135r / min) for 3min. The obtained mixture is poured into an oiled mold, subjected to 30s of high-frequency vibration (60Hz) for vibration compaction, and then placed in a standard curing room for curing. In addition, the water-cement ratio of the mixture is 0.60, the amount of graphene is 0.1% of the mass of the cementitious material (cement and fly ash), the amount of surfactant (melamine) is 0.05% of the mass of the cementitious material, and the amount of carbon fiber is 0.1% of the mass of the cementitious material. The curing age of the specimen is 28 days. When testing the electrical indicators, four electrode sheets are inserted in parallel when the fresh mixture is just poured into the mold.
[0126] Comparative Example 1
[0127] This embodiment provides a method for preparing a conductive aggregate and cement-based piezoresistive sensor based on an interface coating design, and the steps are basically the same as those in Embodiment 1, except that:
[0128] No carbon fiber is added, only conductive aggregate is added.
[0129] Cement, conductive aggregate, silica fume and river sand were mechanically stirred at an orbital speed of 57 r / min for 1 min, and then a mixture of water and surfactant was added, first stirred at a low speed (57 r / min) for 3 min, and then stirred at a high speed (115 r / min) for 1 min. The resulting mixture was poured into an oiled mold, subjected to 30 s of high-frequency vibration (60 Hz) for vibration compaction, and then placed in a standard curing room for curing.
[0130] Comparative Example 2
[0131] A pure cement mortar is provided in this comparative example.
[0132] The cement and river sand were mechanically stirred at an orbital speed of 57 r / min for 1 min, and then a mixture of water and surfactant was added, first stirred at a low speed (57 r / min) for 3 min, and then stirred at a high speed (115 r / min) for 1 min. The resulting mixture was poured into an oiled mold, subjected to 30 s of high-frequency vibration (60 Hz) for vibration compaction, and then placed in a standard curing room for curing.
[0133] Comparative Example 3
[0134] This comparative example provides a cement mortar added with silica fume.
[0135] Cement, 15% silica fume (by cement mass) and river sand were mechanically stirred at an orbital speed of 57 r / min for 1 min, and then a mixture of water and surfactant was added, first stirred at a low speed (57 r / min) for 3 min, and then stirred at a high speed (115 r / min) for 1 min. The resulting mixture was poured into an oiled mold, subjected to 30 s of high-frequency vibration (60 Hz) for vibration compaction, and then placed in a standard curing room for curing.
[0136] Comparative Example 4
[0137] This comparative example provides a graphene-modified cement mortar.
[0138] Cement, 15% silica fume (by cement mass), 0.1% graphene and river sand were mechanically stirred at an orbital speed of 5 r / min for 1 min, and then a mixture of water and surfactant was added, first stirred at a low speed (57 r / min) for 3 min, and then stirred at a high speed (115 r / min) for 1 min. The resulting mixture was poured into an oiled mold, subjected to 30 s of high-frequency vibration (60 Hz) for vibration compaction, and then placed in a standard curing room for curing.
[0139] According to the requirements of GB / T8077-2012, the expansion index is used to characterize the fluidity of the mortar; according to the requirements of GB / T17671-1999, the compressive strength and flexural strength of the mortar specimens are tested. The size of the flexural strength test specimen is 40mm×40mm×160mm, and the cross-sectional area of the compressive strength test specimen is 40mm×40mm. The size of the specimen for resistivity and resistance change rate test is 40mm×40mm×160mm, and the four-electrode method is used for testing. Each performance index is tested three times in parallel, and the results are averaged.
[0140] The performance test results of the conductive aggregate and cement-based piezoresistive sensor based on the interface coating design provided in the above embodiment are shown in the following table:
[0141]
[0142]
[0143] Based on the above embodiments and test results, it can be clearly seen that the conductive aggregate and cement-based piezoresistive sensor preparation method based on the interface coating design provided by the present invention, the introduction of conductive aggregate forms a "conductive skeleton" structure inside the cement mortar, greatly improving the conductivity of the smart mortar (that is, reducing the resistivity), in addition, the conductive aggregate is linked by randomly distributed conductive carbon fibers to form a "three-dimensional conductive network structure", which further greatly increases the conductivity of the conductive cement mortar. Among them, the weakest interface transition zone (aggregate-cement paste interface) in the cement-based material is embedded in the middle of the conductive network, thereby increasing the sensitivity of the cement-based sensor (that is, the resistance change rate). In addition, graphene is coated on the surface of river sand in the form of a coating instead of being directly mixed with cement, thus avoiding the technical bottleneck of uneven dispersion (agglomeration) of graphene (carbon-based nanomaterials) in the cement matrix, thereby avoiding the adverse effects of direct addition of graphene on working performance and mechanical strength; finally, the introduction of ultrafine fly ash can not only reduce the amount of cement (reduce energy consumption and carbon emissions), optimize the system's microstructure, but also improve the fluidity of the system, thereby preparing conductive cement mortar with excellent performance.
[0144] Comparing Examples 1-5, it can be seen that the amount of graphene wrapped on the surface of river sand has little effect on the working performance, mechanical properties and electrical properties of the smart mortar. This is because the specific surface area of graphene is much larger than that of river sand. In this system, the amount of 0.1% of graphene in the cementitious material is sufficient to completely wrap the surface of river sand under the dispersion process of this technical solution, so increasing the amount of graphene has little effect on the performance of the smart mortar. Comparing Examples 1, 6 and 7, it can be seen that the length of the carbon fiber has a significant effect on the electrical properties of the smart mortar. This is mainly because at the same dosage, 3mm, 6mm and 10mm carbon fibers can all be connected to the conductive aggregate (the theoretical spacing of the conductive aggregate is about 100μm), so the shorter the carbon fiber, the greater the number at the same dosage, so the electrical performance of the smart mortar with 3mm carbon fiber is better. Comparing Example 1, Example 8 and Example 9, it can be seen that the amount of carbon fiber added has little effect on the electrical properties of the smart mortar. This is mainly because the "conductive aggregate" and a small amount of carbon fiber can reach the percolation threshold, so adding carbon fiber has little significance for improving the electrical properties. Comparing Example 1, Comparative Example 1 and Comparative Example 2, it can be seen that the introduction of conductive aggregate can reduce the resistivity by about 3 orders of magnitude, and the resistance change rate is increased by 60 times; and the use of conductive aggregate combined with a small amount of carbon fiber can reduce the resistivity of the smart mortar by 4 orders of magnitude, only 210Ω·cm, and the resistance change rate is increased by 167 times. Comparing Example 1, Comparative Example 3 and Comparative Example 4, it can be seen that compared with the smart mortar directly added with the conductive phase (graphene), the use of the present invention can avoid the adverse effects of directly adding graphene on the fluidity and mechanical strength of the mixture.
[0145] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0146] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A method for preparing a conductive aggregate, characterized in that: include: Mixing graphene and water for 1-3 minutes, modifying the surface of graphene with a surfactant, and ultrasonically dispersing the graphene under ice bath conditions to obtain a graphene dispersion, wherein the surfactant is melamine, and the mass ratio of the surfactant to the graphene is 0.50-0.55:1; Mixing a mixed system of graphene, polystyrene sulfonic acid and water in the graphene dispersion with a PVDF emulsion to form a conductive polymer dispersion, wherein the graphene is a highly conductive graphene; The river sand is immersed in the conductive polymer dispersion, and after stirring and drying, an aggregate with a dense conductive polymer film deposited on the surface is obtained, namely, conductive aggregate. The particle size of the river sand is 0.075-4.75 m.
2. The preparation method according to claim 1, characterized in that: The PVDF emulsion is Arkema Kynar Flex2751 copolymer emulsion.
3. The preparation method according to claim 1, characterized in that: The stirring speed is 20-30 r / min, and the stirring time is 5-7 min.
4. The preparation method according to claim 1, characterized in that: The drying temperature is 70-80°C and the drying time is 48-72 hours.
5. Conductive aggregate prepared by the preparation method according to any one of claims 1 to 4.
6. A method for preparing a smart cement composite material, characterized in that: include: Cement, fly ash, the conductive aggregate in claim 5 and carbon fiber are dry-mixed, and then water is added to mix to obtain an intelligent cement composite material containing conductive aggregate.
7. The method for preparing the smart cement composite material according to claim 6, characterized in that Specifically include: The mixed system including cement, fly ash, the conductive aggregate and carbon fiber is dry-mixed, and then water is added for mixing, and then stirred at a low speed and then at a high speed to obtain an intelligent cement composite material containing conductive aggregate.
8. The method for preparing the smart cement composite material according to claim 7, characterized in that: The rotation speed of the low-speed stirring is 57-67 r / min, and the stirring time is 3-5 min.
9. The method for preparing the smart cement composite material according to claim 7, characterized in that: The rotation speed of the high-speed stirring is 115-135 r / min, and the stirring time is 1-3 min.
10. The method for preparing the smart cement composite material according to claim 7, characterized in that: The water-to-binder ratio of the mixed system is 0.4-0.
6.
11. The method for preparing the smart cement composite material according to claim 7, characterized in that: The cement is selected from any one of silicate cement and sulphoaluminate cement or a combination of the two; And / or, the fly ash is ultrafine fly ash with a particle size of 5-10 μm and a strength activity index greater than 80%; And / or, the mass ratio of fly ash to cement is 10-15:100; And / or, the carbon fiber is selected from any one or a combination of two or more of chopped carbon fibers having a diameter of 7-9 μm and a length of 3 mm, 6 mm, or 10 mm; and / or, the mass of graphene in the conductive aggregate is 0.1-1.0% of the total mass of cement and fly ash; and / or, the mass of the surfactant in the conductive aggregate is 0.05-0.50% of the total mass of cement and fly ash; And / or, the mass of the carbon fiber is 0.1-0.2% of the total mass of cement and fly ash.
12. The smart cement composite material obtained by the preparation method according to any one of claims 6 to 11, wherein the thickness of the conductive aggregate coating film in the smart cement composite material is 6-8 nm.
13. A cement-based piezoresistive sensor, characterized in that: It is made of the smart cement composite material described in claim 12.
14. Application of the cement-based piezoresistive sensor according to claim 13 in the field of structural health monitoring of buildings, bridges or tunnels.
Citation Information
Patent Citations
Conductive aggregate preparation method and application thereof
CN114455874A