A nano composite coating resistant to flashover voltage and preparation method thereof
By using 5-10nm particle size titanium dioxide anatase nanoparticles and room temperature vulcanized silicone rubber on the surface of the insulator, a nanocomposite coating that resists flashover voltage is prepared, which solves the problem of insufficient electrical insulation performance of distribution line insulators and cable joints. , significantly improves flashover voltage resistance and hydrophobic performance, extends the service life of the insulator and reduces the failure rate.
Patent Information
- Application Number
- CN202310617919.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-05-29
AI Technical Summary
Distribution line insulators are prone to non-penetrating micro-loss defects in complex environments, resulting in frequent grounding failures. Cable connectors are a weak link in cable system failures. The existing technology is difficult to effectively identify and manage, affecting the safe and stable operation of the power grid.
Titanium dioxide anatase nanoparticles with particle size of 5-10nm combined with room temperature vulcanized silicone rubber, and are treated with isothermal ionic ion and modifiers γ-methacryloyloxypropyltrimethoxysilane or γ-aminopropyl Based on the modification of triethoxysilane, nanocomposite coatings that are resistant to flashover voltage are prepared to form hydrophobic, anti-fouling and high flashover resistance coatings.
It significantly improves the electrical insulation performance and mechanical strength of the insulator surface, increases the flashover voltage resistance, improves the hydrophobicity and adhesion properties of the coating, extends the service life of the insulator, and reduces operation and maintenance costs and failure rates.
Smart Images

Figure CN116463055B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, and in particular to a flashover voltage-resistant nano composite coating and a preparation method thereof. Background Art
[0002] Distribution line insulators can support conductors, prevent current from returning to the ground, and increase creepage distance. They can withstand voltage and mechanical stress and play an important role in overhead distribution lines. Affected by factors such as complex operating environment, the failure rate of distribution line insulators remains high, which has seriously affected the safe and stable operation of distribution lines. In particular, the non-penetrating micro-damage defects of insulators that are difficult to find through manual inspections often cause grounding faults frequently in lines in high humidity environments such as thunderstorms due to insufficient insulation creepage distance and insufficient withstand voltage. There is currently no effective identification and treatment method for such defects. It is often necessary to conduct segmented line inspections or even climb poles one by one to check. It takes a long time to find faults and is time-consuming and labor-intensive. At the same time, defective insulators are very easy to break down and cause line disconnection, which increases the difficulty of distribution network operation and maintenance and affects the safe and stable operation of the distribution network. In addition, with the continuous development of social economy, the construction level of urban power supply systems has been continuously improved, and power cables have gradually replaced overhead lines as the main form of delivery in urban distribution networks. In the power cable system, the cable joint (including the terminal head and the intermediate joint) is one of the weakest links. Statistics show that in the case of non-external force damage, the failure caused by the cable joint accounts for 80% of the cable system failures. Polymer insulating dielectrics are widely used as insulating materials for power equipment, and their performance largely determines the quality of power equipment. For high-voltage and ultra-high-voltage cables, with the development of smart grids based on ultra-high voltage power grids, the voltage level and capacity of power transmission and distribution equipment are constantly improving, and the working field strength of cable insulation is constantly increasing. The insulation failure and aging under the action of operating voltage, heat, mechanical force, etc. have become a hidden danger to the reliable operation of cables and an important source of endangerment to the safe operation of power grids.
[0003] Explore the technical solutions for modifying the surface components and surface morphology of insulators, improve the performance of insulators by modifying the surface of insulators, extend their service life, reduce the labor intensity of operation and maintenance personnel, and ensure safe and stable operation of the line. The insulation performance of cable joint materials is closely related to the surface state of the materials. The surface state of the material includes the characteristics of the material itself, surface flatness, degree of contamination, etc. In order to ensure the safe and stable operation of power cables and suppress the occurrence of surface flashover, researchers modify the insulating materials through plasma treatment, fluorination, surface coating and other methods. Among them, the coating technology can adjust the surface state of the insulating material as needed by changing the coating material. In addition, in the cable joints in actual engineering operation, the electrical performance of the outer sheath of the cable joint is improved by simple spraying technology, and the surface discharge is avoided to the greatest extent. It is more cost-saving and easier to prevent faults in advance, which greatly reduces the operating cost of the cable line.
[0004] In order to further improve the surface electrical insulation performance of distribution line insulators, enhance the mechanical strength and electrical insulation performance of silicone rubber, and make it meet the operating requirements, it is necessary to modify and strengthen the surface of the insulator or silicone rubber. Since the polymer nano-dielectric was proposed by Lewis in 1994, the research on dielectrics has shifted from traditional theory to nanoscale mesoscopic theory. Adding nanoscale inorganic fillers to the polymer matrix and then introducing special effects at the microscale inside the composite material will have a great impact on the macroscopic properties of the material. Due to the large specific surface area and high surface activity of nano-TiO2 particles, a small amount of doping can introduce a large number of interface areas into the composite material, significantly improving the electrical properties of the polymer matrix, such as improving the volume resistivity and breakdown strength of the matrix, as well as improving the mechanical properties and thermal stability of the material. However, the existing coatings with added titanium dioxide have poor pressure resistance and hydrophobicity, and cannot effectively improve the operating reliability of insulators and power cables. Summary of the invention
[0005] The purpose of the present invention is to further improve the surface electrical insulation performance of the distribution line insulator, and enhance the mechanical strength and electrical insulation performance of silicone rubber, and to propose a method for preparing a nano-composite coating with flashover voltage resistance. RTV power anti-pollution flashover coating is used as the base material, TiO2 nanoparticles are selected for doping, and different doping ratios are used to prepare the anti-pollution flashover composite coating material.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A nano composite coating resistant to flashover voltage comprises the following components in parts by weight:
[0008] Room temperature vulcanized silicone rubber 91-97 parts; titanium dioxide nanoparticles 3-9 parts, modifier 7-9 parts and solvent 20-35 parts;
[0009] The titanium dioxide nanoparticles are titanium dioxide anatase, and the particle size of the titanium dioxide anatase is 5-10 nm.
[0010] The design idea of the above technical solution is to select titanium dioxide anatase with an extremely small particle size range as the filler of the composite material, which can be evenly dispersed in the matrix material after modification. Compared with titanium dioxide with a particle size range of 500~800nm commonly used in the prior art, nanoparticles with small particle size are more likely to form hydrophobic, anti-fouling and highly flashover resistant materials. Experiments have found that the dispersion effects of nanoparticles with particle sizes of 25nm and 10nm are equivalent, and the flashover resistance voltage can reach 8.794kV, which is about 47.01% higher than the flashover voltage of general flashover resistant coatings and materials.
[0011] As a further preferred embodiment of the above technical solution, the modifier includes at least one of γ-methacryloxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane. Modifying the nanoparticles with γ-methacryloxypropyltrimethoxysilane or γ-aminopropyltriethoxysilane can make the surface of the nanoparticles hydrophobic, promote the dispersion of the nanoparticles in the matrix, and ensure the stability of the composite material performance.
[0012] As a further preferred embodiment of the above technical solution, the silicone rubber is room temperature vulcanized silicone rubber. As the base material of the coating, the room temperature vulcanized silicone rubber has a more suitable viscosity and curing time than other silicone rubbers.
[0013] As a further preferred embodiment of the above technical solution, the solvent includes at least one of anhydrous ethanol, methanol and acetone.
[0014] As a further preferred embodiment of the above technical solution, the flashover voltage resistant nanocomposite coating further includes 0.1 to 0.3 parts by mass of a pH adjuster, and the pH adjuster includes at least one of oxalic acid or hydrochloric acid.
[0015] Based on the same technical concept, the present invention also provides a method for preparing the above-mentioned nano-composite coating with flashover resistance, comprising the following steps:
[0016] (1) treating titanium dioxide nanoparticles with isothermal plasma for 0.5 to 2 minutes, adding the nanoparticles to a mixed solution of a solvent and deionized water, and stirring the mixture to obtain a mixed solution A;
[0017] (2) adding the modifier to the mixed solution A, stirring at 70-90° C. for 50-70 min, and drying at 90-110° C. for 12-24 h to obtain modified titanium dioxide nanoparticles;
[0018] (3) adding the modified titanium dioxide nanoparticles into a solvent, stirring and ultrasonically dispersing the mixture to obtain a mixed solution B;
[0019] (4) Add the mixed liquid B into the silicone rubber, stir evenly and then remove bubbles to obtain the nano-composite coating with flashover voltage resistance.
[0020] As a further preferred embodiment of the above technical solution, when the titanium dioxide nanoparticles are treated with plasma in step (1), the plasma treatment conditions are a sinusoidal voltage with an applied voltage of 1 kV and a frequency of 20 kHz under a nitrogen environment at room temperature.
[0021] As a further preferred embodiment of the above technical solution, in step (1), the stirring speed is 500-600 r / min, and the stirring time is 10-20 min.
[0022] As a further preferred embodiment of the above technical solution, in step (3), the stirring speed is 300-700 r / min, the stirring time is 20-30 min, and the ultrasonic time is 25-35 min.
[0023] As a further preferred embodiment of the above technical solution, the stirring operation in step (4) is: first, stirring at a stirring speed of 300-700 r / min for 10-15 min, and then stirring at a stirring speed of 500-900 r / min for 60-90 min.
[0024] As a further preferred embodiment of the above technical solution, in step (4), defoaming is achieved by ultrasonic cleaning, and the cleaning time is 20 to 30 minutes.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention adopts titanium dioxide anatase with a particle size of 5-10nm as a filler, and uses γ-methacryloxypropyltrimethoxysilane or γ-aminopropyltriethoxysilane as a modifier. The nanoparticles after surface modification have a hydrophobic surface and can be uniformly dispersed in a base material. Compared with the material with a titanium dioxide filler particle size of 500-800nm in the prior art, the coating formed by the coating of the present invention has good hydrophobic, anti-fouling and flashover resistance performance, and the flashover resistance voltage is generally 8.794kV, which is about 47.01% higher than the flashover voltage of a general flashover-resistant coating. Reasonable matching can provide long-term protection, and has excellent hydrophobicity and adhesion performance. According to tests, the static hydrophobic angle is improved by about 74.1° compared with the general flashover-resistant coating. In a tensile test, the coating and the base material are kept in good contact, without peeling or falling off, and have good anti-fouling, flame retardant and acid and alkali resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The preparation process of the nanocomposite coating is as follows:
[0028] Figure 2 is a SEM image of the coating formed by the composite coating of Examples 1 to 3 and Comparative Example 1;
[0029] Figure 3 It is a test diagram of the hydrophobic angle of the coating formed by the composite coating of Examples 1 to 3 and Comparative Example 1;
[0030] Figure 4 is a relative dielectric constant diagram of the coating formed by the composite coatings of Examples 1 to 3 and Comparative Example 1;
[0031] Figure 5 It is a surface potential decay diagram of the coating formed by the composite coating of Examples 1 to 3 and Comparative Example 1. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below in conjunction with specific embodiments.
[0033] Embodiment 1:
[0034] The composite coating for flashover voltage resistance of the present embodiment comprises the following components in parts by weight:
[0035] 97 parts of room temperature vulcanized silicone rubber, 35 parts of solvent, 3 parts of titanium dioxide nanoparticles, 0.03 parts of pH adjuster, and 9 parts of modifier; wherein the solvent is anhydrous ethanol, the titanium dioxide nanoparticles are titanium dioxide anatase with a particle size of 10 nm, the pH adjuster is oxalic acid, and the modifier is γ-methacryloxypropyltrimethoxysilane.
[0036] The preparation method of the composite coating with flashover voltage resistance of this embodiment is as follows: Figure 1 As shown, the following steps are included:
[0037] (1) After titanium dioxide nanoparticles were treated with isothermal plasma for 1 min, they were added to a solvent and a deionized water solution and stirred at a constant speed of 500 r / min for 20 min to obtain a mixed solution A; the plasma treatment conditions were a sinusoidal voltage of 1 kV and 20 kHz under room temperature nitrogen environment;
[0038] (2) Add the modifier to the mixed solution A, stir at 80°C and 300 r / min for 60 min, return to room temperature, and dry in an oven at 100°C for 24 h to obtain modified titanium dioxide nanoparticles;
[0039] (3) adding the modified titanium dioxide nanoparticles into the solvent, stirring uniformly at 300 r / min for 20 min, and ultrasonically dispersing for 30 min to obtain a mixed solution B;
[0040] (4) Add the mixed solution B to the room temperature vulcanized silicone rubber, stir at a constant speed of 300 r / min for 10 min, then increase the speed to 500 r / min and stir at a constant speed for 1 h. After that, ultrasonic cleaning is performed for 30 min to remove bubbles, thereby obtaining the flashover voltage resistant composite coating of the present embodiment.
[0041] Comparative Example 1:
[0042] The difference between the composite coating of this comparative example and Example 1 is that the composite coating of this comparative example does not add titanium dioxide nanoparticles and modifiers, and the other components and addition amounts are consistent with those of Example 1.
[0043] The preparation method of the composite coating of this comparative example is different from that of Example 1 in that the preparation method of the composite coating of this comparative example does not include steps (1) to (3) related to titanium dioxide nanoparticles and modifiers.
[0044] Comparative Example 2:
[0045] The difference between the composite coating of this comparative example and Example 1 is that the addition amount of titanium dioxide nanoparticles in the composite coating of this comparative example is 1 part by mass, and the other components, addition amounts and preparation method of the composite coating are consistent with those in Example 1.
[0046] Comparative Example 3:
[0047] The composite coating of this comparative example is compared with Example 1, except that in the preparation method of the composite coating of this comparative example, the titanium dioxide nanoparticles are not treated with low-temperature plasma before being added to the solvent and deionized water solution, and the other components, addition amounts and preparation method of the composite coating are consistent with Example 1.
[0048] Comparative Example 4:
[0049] The difference between the composite coating of this comparative example and Example 1 is that no modifier is added to the composite coating of this comparative example, and the other components, addition amounts and preparation method of the composite coating are consistent with those of Example 1.
[0050] Comparative Example 5:
[0051] The composite coating of this comparative example is compared with Example 1, except that in the preparation method of the composite coating of this comparative example, the titanium dioxide nanoparticles are treated with low-temperature plasma for 10 minutes before being added to the solvent and deionized water solution, and the other components, addition amounts and preparation method of the composite coating are consistent with Example 1.
[0052] Comparative Example 6:
[0053] The difference between the composite coating of this comparative example and Example 1 is that the particle size of the titanium dioxide nanoparticles in the composite coating of this comparative example is 100 nm, and the other components, addition amounts and preparation method of the composite coating are consistent with those in Example 1.
[0054] Comparative Example 7:
[0055] The difference between the composite coating of this comparative example and Example 1 is that the particle size of the titanium dioxide nanoparticles in the composite coating of this comparative example is 1 μm, and the other components, addition amounts and preparation method of the composite coating are consistent with those in Example 1.
[0056] The flashover voltage resistant composite coating of Example 1 and the composite coatings of each comparative example were dried at room temperature for 48 hours to form a coating, and the coating properties were tested. The results are shown in Table 1. The results show that the coating formed by the composite coating of the present invention has good pressure resistance, hydrophobicity and thermal stability.
[0057] Table 1: Test results of composite coating properties of Example 1 and comparative examples
[0058] Sample composition <![CDATA[Particle diameter of TiO2]]> Plasma treatment time Modifier addition Breakdown voltage / kV Hydrophobic angle a / degree Comparative Example 1 No Additive —— —— —— 15.9 104 Comparative Example 2 <![CDATA[1 part of TiO2]]> 10nm 1min Add to 16.63 110 Comparative Example 3 <![CDATA[3 parts of TiO2]]> 10nm Unprocessed Add to 18.12 142 Comparative Example 4 <![CDATA[3 parts of TiO2]]> 10nm 1min Not added 17.75 135 Example 1 <![CDATA[3 parts of TiO2]]> 10nm 1min Add to 19.93 141 Comparative Example 5 <![CDATA[3 parts of TiO2]]> 10nm 10min Add to 18.32 130 Comparative Example 6 <![CDATA[3 parts of TiO2]]> 100nm 1min Add to 16.54 119 Comparative Example 7 <![CDATA[3 parts of TiO2]]> 1 micron 1min Add to 15.32 110
[0059] Embodiment 2:
[0060] The composite coating for flashover voltage resistance of the present embodiment comprises the following components in parts by weight:
[0061] 95 parts of room temperature vulcanized silicone rubber, 8 parts of modifier, 6 parts of titanium dioxide nanoparticles, 25 parts of solvent and 0.2 parts of pH adjuster; wherein the solvent is acetone, the titanium dioxide nanoparticles are selected as titanium dioxide anatase with a particle size of 10 nm, the pH adjuster is oxalic acid, and the modifier is γ-methacryloxypropyltrimethoxysilane.
[0062] The preparation method of the composite coating with flashover voltage resistance of the present embodiment comprises the following steps:
[0063] (1) After titanium dioxide nanoparticles were treated with isothermal plasma for 1 min, they were added to a solvent and a deionized water solution and stirred at a constant speed of 500 r / min for 20 min to obtain a mixed solution A; the plasma treatment conditions were a sinusoidal voltage of 1 kV and 20 kHz under room temperature nitrogen environment;
[0064] (2) Add the modifier to the mixed solution A, stir at 80°C and 300 r / min for 60 min, return to room temperature, and dry in an oven at 100°C for 24 h to obtain modified titanium dioxide nanoparticles;
[0065] (3) adding the modified titanium dioxide nanoparticles into the solvent, stirring uniformly at 500 r / min for 20 min, and ultrasonically dispersing for 30 min to obtain a mixed solution B;
[0066] (4) Add the mixed solution B to the room temperature vulcanized silicone rubber, stir at a constant speed of 500 r / min for 10 min, then adjust the speed to 800 r / min and stir for 1.5 h. Then, ultrasonically clean the mixture for 30 min to remove bubbles, thereby obtaining the flashover voltage resistant composite coating of the present embodiment.
[0067] Comparative Example 8:
[0068] The difference between the composite coating of this comparative example and Example 2 is that the addition amount of titanium dioxide nanoparticles in the composite coating of this comparative example is 1 part by mass, and the other components, addition amounts and preparation method of the composite coating are consistent with those in Example 2.
[0069] Comparative Example 9:
[0070] The composite coating of this comparative example is compared with Example 2, except that in the preparation method of the composite coating of this comparative example, the titanium dioxide nanoparticles are not treated with low-temperature plasma before being added to the solvent and deionized water solution, and the other components, addition amounts and preparation method of the composite coating are consistent with Example 2.
[0071] Comparative Example 10:
[0072] The difference between the composite coating of this comparative example and Example 2 is that no modifier is added to the composite coating of this comparative example, and the other components, addition amounts and preparation method of the composite coating are consistent with those of Example 2.
[0073] Comparative Example 11:
[0074] The composite coating of this comparative example is compared with Example 2, except that in the preparation method of the composite coating of this comparative example, the titanium dioxide nanoparticles are treated with low-temperature plasma for 10 minutes before being added to the solvent and deionized water solution, and the other components, addition amounts and preparation method of the composite coating are consistent with Example 2.
[0075] Comparative Example 12:
[0076] The difference between the composite coating of this comparative example and Example 2 is that the particle size of the titanium dioxide nanoparticles in the composite coating of this comparative example is 100 nm, and the other components, addition amounts and preparation method of the composite coating are consistent with those of Example 2.
[0077] Comparative Example 13:
[0078] The difference between the composite coating of this comparative example and Example 2 is that the particle size of the titanium dioxide nanoparticles in the composite coating of this comparative example is 1 μm, and the other components, addition amounts and preparation method of the composite coating are consistent with those of Example 2.
[0079] The flashover voltage resistant composite coating of Example 2 and the composite coatings of each comparative example were dried at room temperature for 48 hours to form a coating, and the coating properties were tested. The results are shown in Table 2. The results show that the coating formed by the composite coating of the present invention has good pressure resistance, hydrophobicity and thermal stability.
[0080] Table 2: Test results of composite coating properties of Example 2 and comparative examples
[0081]
[0082] Embodiment 3:
[0083] The composite coating for flashover voltage resistance of the present embodiment comprises the following components in parts by weight:
[0084] 91 parts of room temperature vulcanized silicone rubber, 35 parts of solvent, 9 parts of titanium dioxide nanoparticles, 0.3 parts of pH adjuster, and 9 parts of modifier; wherein the solvent is acetone, the titanium dioxide nanoparticles are titanium dioxide anatase with a particle size of 25 nm, the pH adjuster is hydrochloric acid, and the modifier is γ-aminopropyltriethoxysilane.
[0085] The preparation method of the composite coating with flashover voltage resistance of the present embodiment comprises the following steps:
[0086] (1) After titanium dioxide nanoparticles were treated with isothermal plasma for 1 min, they were added to a solvent and a deionized water solution and stirred at a constant speed of 500 r / min for 20 min to obtain a mixed solution A; the plasma treatment conditions were a sinusoidal voltage of 1 kV and 20 kHz under room temperature nitrogen environment;
[0087] (2) Add the modifier to the mixed solution A, stir at 90°C and 500 r / min for 50 min, return to room temperature, and dry in an oven at 100°C for 24 h to obtain modified titanium dioxide nanoparticles;
[0088] (3) adding the modified titanium dioxide nanoparticles into the solvent, stirring uniformly at 500 r / min for 20 min, and ultrasonically dispersing for 30 min to obtain a mixed solution B;
[0089] (4) Add the mixed solution B to the room temperature vulcanized silicone rubber, stir at a constant speed of 500 r / min for 10 min, then adjust the speed to 800 r / min and stir at a constant speed for 1 h. Then, ultrasonically clean the mixture for 30 min to remove bubbles, thereby obtaining the flashover voltage resistant composite coating of this embodiment.
[0090] Comparative Example 14:
[0091] The difference between the composite coating of this comparative example and Example 3 is that the addition amount of titanium dioxide nanoparticles in the composite coating of this comparative example is 1 part by mass, and the other components, addition amounts and preparation method of the composite coating are consistent with those of Example 3.
[0092] Comparative Example 15:
[0093] The composite coating of this comparative example is compared with Example 3, except that in the preparation method of the composite coating of this comparative example, the titanium dioxide nanoparticles are not treated with low-temperature plasma before being added to the solvent and deionized water solution, and the other components, addition amounts and preparation method of the composite coating are consistent with Example 3.
[0094] Comparative Example 16:
[0095] The difference between the composite coating of this comparative example and Example 3 is that no modifier is added to the composite coating of this comparative example, and the other components, addition amounts and preparation method of the composite coating are consistent with those of Example 3.
[0096] Comparative Example 17:
[0097] The composite coating of this comparative example is compared with Example 3, except that in the preparation method of the composite coating of this comparative example, the titanium dioxide nanoparticles are treated with low-temperature plasma for 10 minutes before being added to the solvent and deionized water solution, and the other components, addition amounts and preparation method of the composite coating are consistent with Example 3.
[0098] Comparative Example 18:
[0099] The difference between the composite coating of this comparative example and Example 3 is that the particle size of the titanium dioxide nanoparticles in the composite coating of this comparative example is 100 nm, and the other components, addition amounts and preparation method of the composite coating are consistent with those of Example 3.
[0100] Comparative Example 19:
[0101] The difference between the composite coating of this comparative example and Example 3 is that the particle size of the titanium dioxide nanoparticles in the composite coating of this comparative example is 1 μm, and the other components, addition amounts and preparation method of the composite coating are consistent with those of Example 3.
[0102] The flashover voltage resistant composite coating of Example 3 and the composite coatings of each comparative example were dried at room temperature for 48 hours to form a coating, and the coating properties were tested. The results are shown in Table 3. The results show that the coating formed by the composite coating of the present invention has good pressure resistance, hydrophobicity and thermal stability.
[0103] Table 3: Test results of composite coating properties of Example 3 and comparative examples
[0104]
[0105] The coatings formed by the composite coatings of Examples 1-3 and Comparative Example 1 were tested, and their SEM images are shown in FIG. Figure 2 As shown ( Figure 2 a, b, c, d are the characterization results of Examples 1-3 and Comparative Example 1, respectively), the hydrophobicity test results are as follows Figure 3 As shown ( Figure 3 a, b, c, d are the characterization results of Examples 1-3 and Comparative Example 1, respectively), the relative dielectric constant test results are as follows Figure 4 The surface potential decay results are shown in Figure 5 shown.
[0106] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. For those skilled in the art, improvements and changes obtained without departing from the technical concept of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a nano-composite coating with flashover resistance, characterized in that: The nano composite coating with flashover voltage resistance comprises the following components in parts by mass: 91-97 parts of silicone rubber, 3-6 parts of titanium dioxide nanoparticles, 7-9 parts of modifier and 20-35 parts of solvent; The titanium dioxide nanoparticles are titanium dioxide anatase, and the particle size of the titanium dioxide anatase is 5-10 nm; the modifier includes one or two of γ-methacryloxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane; the silicone rubber is room temperature vulcanized silicone rubber; The preparation method comprises the following steps: (1) Titanium dioxide nanoparticles were treated with low-temperature plasma for 0.5 to 2 minutes, and then added to a mixed solution of a solvent and deionized water, and stirred to obtain a mixed solution A; the plasma treatment conditions were a sinusoidal voltage of 1 kV and 20 kHz under a nitrogen environment at room temperature; (2) adding the modifier to the mixed solution A, stirring at 70-90° C. for 50-70 min, and drying at 90-110° C. for 12-24 h to obtain modified titanium dioxide nanoparticles; (3) adding the modified titanium dioxide nanoparticles into a solvent, stirring and ultrasonically dispersing the mixture to obtain a mixed solution B; (4) Add the mixed liquid B into the silicone rubber, stir evenly and then remove bubbles to obtain the nano-composite coating with flashover voltage resistance.
2. The method for preparing the nano-composite coating with flashover voltage resistance according to claim 1, characterized in that: The solvent includes at least one of anhydrous ethanol, methanol and acetone.
3. The method for preparing the nano-composite coating with flashover resistance according to claim 1, characterized in that: The flashover voltage-resistant nanocomposite coating further comprises 0.1 to 0.3 parts by mass of a pH regulator, wherein the pH regulator comprises at least one of oxalic acid or hydrochloric acid.
4. The method for preparing the nano-composite coating with flashover voltage resistance according to claim 1, characterized in that: In step (1), the stirring speed is 500-600 r / min and the stirring time is 18-25 min.
5. The method for preparing the flashover voltage resistant nanocomposite coating according to claim 1, characterized in that: In step (3), the stirring speed is 300-500 r / min, the stirring time is 18-25 min, the ultrasonic frequency is 40 kHz, and the ultrasonic time is 25-35 min.
6. The method for preparing the nano-composite coating with flashover voltage resistance according to claim 1, characterized in that: The stirring operation in step (4) is: first, stirring at a stirring speed of 300-500 r / min for 10-15 min, and then stirring at a stirring speed of 500-800 r / min for 60-90 min.
Citation Information
Patent Citations
Anti-pollution flashover organosilicon coating and preparation method thereof
CN101575482A
Anti-pollution flashover coating for electrical equipment and preparation method of anti-pollution flashover coating
CN109796873A
RTV anti-pollution flashover coating as well as preparation method and application thereof
CN115746701A
Eco-heavy duty coating system with high weatherability A method for preventing contamination
KR100867682B1