A carbon-modified Zr-based mesoporous SiO 2 Nanosphere catalyst and its preparation method and application

By preparing carbon-modified Zr-based mesoporous SiO2 nanosphere catalysts, the problems of numerous byproducts and low stability in the ethanol-to-butadiene process were solved, achieving butadiene production with high selectivity and high conversion rate, which is suitable for industrial application.

CN116474756BActive Publication Date: 2024-11-15DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211582536.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-11-15
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

Existing technologies for producing butadiene from ethanol suffer from problems such as numerous byproducts, insufficient selectivity, and low stability. In particular, the two-step process produces a large number of dehydration and condensation byproducts, leading to decreased reaction selectivity and low stability.

Method used

A carbon-modified Zr-based mesoporous SiO2 nanosphere catalyst was developed. By loading Zr as the active component and utilizing the carbon-modified mesoporous SiO2 nanosphere structure, the generation of by-products was reduced, and the selectivity and conversion rate of butadiene were improved. The reaction stability can reach more than 200 h.

Benefits of technology

It achieves butadiene production with high selectivity and high conversion rate, and the catalyst has better stability than existing technologies, low cost, and is suitable for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116474756B_ABST
    Figure CN116474756B_ABST
Patent Text Reader

Abstract

The present invention relates to a carbon-modified Zr-based mesoporous SiO2 nanosphere catalyst and a preparation method and application thereof, and belongs to the technical field of preparing butadiene from ethanol and acetaldehyde. The catalyst is represented by the formula Zr / NMSS-C, wherein Zr is an active component, NMSS-C is a carrier, and the total loading amount of Zr in the catalyst is 0.5-30wt%; the NMSS-C is a carbon-modified mesoporous silica nanosphere structure. The catalyst is applied to the reaction of preparing butadiene from ethanol and acetaldehyde, can achieve high activity, high selectivity, high stability of ethanol and acetaldehyde, generate the target product butadiene, and has significant advantages such as low cost and easy preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a carbon-modified Zr-based mesoporous SiO 2 The invention discloses a nanosphere catalyst and a preparation method and application thereof, belonging to the technical field of preparing butadiene from ethanol and acetaldehyde. Background Art

[0002] 1,3-Butadiene is a very important chemical raw material. Together with ethylene and propylene, it is called "triene" in the chemical industry. It is widely used in the preparation of various chemical products, including synthetic rubber, synthetic resin, etc. [Tong Liu, Liu Zongzhang, Zhang Minhua. Research Progress of Preparation of 1,3-Butadiene by Ethanol Method [J]. Chemical Industry and Engineering, 2012, 29(04): 38-44.], and its downstream products are widely used in the automotive, medical and building materials industries. In recent years, due to the increasing demand for synthetic rubber, the demand for butadiene has reached 16 million tons / year, and is growing at a rate of 4% per year.

[0003] At present, the preparation of butadiene is mainly obtained by extracting the C4 byproduct of naphtha cracking to produce ethylene, accounting for 97% of the total output, which leads to the fact that the output of butadiene is largely dependent on the output of ethylene [Xu Churong. Research Progress of Butadiene Synthesis Technology in my country [J]. Fine and Specialty Chemicals, 2022, 30(08):10-12.]. In recent years, due to the development of MTO technology and the large-scale application of shale gas technology, the source of ethylene has become more abundant. The diversification of ethylene sources has reduced the demand for traditional naphtha cracking technology, thereby reducing the output of butadiene. In addition, since naphtha cracking technology relies on non-renewable petroleum resources, this method is also not in line with the dual-carbon national policy. Therefore, we urgently need to find a sustainable and green butadiene production route, namely, ethanol to butadiene technology [Liu Zongzhang, Zhang Tong, Xu Yuchao, Jiang Haoxi, Zhang Minhua. Preparation and catalytic performance of MgO / SBA-15 catalyst for ethanol to 1,3-butadiene [J]. Applied Chemistry, 2019, 36(02): 176-181.].

[0004] The technology of producing butadiene from ethanol has a long history. As early as 1915, Ostromyslensky used ethanol acetaldehyde as raw materials and a catalyst with a dehydration function to synthesize butadiene. The technology of producing butadiene from ethanol was the main process for industrial production of butadiene before World War II, which ensured the large-scale synthesis of important strategic material rubber [Tian Yuan, Shan Yuhua, Shi Jun, Wan Yu, Feng Yangyang, Zheng Yitian. The influence of catalyst preparation method on the synthesis of 1,3-butadiene from ethanol [J]. Modern Chemical Industry, 2016, 36(07): 104-108.]. In the 1960s, with the advancement of oil extraction technology, naphtha cracking technology has made great progress, greatly increasing the production of butadiene, and the method of extracting butadiene from the by-product of C4 fraction has become popular all over the world. At present, the production of butadiene from C4 fraction still accounts for 97% of the global share. Until 2011, due to the continuous rise in oil prices, the increasing depletion of fossil fuel resources, and people's in-depth understanding of the concept of green sustainable development, people gradually shifted the focus of energy utilization to renewable resources. The technology of ethanol to butadiene has a chance to revive.

[0005] Ethanol, as a green and sustainable energy source, can be extracted from abundant biomass. In recent years, coal-to-ethanol projects have also achieved industrial production. Therefore, using abundant ethanol as raw material to prepare butadiene will be a process route with broad prospects and in line with the dual carbon goals of carbon peak and carbon neutrality [Pomalaza, G.; Arango Ponton, P.; Capron, M.; Dumeignil, F., Ethanol-to-butadiene: the reaction and its catalysts. Catal. Sci. Techn., 2020, 10, 4860-4911.].

[0006] There are two types of ethanol-to-butadiene production processes, namely the one-step process and the two-step process. The one-step process refers to using only ethanol as the raw material to produce butadiene in one step. The two-step process refers to using ethanol and acetaldehyde as co-feed to produce butadiene. The two-step process has higher stability because it does not contain a dehydrogenation center, but it will inevitably produce more dehydration and condensation by-products, resulting in a decrease in reaction selectivity. At present, the maximum stability of this reaction is only 168 hours, and there is still room for further improvement. Summary of the invention

[0007] The purpose of the present invention is to provide a carbon-modified Zr-based mesoporous SiO 2 Nanosphere catalyst and its preparation method and its application in the two-step preparation of butadiene from ethanol and acetaldehyde. 2Nanospheres are prepared and loaded with Zr to reduce the production of by-products. At the same time, higher butadiene selectivity and conversion rate are obtained, and the reaction can run stably for more than 200 hours.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] On the one hand, the present invention provides a carbon-modified Zr-based mesoporous SiO 2 The nanosphere catalyst is represented by the formula Zr / NMSS-C, wherein Zr is an active component, NMSS-C is a carrier, and the total loading amount of Zr in the catalyst is 0.5-30wt%; the NMSS-C is a carbon-modified mesoporous silica nanosphere structure.

[0010] In the above technical solution, further, the NMSS-C carrier is SiO 2 The nanospheres are stacked, the diameter of the silica nanospheres is 10-100nm, and the diameter of the stacked mesopores is 2-50nm.

[0011] In the above technical solution, further, the loading amount of Zr in the catalyst is 1-25wt%; the diameter of the silica nanospheres is 20-50nm, and the size of the accumulated mesopores is 5-40nm.

[0012] Another aspect of the present invention provides the above-mentioned carbon-modified Zr-based mesoporous SiO 2 The preparation method of the nanosphere catalyst is characterized in that: a soluble salt solution of Zr is impregnated into a NMSS-C carrier, dried at 60-200°C, and then calcined in an inert atmosphere at a calcination temperature of 350-750°C, preferably 500-700°C, and a calcination time of 2-8h, preferably 2-6h, to obtain the catalyst Zr / NMSS-C.

[0013] In the above technical solution, further, the soluble salt of Zr is one or more of zirconium nitrate, zirconium chloride, zirconium oxynitrate, zirconium oxychloride, and zirconium n-propoxide.

[0014] In the above technical solution, further, the preparation method of the NMSS-C carrier comprises the following steps:

[0015] (1) Using oil and water phase solvents, dissolving the template in the water phase solvent, adding organic amines as catalysts, heating to 45-80°C and stirring for 0.5-2h;

[0016] (2) adding a silicon source dissolved in an oil phase solvent to the mixed solution obtained in step (1), stirring at 60-90° C. for 8-20 h, removing the upper oil phase, and then heating to 80-110° C. and stirring for aging for 2-4 h;

[0017] (3) The solid product obtained in step (2) is centrifuged and washed, and dried at 60-120° C., and then calcined at 200-450° C. for 1-4 h under an inert gas or air atmosphere to obtain a black solid, which is the NMSS-C.

[0018] In the above technical solution, further, the organic amine catalyst is one or more of ethanolamine, diethanolamine and triethanolamine;

[0019] The template agent is one or more of cetyltrimethylammonium chloride (CTAC), cetyltrimethylammonium bromide (CTAB), P123, P105, and F127;

[0020] The silicon source is one or more of tetraethyl orthosilicate, silica sol, and fumed silica;

[0021] The oil phase solvent is one or more of cyclohexane, 1-octadecene and decalin.

[0022] In another aspect, the present invention provides an application of the above catalyst in the reaction of ethanol and acetaldehyde to butadiene, characterized in that: the reaction is carried out in a fixed bed reactor at atmospheric pressure, the molar ratio of acetaldehyde to ethanol is 1:1-1:5, preferably 1:1-1:3, and the reaction space velocity is WHSV=0.12-10h -1 , preferably WHSV = 0.25-6h -1 , using inert gas as carrier gas, carrier gas space velocity GSHV = 500-10000h -1 , preferably 3000-5000h -1 , the reaction temperature is 200-500°C, preferably 300-400°C.

[0023] In the above technical solution, further, the inert gas is one or more of nitrogen, argon and helium.

[0024] The beneficial effects of the present invention are:

[0025] (1) The present invention uses cheap metal zirconium as the active component, which is cheaper than other tantalum-based and hafnium-based catalysts.

[0026] (2) The synthesis cycle of NMSS-C in the present invention is short, the process is relatively simple, and it is easy to produce in large quantities. At the same time, the template agent in the preparation process is cheaper than the template agents of other molecular sieves, and the industrialization cost is lower.

[0027] (3) The catalyst of the present invention has high reaction stability, which is superior to the currently reported Zr / deAl-beta, Zr / SBA-15 and Zr / SiO 2 etc. catalysts.

[0028] (4) Under the conditions of preferred space velocity and temperature, the conversion rate of ethanol and acetaldehyde on the preferred catalyst is as high as 90% or more, and the selectivity is above 85%.

[0029] (5) The Zr / NMSS-C catalyst has high butadiene selectivity in the reaction of ethanol and acetaldehyde to butadiene. Under the optimized reaction conditions, the butadiene selectivity is as high as 85% or more. Taking the above factors into consideration, the catalyst of the present invention has a good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The adsorption isotherms and pore size distribution diagrams of 8% Zr / NMSS-C and 16% Zr / NMSS-C, where a is the adsorption isotherm diagram and b is the pore size distribution diagram;

[0031] Figure 2 This is the SEM image of 8% Zr / NMSS-C;

[0032] Figure 3 XRD pattern of 8% Zr / NMSS-C;

[0033] Figure 4 This is the stability investigation result of 8% Zr / NMSS-C;

[0034] Figure 5 This is the stability investigation result of 8% Zr / deAl-beta;

[0035] Figure 6 8% Zr / SiO 2 Stability test results. DETAILED DESCRIPTION

[0036] The following is further detailed description through specific embodiments.

[0037] Example 1

[0038] Preparation of Zr / NMSS-C catalysts with different loading amounts:

[0039] (1) Preparation of NMSS-C vector:

[0040] Step A, add 96 mL of hexadecyltrimethylammonium chloride (CTAC) aqueous solution (25 wt%) to 144 mL of ultrapure water, then add 0.72 g of triethanolamine (TEA), and stir evenly;

[0041] Step B, transfer the resulting solution to a 500 mL round-bottom flask and slowly stir in a 60 °C oil bath for 1 h;

[0042] Step C, slowly add 80 mL of ethyl orthosilicate / cyclohexane (20 vol / vol%) solution into the above solution, and stir continuously for 12 h in an oil bath at 75°C;

[0043] Step D, completely remove the cyclohexane solution in the upper oil phase, and heat to 90° C. for aging for 3 h;

[0044] Step E, washing the solid product by centrifugation for several times, and drying in an oven at 80° C. overnight;

[0045] Step F, calcining at 300°C for 2h in an air atmosphere at 20mL / min to obtain a black solid, represented by NMSS-C;

[0046] (2) Preparation of X% Zr / NMSS-C catalysts with different loading amounts by impregnation method:

[0047] Step a, dissolving zirconium oxynitrate in water, and impregnating the same volume with the above mesoporous NMSS-C carrier, the loading amount of Zr is selected as 1%, 2%, 4%, 8%, 12%, 16%, respectively, and drying at 100° C. for 8 hours;

[0048] Step b, calcining the above samples at 550°C, 20 mL / min argon atmosphere for 4 h to obtain catalysts with different loading amounts, namely 1% Zr / NMSS-C, 2% Zr / NMSS-C, 4% Zr / NMSS-C, 8% Zr / NMSS-C, 12% Zr / NMSS-C, and 16% Zr / NMSS-C.

[0049] The adsorption isotherms and pore size distributions of 8% Zr / NMSS-C and 16% Zr / NMSS-C prepared in Example 1 are shown in Figure 1 As shown, the SEM and XRD patterns of 8% Zr / NMSS-C are shown in Figure 2 , Figure 3 shown.

[0050] from Figure 1 N 2 The physical adsorption results show that Zr / NMSS-C exhibits a type IV isotherm with an H1-type hysteresis loop, which is a typical mesoporous structure. Figure 2 The SEM results show that the catalyst is composed of 10-30nm silica spheres, and its mesoporous structure (average pore size of 16nm) is mainly derived from SiO 2 The accumulation hole. Figure 3 The XRD results show that the active component Zr is evenly distributed on the carrier, and no obvious ZrO 2 Characteristic peak.

[0051] The pore structure properties of 8% Zr / NMSS-C and 16% Zr / NMSS-C are shown in Table 1.

[0052] Table 1 Pore structure properties of 8% Zr / NMSS-C and 16% Zr / NMSS-C

[0053]

[0054] Example 2

[0055] Preparation of 8% Zr / NMSS-C catalysts at different calcination temperatures: The preparation process is similar to that of Example 1, except that the calcination temperatures are 300°C, 400°C, 550°C, and 700°C.

[0056] Comparative Example 1

[0057] Preparation of X% Zr / NMSS catalysts with different loading amounts:

[0058] (1) Preparation of NMSS vector:

[0059] The preparation process is similar to that of Example 1, except that the solid obtained by drying overnight in Example 1 is calcined in air at 650° C. for 2 h to obtain a white solid, represented by NMSS;

[0060] (2) Preparation of X% Zr / NMSS catalysts with different loading amounts by impregnation method:

[0061] Step a, dissolving zirconium oxynitrate in water, and impregnating it with the above mesoporous NMSS carrier in equal volumes, with the loading amounts of Zr being 1%, 2%, 4%, 8%, 12%, and 16%, respectively, and drying at 100° C. for 8 hours.

[0062] Step b, calcining the above sample at 550° C. in air atmosphere for 4 hours to obtain catalysts with different loading amounts, namely 4% Zr / NMSS, 8% Zr / NMSS, and 16% Zr / NMSS.

[0063] Comparative Example 2

[0064] Preparation of Zr-based catalysts with different types of carriers: The preparation process is similar to that of Example 1, except that the carrier is replaced with deAl-beta, SBA-15 and nano-SiO 2 .

[0065] Test Example 1

[0066] Evaluation process of catalyst for preparing butadiene from ethanol and acetaldehyde: 0.25 g of the catalyst prepared in Example 1 above was pelletized and loaded into a fixed bed reactor, and the raw materials were brought into the reactor by pump feeding and carrier gas (flow rate of 20 mL / min). The ratio of the amount of ethanol and acetaldehyde in the reaction material was 2:1, and the reaction space velocity was WHSV=0.38 h -1 , the reaction temperature is 350℃.

[0067] Reaction conversion and selectivity calculation method:

[0068] Ethanol conversion rate (%) = (n 反应前的乙醇 -n 反应后剩余乙醇 ) / n 反应前的乙醇 *100%

[0069] Acetaldehyde conversion rate (%) = (n 反应前的乙醛 -n 反应后剩余乙醛 ) / n 反应前的乙醛 *100%

[0070] Total conversion rate (%) = (n 反应前的乙醇和乙醛 -n 反应后剩余乙醇和乙醛 ) / n 反应前的乙醇和乙醛 *100%

[0071] Butadiene selectivity (%) = 2n 产物中丁二烯 / (n 反应前的乙醇和乙醛 -n 反应后剩余乙醇和乙醛 )*100%

[0072] The performance of the Zr / NMSS-C catalyst with different loading amounts in Example 1 was evaluated, and the results are shown in Table 2.

[0073] Table 2 Performance evaluation results of Zr / NMSS-C catalysts with different loadings

[0074]

[0075] It can be seen from the reaction results that when the Zr loading is 8-16%, it has relatively good catalytic performance, among which the active component Zr loading has better catalytic performance when it is 8%, and the butadiene yield can reach more than 80%.

[0076] Test Example 2

[0077] The performance of the Zr / NMSS catalyst with different loading amounts in Comparative Example 1 was evaluated. The reaction conditions were the same as those in Test Example 1. The test results are shown in Table 3.

[0078] Table 3 Performance evaluation results of Zr / NMSS catalysts with different loadings

[0079]

[0080] It can be seen from Table 3 that at the same Zr loading, the conversion rate and butadiene selectivity of the Zr / NMSS-C of the present invention are higher than those of the catalyst without carbon modification, which illustrates the uniqueness and excellence of the present invention.

[0081] Test Example 3

[0082] The catalytic performance of the 8% Zr / NMSS-C catalyst prepared at different calcination temperatures in Example 2 was investigated, and the reaction conditions were the same as those in Test Example 1.

[0083] Table 4 Catalytic performance evaluation results of 8% Zr / NMSS-C catalysts prepared at different calcination temperatures

[0084]

[0085] It can be seen from the table that the catalyst provided by the present invention can stably exist and produce the target product butadiene under the condition of a calcination temperature of 300-700°C, and the optimal calcination temperature for the reaction is 550°C.

[0086] Test Example 4

[0087] The catalytic performance of 8% Zr / NMSS-C catalyst at different reaction temperatures was investigated. The reaction conditions were similar to those in Test Example 1. The results are shown in Table 5.

[0088] Table 5 Evaluation results of catalytic performance of 8% Zr / NMSS-C catalyst at different reaction temperatures

[0089]

[0090] It can be seen from Table 5 that the catalyst provided by the present invention can produce the target product butadiene under the reaction conditions of 250-400°C, and the optimal reaction temperature is 350°C.

[0091] Test Example 5

[0092] The catalytic performance of 8% Zr / NMSS-C catalyst at different ethanol-acetaldehyde ratios was investigated. The reaction conditions were similar to those in Test Example 1. The results are shown in Table 6.

[0093] Table 6 Evaluation results of catalytic performance of 8% Zr / NMSS-C catalyst at different ethanol-acetaldehyde ratios

[0094]

[0095] Test Example 6

[0096] The catalytic performance of 8% Zr / NMSS-C catalyst at different reaction space velocities was investigated. The reaction conditions were similar to those in Test Example 1. The results are shown in Table 7.

[0097] Table 7 Evaluation results of catalytic performance of 8% Zr / NMSS-C catalyst at different reaction space velocities

[0098]

[0099] It can be seen from the data in Table 6 and Table 7 that the catalyst provided by the present invention can produce the target product butadiene under the reaction conditions of the aldehyde-alcohol ratio range of 1:1-1:3. When the aldehyde-alcohol ratio is 1:2, the reaction space velocity WHSV=0.38h -1 When , a better catalytic effect can be achieved.

[0100] Test Example 7

[0101] In Test Example 1, the optimal Zr loading is 8%. To further highlight the superiority of the present invention, catalysts with the same Zr loading but different carriers are compared, including 8% Zr / SiO 2 , 8% Zr / deAl-beta and 8% Zr / SBA-15. The reaction conditions were the same as those in Test Example 1. The results are shown in Table 8.

[0102] Table 8 Comparison of catalyst evaluation performance of different carriers

[0103]

[0104] From the results in the table, it can be seen that the catalytic effect of the catalyst 8% Zr / NMSS-C of the present invention in the reaction is significantly better than the catalysts with outstanding catalytic performance reported so far, which shows that the patent of the present invention has unique innovation and superiority.

[0105] Test Case 8

[0106] Comparison of catalyst stability:

[0107] The stability of the catalytic performance of 8% Zr / NMSS-C and other catalysts under the optimal reaction conditions was investigated. The reaction conditions were the same as those in Test Example 1. The results of the stability investigation of 8% Zr / NMSS-C are shown in Figure 4 As shown, the stability test results of 8% Zr / deAl-beta are as follows Figure 5 As shown, 8% Zr / SiO 2 The stability test results are as follows Figure 6 shown.

[0108] 8% Zr / NMSS-C can run stably for more than 200 hours, with a slight decrease in conversion rate and basically unchanged selectivity. Compared with the molecular sieve 8% Zr / deAl-beta with better reaction results reported so far, it has higher stability and butadiene yield, and is better than ordinary 8% Zr / SiO 2 The reaction performance advantage is more obvious.

[0109] In summary, the carbon-modified zirconium-based mesoporous SiO prepared by the air-assisted low-temperature carbonization surfactant template strategy in the present invention 2 Nanosphere catalysts can be used for the reaction of ethanol and acetaldehyde to butadiene. They have the advantages of good activity, high butadiene selectivity, good stability, and low cost. They can also be produced in large quantities and are easy to apply industrially.

Claims

1. A carbon-modified Zr-based mesoporous SiO2 nanosphere catalyst, characterized in that: The catalyst is represented by the formula Zr / NMSS-C, wherein Zr is an active component, NMSS-C is a carrier, and the total loading amount of Zr in the catalyst is 0.5-16 wt %; the NMSS-C is a carbon-modified mesoporous silica nanosphere structure; The preparation method of the NMSS-C carrier comprises the following steps: (1) Using oil and water phase solvents, dissolve the template in the water phase solvent, add organic amines as catalysts, heat to 45-80︒C and stir for 0.5-2 h; (2) Add the silicon source dissolved in the oil phase solvent to the mixed solution obtained in step (1), stir at 60-90°C for 8-20 h, remove the upper oil phase, and then heat to 80-110°C, stir and age for 2-4 h; (3) The solid product obtained in step (2) is washed by centrifugation, dried at 60-120°C, and then calcined at 200-450°C for 1-4 h under an inert gas or air atmosphere to obtain a black solid, which is the NMSS-C.

2. The catalyst according to claim 1, characterized in that: The NMSS-C carrier is formed by stacking SiO2 nanospheres with carbon wrapped on the outer surface. The diameter of the silicon dioxide nanospheres is 10-100 nm, and the pore size of the stacked mesopores is 2-50 nm.

3. The catalyst according to claim 1, characterized in that: The diameter of silica nanospheres is 20-50 nm, and the size of the accumulated mesopores is 5-40 nm.

4. The catalyst according to claim 1, characterized in that: The organic amine is one or more of ethanolamine, diethanolamine and triethanolamine; The template agent is one or more of cetyltrimethylammonium chloride (CTAC), cetyltrimethylammonium bromide (CTAB), P123, P105, and F127; The silicon source is one or more of tetraethyl orthosilicate, silica sol, and fumed silica; The oil phase solvent is one or more of cyclohexane, 1-octadecene and decalin.

5. A method for preparing the carbon-modified Zr-based mesoporous SiO2 nanosphere catalyst according to any one of claims 1 to 4, characterized in that: The soluble salt solution of Zr is impregnated into the NMSS-C carrier and then o After drying at 350-750 °C, the product is calcined in an inert atmosphere. o C, and the calcination time is 2-8 h to obtain the catalyst Zr / NMSS-C.

6. The preparation method according to claim 5, characterized in that: The soluble salt of Zr is one or more of zirconium nitrate, zirconium chloride, zirconium oxynitrate, zirconium oxychloride, and zirconium n-propoxide; The calcination temperature is 500-700 o C, the calcination time is 2-6 h.

7. The preparation method according to claim 5, characterized in that: The calcination temperature is 200-400 o C, the calcination time is 1-4h.

8. Use of the catalyst according to any one of claims 1 to 4 or the catalyst prepared by the preparation method according to any one of claims 5 to 7 in the reaction of ethanol and acetaldehyde to butadiene, characterized in that: The reaction is carried out in a fixed bed reactor at atmospheric pressure, the molar ratio of acetaldehyde to ethanol is 1:1-1:5, and the reaction space velocity range is WHSV=0.12-10 h -1 , using inert gas as carrier gas, carrier gas space velocity GSHV = 500-10000 h -1 , reaction temperature is 300-400 o C.