A tandem catalyst composed of precious metals and molecular sieves for efficient purification of multi-component VOCs
Through the combination of series catalysts, PtSn/CeO2 is prepared by solvothermal synthesis method and MnOx/HZSM-5 is prepared by impregnation method to form PtSn/CeO2&MnOx/HZSM-5 catalyst, which solves the problem of catalyst deactivation in multi-component VOCs treatment and achieves It efficiently catalyzes the oxidation of toluene and trichlorethylene, significantly improving catalytic activity and stability.
Patent Information
- Application Number
- CN202310409567.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Existing technology is difficult to effectively treat complex multi-component volatile organic compounds (VOCs) exhaust gases, especially chlorine-containing VOCs, resulting in catalyst deactivation, and the application of series catalysts in this field has not yet been reported.
PtSn nanoparticles were prepared by solvothermal synthesis and loaded on CeO2, combined with the impregnation method to prepare MnOx/HZSM-5 catalyst, and combined in series to form PtSn/CeO2&MnOx/HZSM-5 catalyst, which was used to catalyze the oxidation of toluene and trichlorethylene. .
It achieves efficient catalytic oxidation of toluene and trichlorethylene, significantly improves catalytic activity and stability, reduces reaction temperature, and is suitable for the treatment of multi-component VOCs.
Smart Images

Figure HDA0004182807890000011 
Figure HDA0004182807890000021 
Figure HDA0004182807890000031
Abstract
Description
Technical Field
[0001] The present invention relates to a platinum-based catalyst and a HZSM-5 type molecular sieve catalyst in series and a preparation method thereof, belonging to the field of catalysis. Specifically, it relates to preparing PtSn nanoparticles by a solvent thermal synthesis method, loading the PtSn nanoparticles onto CeO2 by an adsorption method, and then calcining to form a PtSn / CeO2 catalyst, and preparing MnO2 by an impregnation method. x / HZSM-5 catalyst, PtSn / CeO2 and MnO x / HZSM-5 catalysts are combined in series to finally obtain PtSn / CeO2&MnO x / HZSM-5 catalyst, which has a good effect on the co-catalytic oxidation of toluene and trichloroethylene. Background Art
[0002] With the development of industrial technology, a large amount of industrial waste gas is discharged into the atmosphere, so air pollution control is particularly important. At present, the relevant research on volatile organic compounds (VOCs) waste gas treatment technology has become a hot spot in the field of environmental protection. Among the many methods for treating VOCs, catalytic oxidation is considered to be one of the most effective methods because of its low energy consumption and no secondary pollution. The key to this method is to develop a catalyst with good low-temperature oxidation activity, high-temperature stability and low price. In different industries, the emission sources and characteristics of VOCs are different. Emission pollutants are often discharged in the form of multiple components, and chlorine-containing VOCs (CVOCs) will not degrade naturally, but will accumulate on the catalyst surface, poisoning the catalyst and causing deactivation. Therefore, for actual industry, the stability, recyclability and activity of the catalyst are of higher significance for handling complex multi-component gases. Platinum-based catalysts (loaded noble metal catalysts) are conducive to the formation of intermediate active species, and have the characteristics of high catalytic activity, good selectivity, and long service life. They have outstanding catalytic performance in the catalytic oxidation of alkanes, aromatic hydrocarbons, and CO. However, noble metals are expensive, easy to sinter at high temperatures, and easily deactivated by chlorine poisoning. Usually, one or several non-noble metals are doped to reduce costs and improve performance. For the catalytic oxidation of CVOCs, a commonly used type is molecular sieve catalysts. HZSM-5 molecular sieve, as a typical solid acid, has a special pore structure that makes it have a certain selectivity for the product and the presence of rich acid centers. It is very useful for highly selective catalysis, but its own oxidation ability is insufficient, resulting in more by-products. By introducing other metal elements, the surface acid properties of the molecular sieve can be adjusted and the deep oxidation ability of the catalyst for the intermediate products can be improved. Supported catalysts have been widely used in industry, and better reaction activity, selectivity, and stability can be obtained by adjusting the composition and interface of metal nanoparticles and oxide carriers. Since tandem catalysts have multiple reaction interfaces, single catalysts can be coupled in series and used to catalyze continuous reactions, thereby improving product selectivity and solving the uncontrollability of the reaction. They have outstanding advantages in synthetic routes, but their application in eliminating multi-component VOCs has not yet been reported.
[0003] At present, a lot of research has been done on the catalytic oxidation of toluene or trichloroethylene at home and abroad, and some results have been achieved. Peng et al. (PengRuosi, et al., Chemical Engineering Journal, 2016, 306: 1234-1246) prepared Pt / nanorod CeO2 catalyst by hydrothermal method for catalytic oxidation of toluene. 90%About 150°C. Zhang et al. (Zhang Xing, et al., Applied Catalysis B: Environmental, 2019, 257: 117879) used the template method and NaBH4 reduction method to prepare 2.85AuPd 1.87 / 3DOM CeO2 catalyst for catalytic oxidation of trichloroethylene, the reaction T 90% It is 415℃.
[0004] As far as we know, there is no literature or patent report on utilizing the advantages of relay catalysis to synthesize PtSn / CeO2 and MnO x Study on the catalytic oxidation of mixed VOCs of toluene and trichloroethylene by series coupling of / HZSM-5 catalysts. Summary of the invention
[0005] The present invention is to prepare PtSn nanoparticles by solvent thermal method, load them on CeO2 by adsorption method, and form supported PtSn / CeO2 catalyst by calcination, wherein the loading amount of Pt is 1wt%. x / HZSM-5 catalyst, the above two catalysts are coupled in series to finally form PtSn / CeO2&MnO x / HZSM-5 catalyst.
[0006] The above-mentioned tandem catalyst is characterized in that the prepared PtSn nanocrystals have uniform size, and the MnO x Uniform dispersion, its preparation mainly includes the following steps:
[0007] (1) Preparing PtSn nanoparticles by solvothermal method: Weighing platinum acetylacetonate, stannous chloride dihydrate, polyvinyl pyrrolidone, and N,N-dimethylformamide, stirring and dissolving at room temperature for 20 minutes to form a precursor solution, loading the precursor solution into a reactor, and reacting at 180°C for 12 hours; cooling the reacted solution to room temperature and placing it into a centrifuge tube, adding acetone and ethanol to wash 3-4 times, to obtain PtSn bimetallic nanoparticles, especially Pt3Sn nanoparticles; uniformly dispersing the obtained PtSn nanoparticles into ethanol for storage; preferably, 0.008 mmol of stannous chloride dihydrate, 80 mg of polyvinyl pyrrolidone, and 6 mL of N,N-dimethylformamide are used for every 0.025 mmol of platinum acetylacetonate;
[0008] (2) The particles obtained in the above step (1) are loaded on CeO2 by an adsorption method, and calcined to obtain a PtSn / CeO2 bimetallic catalyst and a Pt / CeO2 catalyst. The specific steps are as follows:
[0009] A certain amount of CeO2 carrier is placed in an ethanol solution containing PtSn, stirred for 12 hours, centrifuged, and dried to obtain a catalyst; the catalyst is placed in a tubular furnace and calcined at 550°C for 2 hours to obtain a supported PtSn / CeO2 bimetallic catalyst; preferably, the loading amount of the Pt element is 1wt%;
[0010] (3) Preparation of HZSM-5 carrier by ion exchange method: weigh commercial molecular sieve ZSM-5 with Si:Al molar ratio of 38 and dissolve it in excess NH4NO3 aqueous solution (NH4NO3 concentration 1 mol / L, 30 mL NH4NO3 aqueous solution for each gram of commercial molecular sieve ZSM-5), carry out ion exchange reaction at 80°C for 6 hours, dry to obtain solid powder, repeat the above steps 4-5 times, put the dried solid powder into a muffle furnace, and calcine at 550°C for 6 hours to obtain HZSM-5 carrier;
[0011] (4) Preparation of MnO by impregnation method x / HZSM-5 catalyst, a certain amount of Mn(NO3)2·4H2O and the HZSM-5 carrier obtained in step (3) were mixed in ethanol, stirred continuously for 10 hours, placed in an oven and dried at 80°C for 10 hours, and the dried powder was placed in a muffle furnace and calcined at 550°C for 5 hours to obtain MnO x / HZSM-5 catalyst, preferably with a theoretical Mn metal loading of 12.0 wt%.
[0012] (5) For the tandem catalyst system, a column is used, the first stage catalyst is PtSn / CeO2, and the second stage catalyst is MnO x / ZSM-5, the two-stage catalysts have the same mass in the reactor, and a small amount of quartz wool is placed between the two layers to separate the two catalysts. The final tandem catalyst is PtSn / CeO2&MnO x / HZSM-5. PtSn / CeO2 and MnO x / ZSM-5 catalyst spacing is no greater than 5 cm, preferably 1 cm.
[0013] The catalyst obtained by the present invention is used for the catalytic oxidation of mixed VOCs of toluene and trichloroethylene, and finally obtains carbon dioxide and water; according to the direction of air flow, it first passes through PtSn / CeO2 and then MnO x / HZSM-5. The temperature of the catalytic reaction is generally greater than 319°C, more preferably greater than or equal to 384°C.
[0014] Under the reaction conditions of toluene concentration of 1000ppm, trichloroethylene concentration of 200ppm, (toluene + trichloroethylene) / oxygen molar ratio of 1 / 400 and space velocity of 40000mL / (gh), the catalyst T 50%-Tol(reaction temperature required when toluene conversion reaches 50%), T 90%-Tol (reaction temperature required when toluene conversion reaches 90%), T 50%-TCE (reaction temperature required for trichloroethylene conversion to reach 50%) and T 90%-TCE (The reaction temperature required when the trichloroethylene conversion rate reaches 90%) is 258°C, 296°C, 319°C and 384°C respectively.
[0015] The invention has the characteristics of novel preparation method and simple preparation process. The advantage of the invention is that different catalysts are connected together by series coupling, PtSn / CeO2&MnO x / HZSM-5 catalyst has excellent catalytic activity for the oxidation of toluene and trichloroethylene, and has good application prospects in the field of multi-component VOCs catalytic oxidation.
[0016] The crystal structure of the obtained catalyst and its catalytic oxidation activity on toluene and trichloroethylene were determined by using instruments such as D8 ADVANCE X-ray diffractometer (XRD) and Shimadzu GC-2014 gas chromatograph (GC). The results show that each sample prepared by the method of the present invention has good crystallinity, and the catalytic oxidation activity of the tandem catalyst on toluene and trichloroethylene is significantly improved compared with the single-stage catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The schematic diagram of the prepared tandem catalyst. In the figure, (A), (B) and (C) are PtSn / CeO2&MnO x / ZSM-5, PtSn / CeO2 and MnO x Schematic diagram of ZSM-5 catalyst.
[0018] Figure 2 The XRD spectra of the prepared catalysts. Curves (a) and (b) are the XRD spectra of Pt and PtSn nanoparticles (NPs), respectively, and (c), (d) and (e) are the XRD spectra of Pt / CeO2, PtSn / CeO2 and MnO x / XRD spectrum of HZSM-5 catalyst.
[0019] Figure 3 The prepared PtSn / CeO2&MnO x / ZSM-5 and comparative samples PtSn / CeO2 and MnO x / Activity curve of ZSM-5 catalyst for catalytic oxidation of xylene. Reaction conditions: 1000ppm toluene + 200ppm trichloroethylene + 40vol% oxygen + nitrogen (balance gas), space velocity 40000mL / (gh). DETAILED DESCRIPTION
[0020] In order to further illustrate the present invention, the following embodiments are described in detail, but the present invention is not limited to the following embodiments.
[0021] Example 1
[0022] (1) Preparation of PtSn nanoparticles by solvothermal method: Add materials according to the molar ratio of metal Pt and Sn of 3:1. Weigh platinum acetylacetonate, stannous chloride dihydrate, polyvinyl pyrrolidone, and N,N-dimethylformamide, stir and dissolve at room temperature for 20 minutes to form a precursor solution, which is loaded into a reactor and reacted at 180°C for 12 hours; the reaction solution is cooled to room temperature and placed in a centrifuge tube, and acetone and ethanol are added to wash 3-4 times to obtain PtSn bimetallic nanoparticles. The prepared PtSn nanoparticles are evenly dispersed in 5mL of ethanol for storage. Preferably, for every 0.025mmol of platinum acetylacetonate, 0.008mmol of stannous chloride dihydrate, 80mg of polyvinyl pyrrolidone, and 6mL of N,N-dimethylformamide are used.
[0023] (2) The particles obtained in the above (1) are loaded on CeO2 by an adsorption method, and then calcined to obtain a PtSn / CeO2 bimetallic catalyst. The specific steps are as follows:
[0024] A certain amount of CeO2 carrier was placed in an ethanol solution containing PtSn, stirred for 12 hours, centrifuged, and dried to obtain a catalyst. The catalyst was placed in a tubular furnace and calcined at 550°C for 2 hours to obtain a supported PtSn / CeO2 bimetallic catalyst.
[0025] (3) Preparation of HZSM-5 carrier by ion exchange method: Weigh commercial molecular sieve ZSM-5 with Si:Al ratio of 38 and dissolve it in an excess of NH4NO3 (1 mol / L, 30 mL / g) aqueous solution. After ion exchange reaction at 80°C for 6 h, dry it to obtain a solid powder. Repeat the above steps 4-5 times. Put the dried solid powder into a muffle furnace and calcine it at 550°C for 6 h to obtain a HZSM-5 carrier.
[0026] (4) Preparation of MnO by impregnation method x / HZSM-5 catalyst, the theoretical metal loading is 12.0wt%. A certain amount of Mn(NO3)2·4H2O was mixed with the HZSM-5 carrier obtained in (3) in ethanol, stirred continuously for 10h, placed in an oven and dried at 80℃ for 10h, and the dried powder was placed in a muffle furnace and calcined at 550℃ for 5h to obtain MnO x / HZSM-5 catalyst.
[0027] For the tandem catalyst system, the first stage catalyst is PtSn / CeO2 and the second stage catalyst is MnOx / ZSM-5, the two-stage catalysts have the same mass in the reactor, and a small amount of quartz wool is placed between the two layers to separate the two catalysts, and finally PtSn / CeO2&MnO x / ZSM-5 tandem catalyst.
[0028] Under the reaction conditions of toluene concentration of 1000ppm, trichloroethylene concentration of 200ppm, (toluene + trichloroethylene) / oxygen molar ratio of 1 / 400 and space velocity of 40000mL / (gh), the catalyst T 90%-Tol (reaction temperature required for toluene conversion to reach 90%) and T 90%-TCE (The reaction temperature required when the trichloroethylene conversion rate reaches 90%) is 296°C and 384°C respectively, and the oxidation products are carbon dioxide and water.
[0029] Example 2 (Comparative Example)
[0030] (1) Preparation of Pt nanoparticles by solvothermal method: Weigh platinum acetylacetonate, polyvinyl pyrrolidone, and N,N-dimethylformamide, stir and dissolve at room temperature for 20 minutes to form a precursor solution, which is then placed in a reactor and reacted at 180°C for 12 hours; the resulting solution is cooled to room temperature and placed in a centrifuge tube, and washed 3-4 times with acetone and ethanol to obtain Pt nanoparticles. The obtained Pt nanoparticles are uniformly dispersed in 5 mL of ethanol for storage. Preferably, 80 mg of polyvinyl pyrrolidone and 6 mL of N,N-dimethylformamide are used for every 0.025 mmol of platinum acetylacetonate.
[0031] (2) The particles obtained in the above step (1) are loaded on CeO2 by an adsorption method, and then calcined to obtain a Pt / CeO2 catalyst. The specific steps are as follows:
[0032] A certain amount of CeO2 carrier was placed in an ethanol solution containing Pt nanoparticles, stirred for 12 hours, centrifuged, and dried to obtain a catalyst. The catalyst was placed in a tubular furnace and calcined at 550°C for 2 hours to obtain a supported Pt / CeO2 catalyst.
[0033] (5) Preparation of HZSM-5 carrier by ion exchange method: Weigh commercial molecular sieve ZSM-5 with Si:Al ratio of 38 and dissolve it in an excess of NH4NO3 (1 mol / L, 30 mL / g) aqueous solution. After ion exchange reaction at 80°C for 6 h, dry it to obtain a solid powder. Repeat the above steps 4-5 times. Put the dried solid powder into a muffle furnace and calcine it at 550°C for 6 h to obtain a HZSM-5 carrier.
[0034] (6) Preparation of MnO by impregnation method x / HZSM-5 catalyst, the theoretical metal loading is 12.0wt%. A certain amount of Mn(NO3)2·4H2O was mixed with the HZSM-5 carrier obtained in (3) in ethanol, stirred continuously for 10h, placed in an oven and dried at 80℃ for 10h, and the dried powder was placed in a muffle furnace and calcined at 550℃ for 5h to obtain MnO x / HZSM-5 catalyst.
[0035] For the tandem catalyst system, the first stage catalyst is Pt / CeO2 and the second stage catalyst is MnO x / ZSM-5, the two-stage catalysts have the same mass in the reactor, and a small amount of quartz wool is placed between the two layers to separate the two catalysts. The final tandem catalyst is Pt / CeO2&MnO x / ZSM-5
[0036] Under the reaction conditions of toluene concentration of 1000ppm, trichloroethylene concentration of 200ppm, (toluene + trichloroethylene) / oxygen molar ratio of 1 / 400 and space velocity of 40000mL / (gh), the catalyst T 90%-Tol (reaction temperature required for toluene conversion to reach 90%) and T 90%-TCE (The reaction temperature required when the trichloroethylene conversion rate reaches 90%) is 316°C and 443°C respectively, and the oxidation products are carbon dioxide and water.
Claims
1. A method for preparing a series catalyst composed of a noble metal and a molecular sieve, characterized in that: The following steps are involved: (1) Preparation of PtSn nanoparticles by solvothermal method: platinum acetylacetonate, stannous chloride dihydrate, polyvinyl pyrrolidone, and N, N-dimethylformamide were weighed and dissolved under stirring at room temperature for 20 min to form a precursor solution, which was then placed in a reactor and reacted at 180°C for 12 h; the resulting solution was cooled to room temperature and placed in a centrifuge tube, and washed 3-4 times with acetone and ethanol to obtain PtSn bimetallic nanoparticles; the obtained PtSn nanoparticles were uniformly dispersed in ethanol for storage; (2) The particles obtained in the above step (1) are loaded on CeO2 by an adsorption method, and then calcined to obtain a PtSn / CeO2 bimetallic catalyst; (3) Preparation of HZSM-5 carrier by ion exchange method: weigh commercial molecular sieve ZSM-5 with Si:Al molar ratio of 38 and dissolve it in excess NH4NO3 aqueous solution. After ion exchange reaction at 80℃ for 6 h, dry it to obtain solid powder. Repeat the above steps 4-5 times. Put the dried solid powder into a muffle furnace and calcine it at 550℃ for 6 h to obtain HZSM-5 carrier. (4) Preparation of MnO by impregnation method x / HZSM-5 catalyst, a certain amount of Mn(NO3)2·4H2O and the HZSM-5 carrier obtained in step (3) were mixed in ethanol, stirred continuously for 10 h, placed in an oven and dried at 80°C for 10 h, and the dried powder was placed in a muffle furnace and calcined at 550°C for 5 h to obtain MnO x / HZSM-5 catalyst; (5) For the tandem catalyst system, a column is used, the first catalyst is PtSn / CeO2, and the second catalyst is MnO x / ZSM-5, the two-stage catalysts have the same mass in the reactor, and a small amount of quartz wool is placed between the two layers to separate the two catalysts. The final tandem catalyst is PtSn / CeO2& MnO x / HZSM-5; PtSn / CeO2 and MnO x / ZSM-5 catalyst spacing is no greater than 5cm.
2. The method according to claim 1, characterized in that Step (1) For every 0.025 mmol of platinum acetylacetonate, there are 0.008 mmol of stannous chloride dihydrate, 80 mg of polyvinyl pyrrolidone, and 6 mL of N, N-dimethylformamide.
3. The method according to claim 1, characterized in that Step (2): Place a certain amount of CeO2 carrier in an ethanol solution containing PtSn, stir for 12 h, centrifuge, and dry to obtain a catalyst; place the catalyst in a tubular furnace and calcine at 550°C for 2 h to obtain a supported PtSn / CeO2 bimetallic catalyst: the loading amount of Pt element is 1 wt%.
4. The method according to claim 1, characterized in that The concentration of NH4NO3 in step (3) is 1 mol / L, and each gram of commercial molecular sieve ZSM-5 corresponds to 30 mL of NH4NO3 aqueous solution.
5. The method according to claim 1, characterized in that Step (4), the theoretical Mn metal loading is 12.0 wt%.
6. The method according to claim 1, characterized in that Step (5) PtSn / CeO2 and MnO x / ZSM-5 catalyst spacing is 1 cm.
7. The method according to claim 1, characterized in that The PtSn bimetallic nanoparticles in step (1) are Pt3Sn nanoparticles.
8. A catalyst prepared according to the method described in any one of claims 1 to 7.
9. Use of the catalyst prepared by the method according to any one of claims 1 to 7 for catalytic oxidation of mixed VOCs of toluene and trichloroethylene to finally obtain carbon dioxide and water; according to the direction of air flow, first pass through PtSn / CeO2 and then MnO x / HZSM-5.
10. The use according to claim 9, wherein the temperature of the catalytic reaction is greater than 319°C.
11. The use according to claim 9, wherein the temperature of the catalytic reaction is greater than or equal to 384°C.
12. The use according to claim 9, under the reaction conditions of a toluene concentration of 1000 ppm, a trichloroethylene concentration of 200 ppm, a (toluene + trichloroethylene) / oxygen molar ratio of 1 / 400 and a space velocity of 40000 mL / (g∙h).
Citation Information
Patent Citations
Gas-solid photocatalytic oxidation of environmental pollutants
CA2045517A1
Two-stage catalytic degradation method for low-concentration VOCs
CN110935309A
Supported platinum-tin bimetallic catalyst for efficient oxidation and purification of p-xylene
CN111545199A
Preparation method and application of Ru / 3DOM SnO2 catalyst with good stability
CN112547059A
Preparation of Mn-Ce-Sb / hierarchical porous ZSM-5 catalyst and low-temperature denitration application thereof
CN113769777A