Preparation method of polycrystalline diamond tool with embedded thin film thermocouple array

By integrating an embedded thin-film thermocouple array on the polycrystalline diamond tool, the problem of traditional contact temperature measurement technology being difficult to accurately measure transient temperature is solved, and high-precision, fast-response temperature measurement is achieved, which is suitable for a variety of processing and drilling. scene.

CN116475418BActive Publication Date: 2024-10-01HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310479246.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-01
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

Traditional contact temperature measurement technology is difficult to accurately measure the transient temperature value of polycrystalline diamond tools, and it will cause damage to the processing of the tool, and there are problems of error and thermal conduction delay in low or high temperature environments.

Method used

Using embedded thin film thermocouple array technology, the thermocouple material is deposited on the cutting edge of the polycrystalline diamond tool, connected through conductive silver glue and deposited with an insulating layer to form a high-precision temperature measurement system that can integrate a large number of thermoelectrics at the tool tip. The couples form an array to accurately measure the cutting edge-workpiece interface temperature and heat flow distribution.

Benefits of technology

It achieves high-precision, fast-response temperature measurement, avoids tool damage, and maintains efficient work in different environments. It is suitable for a variety of processing and drilling scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116475418B_ABST
    Figure CN116475418B_ABST
Patent Text Reader

Abstract

The preparation method of a polycrystalline diamond tool with an embedded thin film thermocouple array is to solve the problem that the thermocouple is too far away from the tool tip in the traditional contact temperature measurement of polycrystalline diamond tools and it is difficult to obtain an accurate transient temperature value. Preparation method: 1. Processing multiple shallow grooves in the tungsten carbide cemented carbide layer of polycrystalline diamond; 2. Polishing; 3. Ultrasonic cleaning; 4. Depositing the first SiO2 insulating layer; 5. Exposing the array pattern A using a mask or photolithography process; 6. Depositing a thin film of thermocouple material A; 7. Exposing the array pattern B using a mask or photolithography process; 8. Depositing a thin film of thermocouple material B; 9. Gluing compensation wires; 10. Depositing the second SiO2 insulating layer; 11. Welding. The present invention integrates a large number of micro-thin film thermocouples on the back face of the polycrystalline diamond tool to form an array, which can accurately measure the cutting edge-workpiece interface temperature and heat flow distribution, and find the thermal stress concentration point.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of temperature sensors, and in particular relates to a method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array, which is applied to the fields of precision machining, geological drilling, etc. Background Art

[0002] Polycrystalline diamond is a superhard material composed of diamond powder and cobalt as a binder sintered on tungsten carbide. It is often used in precision cutting and geological drilling. The large amount of cutting heat generated during high-speed cutting and drilling will cause the temperature of the workpiece and the tool or drill to rise sharply, affecting the quality of the tool, processing accuracy, and the discharge of drill chips or chips. In ultra-low temperature processing in liquid nitrogen environment or low-temperature drilling environment for frozen soil, the increase in cutting temperature is likely to affect the composition and physical and chemical properties of the workpiece, or cause the key substances in the rock and soil layer to volatilize and escape; in room temperature or high temperature processing and drilling environment, if the cutting temperature exceeds 700℃, it is easy for polycrystalline diamond tools to be graphitized under the catalytic action of cobalt. Therefore, accurate measurement of cutting temperature is crucial.

[0003] Commonly used temperature measurement technologies include non-contact infrared measurement and contact thermocouple measurement, but infrared measurement is not accurate enough, has large errors under cooling conditions, and is easily blocked by drill cuttings, making it difficult to directly obtain the temperature distribution at the tool tip, and the temperature inside the hole cannot be obtained under drilling conditions; contact thermocouples usually need to be buried inside the tool or workpiece, which is not only too far away from the tool tip to obtain accurate transient temperature values, but also secondary processing of the tool will cause a decrease in strength; and the point-to-face assembly method using insulating glue has greater errors and heat conduction delays.

[0004] Thin-film thermocouples are thermocouples made by depositing or bonding the two materials that make up the thermocouple on the surface of the temperature measuring object in the form of thin-film thermal junctions, or integrating and embedding them into the tool in the form of interlayers. The thickness is usually in the micron level, with very small thermal junction area and heat capacity. Therefore, a large number of thermocouple arrays can be integrated at the tool tip, and the thermoelectromotive force signal is led out by the compensation line at the back end. It has a series of advantages such as high precision, fast response, and less tool damage. Summary of the invention

[0005] The purpose of the present invention is to solve the problem that the thermocouple in the traditional contact temperature measurement of polycrystalline diamond tools is too far away from the tool tip to obtain accurate transient temperature values, and to provide a method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array.

[0006] The preparation method of the polycrystalline diamond tool with an embedded thin film thermocouple array of the present invention is implemented according to the following steps:

[0007] 1. Cut the polycrystalline diamond material into the shape of a knife blade or a drill blade, and process a plurality of shallow grooves on the edge of the tungsten carbide layer opposite to the cutting edge;

[0008] 2. polishing the tungsten carbide layer of the polycrystalline diamond material to obtain pre-processed polycrystalline diamond;

[0009] 3. Using acetone, ethanol and deionized water to ultrasonically clean the pre-processed polycrystalline diamond in sequence to obtain cleaned polycrystalline diamond;

[0010] Fourth, using a high-purity silicon target material and oxygen and argon as sputtering gases, a first SiO2 insulating layer is deposited on the surface of the tungsten carbide cemented carbide layer to obtain polycrystalline diamond with a SiO2 insulating layer deposited thereon;

[0011] 5. Using a mask or photolithography process, an array pattern A is exposed on a polycrystalline diamond deposited with a SiO2 insulating layer. The shape of the pattern A is that one end is located in a shallow groove and the other end extends linearly to the edge of a blade or a drill blade. Several patterns A are arranged in an array along the width direction of the blade or the drill blade to obtain a polycrystalline diamond with an array pattern A;

[0012] 6. Using a high-purity target made of thermocouple material A, a thin film of thermocouple material A is deposited on the exposed area of ​​the polycrystalline diamond after the array pattern A is prepared, so as to obtain polycrystalline diamond on which thermocouple material A is deposited;

[0013] 7. Using a mask or photolithography process, an array pattern B is exposed on the polycrystalline diamond on which the thermocouple material A is deposited. The shape of the pattern B is that one end is located in a shallow groove, and the other end extends linearly to the edge of a blade or drill. The pattern B overlaps with the pattern A at the edge, and the pattern B does not overlap with the pattern A in other areas. Several patterns B are arranged in an array along the width direction of the blade or drill. The number of patterns B is the same as the number of patterns A, and a polycrystalline diamond with an array pattern B is obtained;

[0014] 8. Then, using a high-purity target made of thermocouple material B, a thin film of thermocouple material B is deposited on the exposed area of ​​the polycrystalline diamond behind the array pattern B, and the thermocouple material A at the linear extension end and the thermocouple material B intersect at the overlapping pattern area of ​​the cutting edge to form a thermal junction, thereby obtaining a polycrystalline diamond after the thin film thermocouple is deposited;

[0015] 9. Connect the compensation wire A to the thermocouple material A film in the shallow groove through the conductive silver glue, connect the compensation wire B to the thermocouple material B film in the shallow groove through the conductive silver glue, and obtain the polycrystalline diamond with the compensation wire after curing, grinding and polishing the conductive silver glue;

[0016] 10. Using high-purity silicon target material and oxygen and argon as sputtering gas, a second SiO2 insulating layer is deposited on the surface of the polycrystalline diamond with compensation wire to obtain a polycrystalline diamond with an embedded thin film thermocouple array;

[0017] 11. Welding the polycrystalline diamond with embedded thin film thermocouple array to a cutter head base or another piece of polycrystalline diamond to obtain a polycrystalline diamond tool with embedded thin film thermocouple array.

[0018] Finally, the present invention performs thermoelectric potential-temperature calibration on the polycrystalline diamond tool with the embedded thin film thermocouple array.

[0019] The present invention integrates a large number of micro-thin film thermocouples to form an array on the back face of the polycrystalline diamond tool near the cutting edge. It can accurately measure the cutting edge-workpiece interface temperature and heat flow distribution, accurately measure the transient temperature value, and find the thermal stress concentration point; it can sense the transient cutting temperature field with ultra-high spatial and temporal resolution without being affected by the wear of the front cutting edge; it can be used in application scenarios such as cutting or drilling through different processing and welding methods, and has a series of advantages such as high precision, fast response, small tool damage, thermocouples are not affected by the external environment, and have a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the cross-sectional structure of a polycrystalline diamond tool with an embedded thin film thermocouple array according to the present invention;

[0021] Figure 2 It is a schematic diagram of a process for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array;

[0022] Figure 3 is a schematic diagram of a cutting edge flank surface machined using polycrystalline diamond with an embedded thin film thermocouple array in Example 1;

[0023] Figure 4 Schematic diagram of a centering rotary drill for polycrystalline diamond machining using an embedded thin film thermocouple array in Example 2. DETAILED DESCRIPTION

[0024] Specific implementation method 1: The preparation method of the polycrystalline diamond tool with an embedded thin film thermocouple array in this implementation method is implemented according to the following steps:

[0025] 1. Cut the polycrystalline diamond material into the shape of a knife blade or a drill blade, and process a plurality of shallow grooves 3 on the edge of the tungsten carbide hard alloy layer 2 opposite to the cutting edge;

[0026] 2. Polishing the tungsten carbide hard alloy layer 2 of the polycrystalline diamond material to obtain pre-processed polycrystalline diamond;

[0027] 3. Using acetone, ethanol and deionized water to ultrasonically clean the pre-processed polycrystalline diamond in sequence to obtain cleaned polycrystalline diamond;

[0028] Fourth, using a high-purity silicon target material and oxygen and argon as sputtering gases, a first SiO2 insulating layer 4 is deposited on the surface of the tungsten carbide hard alloy layer 2 to obtain a polycrystalline diamond with a SiO2 insulating layer deposited thereon;

[0029] 5. Using a mask or photolithography process, an array pattern A is exposed on the polycrystalline diamond deposited with a SiO2 insulating layer. The shape of the pattern A is that one end is located in the shallow groove 3 and the other end extends linearly to the edge of the blade or drill blade. Several patterns A are arranged in an array along the width direction of the blade or drill blade to obtain a polycrystalline diamond with the array pattern A;

[0030] 6. Using a high-purity target made of thermocouple material A, a thin film of thermocouple material A is deposited on the exposed area of ​​the polycrystalline diamond after the array pattern A is prepared, to obtain a polycrystalline diamond on which thermocouple material A5 is deposited;

[0031] 7. Using a mask or photolithography process, an array pattern B is exposed on the polycrystalline diamond on which the thermocouple material A is deposited. The shape of the pattern B is that one end is located in the shallow groove 3, and the other end extends linearly to the edge of the blade or drill blade. The pattern B overlaps with the pattern A at the edge position, and the pattern B does not overlap with the pattern A in other areas. Several patterns B are arranged in an array along the width direction of the blade or drill blade, and the number of patterns B is the same as that of pattern A, to obtain a polycrystalline diamond with array pattern B;

[0032] 8. Then, using a high-purity target made of thermocouple material B, a thermocouple material B6 is deposited on the exposed area of ​​the polycrystalline diamond behind the array pattern B, and the thermocouple material A at the linear extension end and the thermocouple material B intersect at the edge overlap pattern area to form a thermal junction 7, thereby obtaining a polycrystalline diamond after the thin film thermocouple is deposited;

[0033] 9. Connect the compensation wire A9 to the thermocouple material A film in the shallow groove 3 through the conductive silver glue 8, and connect the compensation wire B10 to the thermocouple material B film in the shallow groove 3 through the conductive silver glue. After the conductive silver glue is cured, polished, and the polycrystalline diamond with compensation wire is obtained;

[0034] 10. Using high-purity silicon target material and oxygen and argon as sputtering gas, a second SiO2 insulating layer 11 is deposited on the surface of the polycrystalline diamond with compensation wire to obtain a polycrystalline diamond with an embedded thin film thermocouple array;

[0035] 11. Welding the polycrystalline diamond with embedded thin film thermocouple array to a cutter head base or another piece of polycrystalline diamond to obtain a polycrystalline diamond tool with embedded thin film thermocouple array.

[0036] Finally, the present invention performs thermoelectric potential-temperature calibration on the polycrystalline diamond tool with the embedded thin film thermocouple array.

[0037] Specific embodiment 2: The difference between this embodiment and specific embodiment 1 is that the thickness of the tungsten carbide cemented carbide layer 2 in the polycrystalline diamond material in step 1 is 2 to 5 mm.

[0038] Specific implementation method three: The difference between this implementation method and specific implementation methods one or two is that the depth of the shallow groove 3 in step one is 0.2 mm to 3 mm.

[0039] Specific embodiment 4: The difference between this embodiment and any one of specific embodiments 1 to 3 is that in step 4, the thickness of the first SiO2 insulating layer 4 is 1 to 50 μm.

[0040] Specific implementation method 5: This implementation method is different from specific implementation methods 1 to 4 in that the other ends of pattern A and pattern B in steps 5 and 7 are linearly extended to the cutting edge of the blade or drill blade, and the linear extension end is 0.5 to 3 mm away from the cutting edge.

[0041] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that the thermocouple material A and the thermocouple material B are constantan and copper respectively.

[0042] In this embodiment, the thermocouple material A and the thermocouple material B form a T-type thermocouple.

[0043] Specific implementation method 7: This implementation method is different from specific implementation methods 1 to 5 in that the thermocouple material A and the thermocouple material B are nickel-chromium alloy and nickel-silicon alloy respectively.

[0044] In this embodiment, the thermocouple material A and the thermocouple material B form a K-type thermocouple.

[0045] Specific embodiment eight: This embodiment differs from any one of specific embodiments one to five in that in step six and step eight, a magnetron sputtering or electron beam evaporation process is used to deposit the thermocouple material A film and the thermocouple material B film.

[0046] Specific embodiment 9: This embodiment is different from specific embodiment 8 in that the thickness of the thermocouple material A film and the thermocouple material B film is 1-50 μm.

[0047] Specific implementation method ten: The difference between this implementation method and any one of specific implementation methods one to nine is that the thickness of the second SiO2 insulating layer in step ten is 1 to 50 μm.

[0048] Embodiment 1: The preparation method of the polycrystalline diamond tool with embedded thin film thermocouple array in this embodiment is implemented according to the following steps:

[0049] 1. Cut the polycrystalline diamond material into an equilateral triangle with a side length of 15 mm. The thickness of the polycrystalline layer 1 is 1.5 mm, and the thickness of the tungsten carbide cemented carbide layer 2 is 1.5 mm. Process a plurality of shallow grooves 3 on the edge of the tungsten carbide cemented carbide layer 2 opposite to the cutting edge. The area of ​​the shallow grooves 3 is 1.2*2 mm and the depth is 0.5 mm.

[0050] 2. polishing the tungsten carbide layer of the polycrystalline diamond material to obtain pre-processed polycrystalline diamond;

[0051] 3. Using acetone, ethanol and deionized water to ultrasonically clean the pre-processed polycrystalline diamond for 15 minutes in sequence to obtain cleaned polycrystalline diamond;

[0052] Fourth, using a high-purity silicon target, using oxygen and argon as sputtering gases, with an oxygen flow rate of 2 sccm and an argon flow rate of 20 sccm, a first SiO2 insulating layer 4 with a thickness of 2 μm is deposited on the surface of the tungsten carbide cemented carbide layer 2 under a power of 100 W and a gas pressure of 5 Pa, to obtain a polycrystalline diamond with a SiO2 insulating layer deposited thereon;

[0053] 5. Using a mask process, an array pattern A is exposed on a polycrystalline diamond deposited with a SiO2 insulating layer. The shape of the pattern A is that a block at one end is located in a shallow groove 3, and the other end is linearly extended to the edge of the blade. The linear extension end is 1 mm away from the edge of the cutting edge. Several patterns A are arranged in an array along the width direction of the blade to obtain a polycrystalline diamond with an array pattern A;

[0054] 6. Using a high-purity target made of thermocouple material A, a 1.2 μm thin film 5 of thermocouple material A is deposited on the exposed area of ​​the polycrystalline diamond behind the array pattern A to obtain a polycrystalline diamond on which thermocouple material A5 is deposited;

[0055] 7. Using a mask process, an array pattern B is exposed on the polycrystalline diamond on which the thermocouple material A is deposited. The shape of the pattern B is that one end is in a block shape and is located in the shallow groove 3, and the other end is in a linear shape and extends to the edge of the blade. The pattern B overlaps with the pattern A at the edge, and the pattern B does not overlap with the pattern A in other areas. Several patterns B are arranged in an array along the width direction of the blade, and the number of patterns B is the same as that of patterns A, to obtain a polycrystalline diamond with an array pattern B;

[0056] 8. Then, a high-purity target made of thermocouple material B is used to deposit a 1.2 μm thermocouple material B film 6 on the exposed area of ​​the polycrystalline diamond behind the array pattern B. The (pair of) thermocouple materials A and thermocouple material B at the linear extension end intersect to form a thermal junction 7, and the thermal junction area is 5×10 5 μm 2, the thermocouple material A film and the thermocouple material B film in the shallow groove 3 are arranged at intervals to obtain the deposited polycrystalline diamond;

[0057] 9. Connect the compensation wire A9 to the thermocouple material A film in the shallow groove 3 through the conductive silver glue 8, and connect the compensation wire B10 to the thermocouple material B film in the shallow groove 3 through the conductive silver glue 8. After the conductive silver glue is cured, polished, and polished, a polycrystalline diamond with compensation wire is obtained;

[0058] 10. Using high-purity silicon target material, oxygen and argon as sputtering gas, oxygen flow rate is 2sccm, argon flow rate is 20sccm, and a second SiO2 insulating layer 11 is deposited on the surface of the polycrystalline diamond with compensation wire under the conditions of 100W power and 5Pa pressure. The thickness of the second SiO2 insulating layer is 2μm. After the connection between the compensation wire and the cutting edge is isolated and sealed with insulating glue, the embedded thin film thermocouple array is statically calibrated to obtain a polycrystalline diamond with an embedded thin film thermocouple array.

[0059] 11. Welding the polycrystalline diamond with embedded thin film thermocouple array to a drill bit substrate to obtain a polycrystalline diamond tool with embedded thin film thermocouple array.

[0060] In this embodiment, the material of the thermocouple material A film 5 is nickel-chromium alloy, and the material of the thermocouple material B film 6 is nickel-silicon alloy.

[0061] In step nine of this embodiment, take a K-type thermocouple compensation wire, cut off the hot junction end and peel off 2.5mm of the insulation to expose the internal nickel-chromium alloy and nickel-silicon alloy wires, flatten and trim the shape of the 2mm portion of the alloy wire, and embed it into the pre-machined shallow groove of the tungsten carbide cemented carbide layer according to the same material correspondence.

[0062] A triangular polycrystalline diamond cutting edge with an embedded thin film thermocouple array was fabricated, as shown in the attached Figure 3 As shown. The cutting edge is then connected to the tool holder of a lathe or other processing equipment by clamping or welding. Because of the protective effect of the SiO2 insulating layer, welding and other fixing methods will not affect the thin film thermocouple; the thermocouple is deposited on the tungsten carbide on the back face of the cutting edge to avoid the wear of the polycrystalline diamond on the front face and the impact of the chips; by integrating a large number of micro-thin film thermocouples to form an array near the cutting edge, the cutting edge-workpiece interface temperature and heat flow distribution can be accurately measured to find the thermal stress concentration point; the transient cutting temperature field is sensed with ultra-high spatial and temporal resolution; it has a series of advantages such as high precision, fast response, small tool damage, the thermocouple is not affected by the external environment, and has a wide range of applications.

[0063] Embodiment 2: The preparation method of the polycrystalline diamond tool with embedded thin film thermocouple array in this embodiment is implemented according to the following steps:

[0064] 1. Cut the polycrystalline diamond material into a centering rotary drill base with a width of 30 mm and a height of 20 mm, wherein the thickness of the polycrystalline layer is 0.8 mm, the thickness of the tungsten carbide cemented carbide layer 2 is 1.5 mm, and a plurality of shallow grooves 3 are processed on the edge of the tungsten carbide cemented carbide layer opposite to the cutting edge. The area of ​​the shallow grooves 3 is 1.5*2.5 mm and the depth is 0.5 mm;

[0065] 2. polishing the tungsten carbide layer of the polycrystalline diamond material to obtain pre-processed polycrystalline diamond;

[0066] 3. Using acetone, ethanol and deionized water to ultrasonically clean the pre-processed polycrystalline diamond for 15 minutes in sequence to obtain cleaned polycrystalline diamond;

[0067] Fourth, using a high-purity silicon target material and oxygen and argon as sputtering gases, a first SiO2 insulating layer 4 with a thickness of 1.2 μm is deposited on the surface of the tungsten carbide hard alloy layer 2 to obtain polycrystalline diamond with a SiO2 insulating layer deposited thereon;

[0068] 5. Using a mask process, an array pattern A is exposed on the polycrystalline diamond deposited with a SiO2 insulating layer. The shape of the pattern A is that one end is located in the shallow groove 3, and the other end is linearly extended to the edge of the drill blade. The linear extension end is 0.7 mm away from the edge of the cutting edge. Several patterns A are arranged in an array along the width direction of the drill blade to obtain a polycrystalline diamond with an array pattern A;

[0069] 6. Using a high-purity target made of thermocouple material A, a thermocouple material A film 5 is deposited on the exposed area of ​​the polycrystalline diamond behind the array pattern A to obtain a polycrystalline diamond on which the thermocouple material A is deposited;

[0070] 7. Using a mask process, an array pattern B is exposed on the polycrystalline diamond on which the thermocouple material A is deposited. The shape of the pattern B is that one end is located in the shallow groove 3, and the other end extends linearly to the cutting edge of the drill blade. The pattern B overlaps with the pattern A at the cutting edge, and the patterns in other areas do not overlap. Several patterns B are arranged in an array along the width direction of the drill blade, and the number of patterns A and patterns B is the same, so as to obtain a polycrystalline diamond with an array pattern B;

[0071] 8. Then, a high-purity target made of thermocouple material B is used to deposit a thermocouple material B film 6 on the exposed area of ​​the polycrystalline diamond behind the array pattern B. The thermocouple material A at the linear extension end intersects with the thermocouple material B to form a thermal junction 7. The thermal junction area is 5×10 5 μm 2 , the thermocouple material A film and the thermocouple material B film in the shallow groove 3 are arranged at intervals to obtain the deposited polycrystalline diamond;

[0072] 9. Connect the compensation wire A9 to the thermocouple material A film in the shallow groove 3 through the conductive silver glue, connect the compensation wire B10 to the thermocouple material B film in the shallow groove 3 through the conductive silver glue, and obtain the polycrystalline diamond with compensation wire after curing, grinding and polishing the conductive silver glue;

[0073] 10. Using high-purity silicon target material, oxygen and argon as sputtering gas, a second SiO2 insulating layer is deposited on the surface of the polycrystalline diamond with compensation wire, the thickness of the second SiO2 insulating layer is 1.2 μm, and the connection between the compensation wire and the cutting edge is isolated and sealed with insulating glue, and then the embedded thin film thermocouple array is statically calibrated to obtain a polycrystalline diamond with an embedded thin film thermocouple array;

[0074] 11. Weld the polycrystalline diamond with embedded thin film thermocouple array to another piece of polycrystalline diamond to obtain a polycrystalline diamond centering rotary drill with embedded thin film thermocouple array.

[0075] In this embodiment, the material of the thermocouple material A film is constantan, and the material of the thermocouple material B film is copper.

[0076] In step seven of this embodiment, take a T-type thermocouple compensation wire, cut off the hot junction end and peel off 3mm of the insulation to expose the internal nickel-chromium alloy and nickel-silicon alloy wires, flatten and trim the shape of the 2.5mm portion of the alloy wire, and embed it into the pre-processed shallow groove of the tungsten carbide cemented carbide layer according to the same material correspondence.

[0077] This embodiment is aligned with the tungsten carbide surface of the other half of the polycrystalline diamond centering rotary drill of the same material and size but without thin film thermocouple deposition and welded together to form a sandwich structure centering rotary drill. The polycrystalline layer is used for cutting on both sides, the tungsten carbide is located in the middle for support, and the embedded thin film thermocouple array is sandwiched between the two layers of tungsten carbide. After the connection between the compensation wire and the drill blade is isolated and sealed with insulating glue, the static temperature calibration of the embedded thin film thermocouple array is performed. The polycrystalline diamond centering rotary drill with an embedded thin film thermocouple array is completed.

[0078] Because of the SiO2 insulating protective layer, welding will not affect the thin-film thermocouple; the thermocouple is integrated inside the drill blade to avoid wear of the polycrystalline diamond on the front cutting edge and impact of chips; by integrating a large number of micro-thin-film thermocouples to form an array near the cutting edge, the drill blade-rock and soil interface temperature and heat flow distribution can be accurately measured to find the thermal stress concentration point; the transient drilling temperature field is sensed with ultra-high spatial and temporal resolution; it has a series of advantages such as high precision, fast response, small tool damage, thermocouple is not affected by the external environment, and has a wide range of applications.

Claims

1. A method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array, characterized in that The preparation method is achieved by the following steps:

1. Cutting the polycrystalline diamond material into the shape of a knife blade or a drill blade, and processing a plurality of shallow grooves (3) on the edge of the tungsten carbide hard alloy layer (2) opposite to the cutting edge; 2. polishing the tungsten carbide hard alloy layer (2) of the polycrystalline diamond material to obtain pre-processed polycrystalline diamond; 3. Using acetone, ethanol and deionized water to ultrasonically clean the pre-processed polycrystalline diamond in sequence to obtain cleaned polycrystalline diamond; Fourth, using a high-purity silicon target material and oxygen and argon as sputtering gases, a first SiO2 insulating layer (4) is deposited on the surface of the tungsten carbide hard alloy layer (2) to obtain polycrystalline diamond deposited with the SiO2 insulating layer; 5. Using a mask process, an array pattern A is exposed on the polycrystalline diamond deposited with a SiO2 insulating layer, wherein the pattern A has one end located in the shallow groove (3) and the other end extending linearly to the edge of the blade or drill blade, and a plurality of patterns A are arranged in an array along the width direction of the blade or drill blade to obtain a polycrystalline diamond with the array pattern A; 6. Using a high-purity target made of thermocouple material A, a thin film of thermocouple material A is deposited on the exposed area of ​​the polycrystalline diamond after the array pattern A is prepared (5), thereby obtaining a polycrystalline diamond on which the thermocouple material A is deposited; 7. Using a mask process, an array pattern B is exposed on the polycrystalline diamond on which the thermocouple material A is deposited. The shape of the pattern B is that one end is located in the shallow groove (3) and the other end extends linearly to the cutting edge of the blade or drill. The pattern B overlaps with the pattern A at the cutting edge, and the pattern B does not overlap with the pattern A in other areas. A plurality of patterns B are arranged in an array along the width direction of the blade or drill. The number of patterns B is the same as the number of patterns A, thereby obtaining a polycrystalline diamond with an array pattern B.

8. Then, using a high-purity target made of thermocouple material B, a thermocouple material B film is deposited on the exposed area of ​​the polycrystalline diamond behind the array pattern B (6), and the thermocouple material A at the linear extension end and the thermocouple material B intersect in the overlapping pattern area of ​​the cutting edge to form a thermal junction (7), thereby obtaining the polycrystalline diamond after the thin film thermocouple is deposited; 9. Connecting the compensation wire A (9) to the thermocouple material A film in the shallow groove (3) through the conductive silver glue (8), connecting the compensation wire B (10) to the thermocouple material B film in the shallow groove (3) through the conductive silver glue, and obtaining polycrystalline diamond with compensation wire after curing, grinding and polishing the conductive silver glue; 10. Using a high-purity silicon target material and oxygen and argon as sputtering gases, a second SiO2 insulating layer (11) is deposited on the surface of the polycrystalline diamond with compensation wires to obtain a polycrystalline diamond with an embedded thin film thermocouple array; 11. Welding the polycrystalline diamond with embedded thin film thermocouple array to a cutter head base or another piece of polycrystalline diamond to obtain a polycrystalline diamond tool with embedded thin film thermocouple array.

2. The method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array according to claim 1, characterized in that In step 1, the thickness of the tungsten carbide hard alloy layer (2) in the polycrystalline diamond material is 2 to 5 mm.

3. The method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array according to claim 1, characterized in that The depth of the shallow groove (3) in step 1 is 0.2 mm to 3 mm.

4. The method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array according to claim 1, characterized in that In step 4, the thickness of the first SiO2 insulating layer (4) is 1 to 50 μm.

5. The method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array according to claim 1, characterized in that In step 5 and step 7, the other end of pattern A and pattern B is extended linearly to the cutting edge of the blade or drill blade, and the linear extension end is 0.5 to 3 mm away from the cutting edge.

6. The method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array according to claim 1, characterized in that The thermocouple material A and the thermocouple material B are constantan and copper respectively.

7. The method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array according to claim 1, characterized in that The thermocouple material A and the thermocouple material B are nickel-chromium alloy and nickel-silicon alloy respectively.

8. The method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array according to claim 1, characterized in that In step six and step eight, a thermocouple material A film and a thermocouple material B film are deposited by magnetron sputtering or electron beam evaporation process.

9. The method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array according to claim 1, characterized in that The thickness of the thermocouple material A film and the thermocouple material B film is 1 to 50 μm.

10. The method for preparing a polycrystalline diamond tool with an embedded thin film thermocouple array according to claim 1, characterized in that In step 10, the thickness of the second SiO2 insulating layer is 1-50 μm.