A method and device for producing crystalline aluminum chloride and PAFC using solid waste
By reacting the solid waste salt sodium chloride with concentrated sulfuric acid and coal gangue, crystalline aluminum chloride and PAFC are obtained, which solves the problem of unutilized resources, and achieves efficient and low-cost resource recycling and environmental protection effects, which is suitable for industrialization Promotion.
Patent Information
- Application Number
- CN202310436054.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-04-21
AI Technical Summary
Resources such as coal gangue, solid waste salt sodium sulfate and sodium chloride have not been fully developed and utilized, resulting in resource waste and environmental pollution.
By exothermic reaction of the solid waste salt sodium chloride with concentrated sulfuric acid to generate sodium bisulfate and hydrogen chloride gas, crystalline aluminum chloride and polymeric aluminum chloride (PAFC) were prepared and passed The multi-step process is carried out to hydrolysis, polymerization and evaporation to obtain high-purity PAFC products, while recycling miscellaneous salts and silicon slag.
It realizes efficient utilization of resources, reduces energy consumption and costs, improves processing efficiency, product recovery rate and purity, is suitable for industrial promotion, and does not require thermal energy consumption, saves part of the thermal energy consumption, and is suitable for environmentally friendly industrial applications.
Smart Images

Figure CN116477651B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of industrial solid waste treatment, and in particular relates to a method and a device for producing crystalline aluminum chloride and polyaluminum ferric chloride (PAFC) by utilizing solid waste. Background Art
[0002] Coal gangue is solid waste discharged during the coal mining and coal washing process. It is a kind of black-gray rock with low carbon content and harder than coal that accompanies the coal seam during the coal formation process. It includes excavation gangue during tunnel excavation, gangue mined from the roof, floor and interlayer during mining, and washed gangue picked out during coal washing. Its main components are Al2O3 and SiO2. It also contains varying amounts of Fe2O3, CaO, MgO, TiO2, Na2O, K2O, P2O5, SO3 and trace rare elements (gallium, vanadium, titanium, cobalt). At present, a large amount of coal gangue has not been comprehensively utilized. In addition, the solid waste salts sodium sulfate and sodium chloride in coal chemical wastewater treatment have not been fully and comprehensively developed and utilized.
[0003] Due to the existence of the above-mentioned technical problems, it is necessary to further comprehensively develop and utilize resources such as coal gangue, solid waste salt sodium sulfate and sodium chloride. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a method and device for producing crystalline aluminum chloride and polyaluminum ferric chloride (PAFC) using solid waste.
[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0006] A method for producing crystalline aluminum chloride and PAFC using solid waste comprises the following steps:
[0007] (1) drying the solid waste salt sodium chloride and preheating it at the same time, reacting it with concentrated sulfuric acid to generate sodium bisulfate and hydrogen chloride gas in an exothermic reaction, and controlling the reaction temperature (to ensure the reaction speed);
[0008] (2) subjecting the coal gangue to high temperature activation and mechanical activation to obtain activated coal gangue;
[0009] (3) mixing the activated coal gangue obtained in step (2) with hydrochloric acid and / or the hydrochloric acid mother liquor obtained in step (4), adding iron ore or iron oxide for stirring and acid hydrolysis leaching, and obtaining an aluminum chloride solution containing iron chloride and silicon slag;
[0010] (4) allowing the aluminum chloride solution containing ferric chloride obtained in step (3) to absorb the hydrogen chloride gas obtained in step (1) and / or step (5) to precipitate crystalline aluminum chloride, and the obtained hydrochloric acid mother liquor is returned to step (3) for repeated utilization;
[0011] (5) mixing the aluminum chloride solution containing ferric chloride obtained in step (3) with the (partial) crystallized aluminum chloride obtained in step (4), stirring to make them re-saturated, performing hydrolysis and polymerization reaction under certain temperature and pressure conditions, and releasing hydrogen chloride gas, and obtaining a polymer product through evaporation, crystallization, filter pressing, and drying to obtain a PAFC product;
[0012] (6) The remaining liquid after evaporation and crystallization in step (5) is separated into a salt solution by nanofiltration, and a soda solution is added to neutralize and remove impurities before recycling.
[0013] The above method further comprises the following steps: in step (1), the solid waste salt sodium chloride is solid waste salt sodium chloride obtained from various sewage, wastewater treatment or chemical production, and its water content is 3-5%; the drying and preheating temperature of the solid waste salt sodium chloride is 140-150° C., and the reaction temperature is controlled to be increased to 220-230° C.; and the concentrated sulfuric acid is 98% concentrated sulfuric acid.
[0014] Furthermore, in step (2), the main components of the coal gangue are Al2O3 and SiO2, and it also contains a small amount of any one or more of Fe2O3, CaO, MgO, TiO2, Na2O, K2O, etc.; the temperature of the high-temperature activation is 650-700°C; during the high-temperature activation, fuel gas is introduced into the activation furnace to assist combustion and heat, and 700-800 kPaG of steam is produced with deionized water, and the steam is used for heating the hydrolysis and polymerization reactions in step (5) or the evaporation and concentration of the separation of sodium chloride and sodium sulfate (also known as thermal denitrification), and the raw materials that can replace the coal gangue are all substances containing aluminum or aluminum oxide; the specific operation of the mechanical activation is: crushing the coal gangue after high-temperature activation.
[0015] Furthermore, in step (3), the stirring and acid hydrolysis leaching time is 0.8 to 1.2 hours, and the pH value is controlled to be less than 4 during the stirring and acid hydrolysis leaching.
[0016] Furthermore, in step (5), the temperature of the hydrolysis and polymerization reaction is controlled at 150-160° C., the pressure is controlled at 0.5-0.6 MPaG, and the polymerization time is controlled at 30-50 min. The specific operation of the evaporation crystallization is as follows: negative pressure flash evaporation is performed using a PAFC polymerization kettle at a vacuum degree of -85--90 kPaG, the generated acidic water vapor enters a surface condenser for condensation, and the solution in the kettle is reduced from 150-160° C. to below 60° C.; then the slurry in the PAFC polymerization kettle and the slurry in the PAFC scraper film evaporation concentrator are filtered and dried together to obtain a PAFC product.
[0017] Furthermore, in step (6), the impure salt is a mixed salt of any one or more of sodium chloride, potassium chloride, calcium chloride, and magnesium chloride, and the impure salt is acidic;
[0018] The recycling specifically comprises the following steps: when the potassium chloride content is relatively high (the potassium bisulfate content of the solid waste salt sodium chloride obtained by evaporating and returning to the double salt evaporation and concentration step to produce sodium bisulfate does not meet the requirement), the impurity-removed impurity salt solution is evaporated and concentrated to obtain an impurity salt slurry with a solid-liquid ratio of 25-35%, and then the impurity salt is recycled after being dehydrated by plate and frame filter pressing (impurity salt recovery scheme 1); when the potassium chloride content is relatively low, the impurity-removed impurity salt solution is returned to the step (5) and mixed with the aluminum chloride solution containing ferric chloride and the crystalline aluminum chloride for recycling (impurity salt recovery scheme 2).
[0019] Reaction principle of the present invention:
[0020] 1. Gangue activation mechanism: First, high-temperature activation is carried out, the main purpose of which is to remove carbon; then mechanical activation is carried out, and the activated gangue is crushed with an activated gangue crusher to increase its activity and improve the acid hydrolysis reaction rate.
[0021] 2. Sodium bisulfate reaction principle: Solid sodium chloride reacts with 98% concentrated sulfuric acid at 220-230°C (this reaction is an exothermic reaction, and the preheating temperature of solid sodium chloride is 140-150°C). The chemical reaction formula is as follows:
[0022] NaCl+H2SO4(concentrated)→NaHSO4+HCl↑
[0023] 3. Crystallization principle of aluminum chloride hexahydrate: The solubility of hydrogen chloride is much greater than that of aluminum chloride. When aluminum chloride solution absorbs hydrogen chloride gas, hydrogen chloride gas dissolves in water to generate hydrochloric acid, thereby precipitating crystalline aluminum chloride (AlCl3·6H2O). The chemical reaction formula is as follows:
[0024] AlCl3+6H2O→AlCl3·6H2O
[0025] 4. Principle of acid hydrolysis reaction: Al2O3, Fe2O3, Na2O, K2O, CaO, MgO, etc. in activated coal gangue react with HCl in hydrochloric acid mother liquor to generate AlCl3, NaCl, KCl, CaCl2, etc. (SiO2, TiO2 do not react chemically with HCl in hydrochloric acid mother liquor). The chemical reaction formula is as follows:
[0026] Al2O3+6HCl→2AlCl3+3H2O
[0027] Fe2O3+6HCl→2FeCl3+3H2O
[0028] Na2O+2HCl→2NaCl+H2O
[0029] K2O+2HCl→2KCl+H2O
[0030] CaO+2HCl→CaCl2+H2O
[0031] MgO+2HCl→MgCl2+H2O
[0032] 5. Principle of PAFC hydrolysis and polymerization reaction: PAFC is a mixture of hydrolysis and polymerization of most AlCl3 and a small part of FeCl3. It is a better flocculant, and its flocculation effect far exceeds that of PAC. The chemical reaction formula is as follows:
[0033] 2MAlCl3+nMH2O→{Al2(OH) n Cl 6-n} M +nMHCl↑
[0034] 2NFeCl3+mNH2O→{Al2(OH) m Cl 6-m} N +mNHCl↑
[0035] {Al2(OH) n Cl 6-n} M +{Al2(OH) m Cl 6-m} N →{Al2(OH) n Cl 6-n} M ·{Al2(OH) m Cl 6-m} N (m and n are natural numbers less than 6, and M and N are natural numbers ≤10).
[0036] 6. Neutralization of mixed salt solution and removal of calcium and magnesium reaction principle: Use soda ash to neutralize the hydrochloric acid in the mixed salt solution to generate sodium chloride and water, which react with calcium chloride and magnesium chloride to generate calcium carbonate and magnesium carbonate precipitation. The chemical reaction formula is as follows:
[0037] Na2CO3+2HCl→2NaCl+CO2↑+H2O
[0038] Na2CO3+CaCl2→2NaCl+CaCO3↓
[0039] Na2CO3+MgCl2→2NaCl+MgCO3↓
[0040] The above method has the advantages of low energy consumption, low cost, high processing efficiency, energy saving and environmental protection, complete reaction, high product recovery rate and purity, etc., and is suitable for industrial promotion and application; all solid waste coal gangue and solid waste sodium chloride from coal chemical industry are used as production raw materials, solid waste silicon slag produced in the production process can be used as construction sand, solid waste miscellaneous salt can be used as quenching salt in heat treatment (miscellaneous salt recovery scheme 1), and the miscellaneous salt solution can be directly returned to the double salt evaporation and concentration process for recycling (miscellaneous salt recovery scheme 2), waste gas and flue gas are treated according to the national gas boiler flue gas treatment method, and wastewater is returned to the front-end sewage treatment system for treatment; aluminum chloride solution is used to absorb hydrogen chloride gas to precipitate crystalline aluminum chloride (AlCl3·6H2O), without the consumption of thermal energy, a part of which is sold as a product, and the other part is used for the re-saturation of aluminum chloride solution, which relatively saves part of the thermal energy consumption of PAFC evaporation.
[0041] In the above method, the vacuum degree of negative pressure flash evaporation in the PAFC polymerization kettle is controlled to be -85 to -90 kPaG, the generated acidic water vapor enters the surface condenser for condensation, and the solution in the kettle is reduced from 150 to 160°C to below 60°C, which can save part of the heat energy of PAFC evaporation; water is circulated in the system (for example, the water used for plate and frame washing is the acidic condensed water in the system), and only water loss and water carried away by the product need to be supplemented; in the process of activation of coal gangue, all carbon components of coal gangue are burned, and all its heat energy is used to produce steam for the system.
[0042] Based on a general inventive concept, the present invention also provides a device for the above method, which includes a coal gangue acid hydrolysis and leaching main system, an aluminum chloride crystallization and hydrogen chloride absorption main system, a PAFC polymerization main system, and a miscellaneous salt recovery main system connected in sequence. The device also includes a sodium bisulfate auxiliary system connected to the aluminum chloride crystallization and hydrogen chloride absorption main system, and a coal gangue activation auxiliary system connected to the coal gangue acid hydrolysis and leaching main system.
[0043] The sodium bisulfate auxiliary system provides the required hydrogen chloride gas for the main system, and the gangue activation auxiliary system provides the required activated gangue for the main system. The activated gangue provided by the gangue activation auxiliary system and the hydrochloric acid mother liquor provided by the aluminum chloride crystallization and hydrogen chloride absorption main system are acid-lyzed and leached in the gangue acid-lyzed leaching main system to obtain aluminum chloride solution and silicon slag, which can be shipped and sold as building materials. The aluminum chloride solution absorbs the hydrogen chloride gas in the aluminum chloride crystallization and hydrogen chloride absorption main system, and precipitates crystalline aluminum chloride. The aluminum chloride solution and the crystalline aluminum chloride are transported to the PAFC polymerization main system, and after being re-saturated, they are hydrolyzed and polymerized at 150-160°C and 0.5-0.6MPaG to obtain PAFC, which is evaporated and crystallized to obtain PAFC products, and the PAFC solution is separated by nanofiltration to obtain the impure salt solution. The impure salt solution provided by the PAFC polymerization main system is evaporated and crystallized in the impure salt recovery main system and recycled (impurity salt recovery plan 1). The impure salt solution can be directly returned to the double salt evaporation and concentration process for recycling (impurity salt recovery plan 2), thereby improving the recovery rate and reducing solid waste.
[0044] The above-mentioned device, further, the main system for acid hydrolysis and leaching of coal gangue includes an activated coal gangue hanging hopper, an acid hydrolysis leaching tank, an acid hydrolysis slurry pump, an acid hydrolysis plate and frame filter press, and an acid hydrolysis silicon slag hopper connected in sequence; after the activated coal gangue hanging hopper is filled with the required amount of activated coal gangue, the hanging device is placed at the feed inlet of the acid hydrolysis leaching tank to load the activated coal gangue into the acid hydrolysis leaching tank;
[0045] The liquid inlet end of the acidolysis leaching tank is connected to the crystallization plate-frame filter press of the aluminum chloride crystallization and hydrogen chloride absorption main system;
[0046] The liquid outlet of the acid hydrolysis plate-frame filter press is respectively connected to the absorption circulation tank and tail gas absorption circulation tank of the aluminum chloride crystallization and hydrogen chloride absorption main system, and the aluminum chloride mother liquor tank of the PAFC polymerization main system; the material outlet of the acid hydrolysis plate-frame filter press is connected to the acid hydrolysis silicon slag hopper; the acid hydrolysis plate-frame filter press is also connected to a washing water pump and an acidic water tank;
[0047] The liquid outlet of the acid hydrolysis plate and frame filter press is also connected to the tail gas absorption circulation tank of the aluminum chloride crystallization and hydrogen chloride absorption main system, so that the acidic water delivered by the cleaning water pump is used to wash the plate and frame and then recycled in the system.
[0048] Furthermore, the aluminum chloride crystallization and hydrogen chloride absorption main system comprises a crystallization absorption tower, an absorption circulation tank, an absorption circulation pump, an absorption salt pump, a crystallization plate and frame filter press, and a crystallization filter cake hopper connected in sequence;
[0049] The air inlet end of the crystallization absorption tower is connected to the Mannheim reactor of the sodium bisulfate auxiliary system and the PAFC polymerization kettle of the PAFC polymerization main system respectively; the air outlet end of the crystallization absorption tower is connected to the hydraulic jet pump, and the hydraulic jet pump is connected to the acid water pump and the tail gas absorption circulation tank in sequence;
[0050] The liquid inlet end of the absorption circulation tank is respectively connected to the tail gas absorption circulation tank, the crystallization absorption tower, and the acid hydrolysis plate-frame filter press of the coal gangue acid hydrolysis and leaching main system;
[0051] The liquid outlet end of the crystallization plate-frame filter press is connected to the acid hydrolysis leaching tank of the coal gangue acid hydrolysis leaching main system, and the material outlet end of the crystallization plate-frame filter press is connected to the crystallization filter cake hopper;
[0052] The discharge end of the crystallization filter cake hopper is connected to the PAFC polymerization kettle of the PAFC polymerization main system.
[0053] Furthermore, the PAFC polymerization main system includes an aluminum chloride mother liquor tank, an aluminum chloride mother liquor pump, a PAFC polymerization kettle, a PAFC slurry buffer tank, a polymerization salt extraction pump, and a polymerization plate and frame filter press connected in sequence;
[0054] The liquid inlet end of the aluminum chloride mother liquor tank is connected to the acid hydrolysis plate-frame filter press of the coal gangue acid hydrolysis and leaching main system;
[0055] The feed end of the PAFC polymerization kettle is connected to the crystallization filter cake hopper of the aluminum chloride crystallization and hydrogen chloride absorption main system; the liquid inlet end of the PAFC polymerization kettle is connected to the liquid outlet end of the aluminum chloride mother liquor pump; the gas outlet end of the PAFC polymerization kettle is respectively connected to the surface condenser (opened when the pressure is reduced after the polymerization is completed, and closed during the polymerization reaction), and the crystallization absorption tower of the aluminum chloride crystallization and hydrogen chloride absorption main system (opened during the polymerization reaction and the pressure in the kettle is adjusted, and closed when the pressure is reduced after the polymerization is completed);
[0056] The liquid inlet end of the PAFC slurry buffer tank is connected to the PAFC polymerization kettle and the PAFC scraper film evaporation concentrator respectively;
[0057] Further preferably, the discharge end of the polymer plate and frame filter press is connected in sequence to a PAFC filter cake hopper and a belt dryer; the liquid discharge end of the polymer plate and frame filter press is connected in sequence to a PAFC filtrate storage tank, a PAFC nanofiltration pump, a PAFC nanofiltration membrane, a PAFC buffer tank, a PAFC solution pump, a PAFC scraped film evaporation concentrator, a surface condenser, and a vacuum pump.
[0058] Further, the main system for recovering impure salts includes an impure salt solution buffer tank, an impure salt solution pump, a calcium slag plate-frame filter press, a calcium slag filter cake hopper, an impure salt scraper film evaporation concentrator, an impure salt slurry tank, an impure salt slurry pump, an impure salt plate-frame filter press, and an impure salt filter cake hopper, which are connected in sequence;
[0059] The liquid inlet end of the mixed salt solution buffer tank is respectively connected to the PAFC nanofiltration membrane of the PAFC polymerization main system and the mixed salt plate and frame filter press;
[0060] The gas outlet end of the impure salt scraper thin film evaporation concentrator is connected to the surface condenser of the PAFC polymerization main system.
[0061] Furthermore, the sodium bisulfate auxiliary system includes a bucket elevator, a screw conveyor dryer, a Mannheim reactor, a discharging screw conveyor, a concentrated sulfuric acid high-level tank, a concentrated sulfuric acid storage tank, a concentrated sulfuric acid pump, and a concentrated sulfuric acid unloading tank, which are connected in sequence; the gas outlet end of the Mannheim reactor is connected to the crystallization absorption tower of the aluminum chloride crystallization and hydrogen chloride absorption main system.
[0062] Furthermore, the gangue activation auxiliary system includes a gangue lower hopper, a gangue crusher, a gangue belt conveyor, a gangue furnace coal hopper, a gangue activation furnace, and an activated gangue crusher connected in sequence; the steam output pipe of the gangue activation furnace is connected to the PAFC polymerization kettle, the belt dryer, the PAFC scraper film evaporation concentrator, and the mixed salt scraper film evaporation concentrator of the PAFC polymerization main system, and provides the required heat source for the PAFC polymerization kettle, the belt dryer, the PAFC scraper film evaporation concentrator, the mixed salt scraper film evaporation concentrator, and the double salt evaporation concentration process; the activated gangue coming out of the discharge port of the gangue activation furnace is placed in the activated gangue storage site for cooling, and then crushed by the activated gangue crusher, and then placed in the activated gangue storage site for material preparation, and finally loaded into the activated gangue hanging hopper of the gangue acidolysis leaching main system.
[0063] Furthermore, step (1) of the method is carried out in the sodium bisulfate auxiliary system, step (2) of the method is carried out in the gangue activation auxiliary system; step (3) of the method is carried out in the gangue acid hydrolysis and leaching main system; step (4) of the method is carried out in the aluminum chloride crystallization and hydrogen chloride absorption main system; step (5) of the method is carried out in the PAFC polymerization main system; and step (6) of the method is carried out in the impurity salt recovery main system.
[0064] The overall technical concept of the present invention is as follows:
[0065] (1) The main system of coal gangue acid leaching includes two process lines:
[0066] 1) Aluminum chloride production line by acidolysis of coal gangue: The hydrochloric acid mother liquor from the crystallization plate and frame filter press and the activated coal gangue from the activated coal gangue hanging hopper are placed in the acidolysis leaching tank, and an appropriate amount of activated iron ore or iron oxide (for supplementing the iron content) is added in proportion for stirring and acidolysis leaching. The obtained aluminum chloride solution and silicon slag are discharged from the bottom and transported into the acidolysis plate and frame filter press by an acidolysis slag slurry pump for filtration. A part of the aluminum chloride solution enters the aluminum chloride mother liquor tank for buffering, and the other part enters the absorption circulation tank for absorbing hydrogen chloride gas to precipitate crystalline aluminum chloride. The silicon slag enters the acidolysis silicon slag hopper for buffering.
[0067] 2) Plate and frame washing water line: The acidic condensate and make-up water from the surface condenser enter the acidic water tank buffer, and are transported by a washing water pump into the acid hydrolysis plate and frame filter press to wash the silicon slag. The acidic washing water enters the tail gas absorption circulation tank.
[0068] (2) The main system of aluminum chloride crystallization and hydrogen chloride absorption includes three process lines:
[0069] 1) Hydrogen chloride gas line: Hydrogen chloride gas from the Mannheim reactor and PAFC polymerization kettle enters the crystallization absorption tower, starts the absorption circulation pump to use the circulating mother liquor for circulation absorption (the supplementary aluminum chloride solution in the absorption circulation tank comes from the acid hydrolysis plate and frame filter press), and precipitates crystallized aluminum chloride (AlCl3·6H2O). The unabsorbed hydrogen chloride tail gas enters the hydraulic jet pump, and the acid water pump is started to absorb with acid water.
[0070] 2) Aluminum chloride line: The aluminum chloride solution from the acid hydrolysis plate and frame press enters the absorption circulation tank, and is transported to the crystallization absorption tower by the absorption circulation pump. After absorbing the hydrogen chloride gas, crystalline aluminum chloride (AlCl3·6H2O) is precipitated, and the circulating mother liquor returns to the absorption circulation tank. The crystallized aluminum chloride slurry transported by the absorption salt pump enters the crystallization plate and frame filter press for filtration, and the crystallized filter cake enters the crystallization filter cake hopper for buffering. A part of the crystallized aluminum chloride is packaged and sold, and the other part enters the PAFC polymerization kettle for re-saturation of the aluminum chloride solution.
[0071] 3) Acidic water line: The acidic washing water from the acidolysis plate and frame filter press and the acidic condensed water from the surface condenser enter the tail gas absorption circulation tank for buffering. The acidic water pump is started to transport the acidic water into the hydraulic jet pump to absorb the hydrogen chloride tail gas from the crystallization absorption tower. The absorbed acidic water returns to the tail gas absorption circulation tank. The full flow of acidic water in the tail gas absorption circulation tank enters the absorption circulation tank.
[0072] (3) The PAFC polymerization main system includes four process lines:
[0073] 1) Aluminum chloride line: The aluminum chloride solution from the aluminum chloride mother liquor tank is transported into the PAFC polymerization kettle by an aluminum chloride mother liquor pump, and an appropriate amount of crystallized aluminum chloride wet material from the crystallization filter cake hopper is added for re-saturation.
[0074] 2) Hydrogen chloride gas line: The hydrogen chloride gas produced when aluminum chloride and ferric chloride are hydrolyzed in the PAFC polymerization reactor enters the crystallization absorption tower.
[0075] 3) PAFC line: After the polymerization is completed, the PAFC slurry from the PAFC polymerization kettle and the PAFC evaporated slurry from the PAFC scraper film evaporation concentrator enter the PAFC slurry buffer tank for buffering, and are transported by a polymerization salt pump into the polymerization plate and frame filter press for filtration. The wet material after filtration enters the PAFC filter cake hopper for buffering. The PAFC wet material in the PAFC filter cake hopper enters the belt dryer for drying, and the dried PAFC is packaged. The PAFC filtrate enters the PAFC filtrate storage tank for buffering. The PAFC filtrate in the PAFC filtrate storage tank is transported by a PAFC nanofiltration pump into the PAFC nanofiltration membrane for nanofiltration separation, and the PAFC solution enters the PAFC buffer tank for buffering, and the mixed salt solution enters the mixed salt solution buffer tank for buffering. The PAFC solution in the PAFC buffer tank is transported by a PAFC solution pump into the PAFC scraper film evaporation concentrator for evaporation and concentration, and the PAFC evaporated slurry with a solid-liquid ratio of 25-35% enters the PAFC slurry buffer tank.
[0076] 4) Water vapor line: After the polymerization is completed, negative pressure flash evaporation is carried out in the PAFC polymerization kettle, and the acidic water vapor generated enters the surface condenser for condensation, and the solution in the PAFC polymerization kettle is reduced from 150-160°C to below 60°C; the acidic water vapor generated by the PAFC scraped film evaporation concentrator during evaporation and concentration enters the surface condenser for condensation; the vacuum degree of the system is controlled at -85 to -90 kPaG through the vacuum pump and the surface condenser; part of the acidic condensed water enters the acidic water tank, and the other part enters the tail gas absorption circulation tank.
[0077] (4) The main system for recovering impurities of salts includes three process lines:
[0078] 1) Trash salt line 1 (trash salt recovery scheme 1): add an appropriate amount of pure alkali solution to the trash salt solution buffer tank for neutralization and removal of calcium and magnesium, and control the pH value at 7.0-8.0; the trash salt solution in the trash salt solution buffer tank is transported by a trash salt solution pump into a calcium slag plate-frame filter press for filtration, and the filter cake enters a calcium slag filter cake storage hopper for buffering, and is processed or utilized in batches, and the trash salt clear liquid enters a trash salt scraper film evaporation concentrator for evaporation and concentration, and a trash salt slurry with a solid-liquid ratio of 25-35% is obtained and enters a trash salt slurry tank; the trash salt slurry in the trash salt slurry tank is transported by a trash salt slurry pump into a trash salt plate-frame filter press for filtration, and the trash salt filter cake enters a trash salt filter cake hopper for buffering and packaging. The trash salt mother liquor after filtration enters a trash salt solution buffer tank for buffering.
[0079] 2) Trash salt line 2 (trash salt recovery scheme 2): add appropriate amount of pure alkali solution to the trash salt solution buffer tank for neutralization and removal of calcium and magnesium, and control the pH value at 7.0-8.0; the trash salt solution in the trash salt solution buffer tank is transported by the trash salt solution pump into the calcium slag plate and frame filter press for filtration, and the filter cake enters the calcium slag filter cake storage hopper for buffering, and is processed or utilized in batches, and the trash salt clear liquid is returned to the double salt evaporation and concentration process for recycling.
[0080] 3) Water vapor line: The water vapor generated by the scraper thin film evaporation concentrator during evaporation and concentration enters the surface condenser for condensation; the vacuum degree of the system is controlled at -85 to -90 kPaG through the vacuum pump and the surface condenser.
[0081] Compared with the prior art, the present invention has the following beneficial effects:
[0082] 1. The method of the present invention has the advantages of low energy consumption, low cost, high processing efficiency, energy saving and environmental protection, complete reaction, high product recovery rate and purity, etc., and is suitable for industrial promotion and application; all solid waste coal gangue and solid waste sodium chloride from coal chemical industry are used as production raw materials, solid waste silicon slag produced in the production process can be used as building sand, solid waste miscellaneous salt can be used as quenching salt in heat treatment, waste gas and flue gas are treated according to the national gas boiler flue gas treatment method, and waste water is returned to the front-end sewage treatment system for treatment; aluminum chloride solution is used to absorb hydrogen chloride gas to precipitate crystalline aluminum chloride (AlCl3·6H2O), there is no heat energy consumption, one part is sold as a product, and the other part is re-saturated with aluminum chloride solution, which relatively saves part of the heat energy consumption of PAFC evaporation.
[0083] 2. In the method of the present invention, negative pressure flash evaporation is carried out in a PAFC polymerization kettle at a vacuum degree of -85 to -90 kPaG, the generated acidic water vapor enters the surface condenser for condensation, and the solution in the kettle is reduced from 150 to 160° C. to below 60° C., thereby saving part of the heat energy of PAFC evaporation; water is circulated in the system (including plate and frame washing water, which is acidic condensed water in the system), and only part of the water carried away and lost by the product is supplemented; in the process of activation of coal gangue, all the carbon components of coal gangue are burned, and all its heat energy is used to produce steam for the system.
[0084] 3. The device of the present invention does not need to be equipped with a boiler system or a heating system. It adopts the method of burning fuel gas (referring to combustible gases such as natural gas, coal gas, hydrogen, etc.) and coal gangue in the coal gangue activation furnace at the same time. While realizing the activation of coal gangue, it can also produce steam as the heat source of the system, saving the investment and operation costs of the boiler; the Mannheim reactor is used to produce sodium bisulfate, and there is no need to set up a gas heating device; the crystallization absorption tower adopts an empty tower large flow multi-layer jet absorption structure, which has the advantages of simple equipment structure, large operation flexibility, good absorption effect, mature technology, and convenient operation and maintenance. etc.; since PAFC polymerization is carried out under acidic medium conditions, the PAFC polymerization kettle adopts an enamel kettle, the surface condenser adopts a graphite heat exchanger, and the solid-liquid separation equipment adopts a plate and frame filter press; membrane technology (nanofiltration membrane) is used to separate PAFC solution and impure salt solution, which has the advantages of high separation efficiency, low energy consumption, and short process route; the processing capacity of PAFC and impure salt evaporation and concentration is relatively small, and a scraper film concentration evaporator is selected for concentration and evaporation, which has the advantages of short process route, simple equipment structure, low start-up and shutdown energy consumption, mature technology, and easy operation and maintenance.
[0085] 4. The present invention selects appropriate equipment according to the requirements of each process step, and realizes the overall optimization of the device on the basis of satisfying the process requirements such as complete reaction of individual equipment. It can not only meet the needs of large-scale industrial production equipment, but also has the advantages of simple structure, complete functions, easy operation, advanced and mature technology, etc. The whole set of equipment has the advantages of low purchase cost, low production energy consumption and high processing efficiency, especially realizing the energy-saving and environmental protection effect of producing crystalline aluminum chloride and PAFC from solid waste, and basically no three wastes are generated, and has the advantages of high product recovery rate and high purity, etc., which is suitable for industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0086] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0087] Figure 1 A schematic diagram of a complete process flow of the method for producing crystalline aluminum chloride and PAFC using solid waste provided by the present invention.
[0088] Figure 2 A schematic diagram of the general process flow of the method for producing crystalline aluminum chloride and PAFC using solid waste provided by the present invention.
[0089] Figure 3 The present invention provides a schematic diagram of the process flow of the main system for acid hydrolysis and leaching of coal gangue.
[0090] Figure 4 The present invention provides a schematic diagram of the process flow of the main system for aluminum chloride crystallization and hydrogen chloride absorption.
[0091] Figure 5 This is a schematic diagram of the process flow of the PAFC polymerization main system provided by the present invention.
[0092] Figure 6 This is a schematic diagram of the process flow of the main system for recovering impurities of salts provided by the present invention.
[0093] Figure 7 The present invention provides a schematic diagram of the process flow of the sodium bisulfate auxiliary system.
[0094] Figure 8 A schematic diagram of the process flow of the gangue activation auxiliary system provided by the present invention.
[0095] Fig. 9 A schematic diagram of the general device structure of the method for producing crystalline aluminum chloride and PAFC provided by the present invention.
[0096] Fig.10 The present invention provides a schematic diagram of the specific device structure of the main system for acid hydrolysis and leaching of coal gangue.
[0097] Fig.11 The present invention provides a schematic diagram of the specific device structure of the aluminum chloride crystallization and hydrogen chloride absorption main system.
[0098] Fig.12 This is a schematic diagram of the specific device structure of the PAFC polymerization main system provided by the present invention.
[0099] Fig.13 This is a schematic diagram of the specific device structure of the main system for recovering impurities of salts provided by the present invention.
[0100] Fig.14 The present invention provides a schematic diagram of the specific device structure of the sodium bisulfate auxiliary system.
[0101] Fig.15 A schematic diagram of the specific device structure of the gangue activation auxiliary system provided by the present invention.
[0102] Legend:
[0103] 1. Coal gangue acid leaching main system; 2. Aluminum chloride crystallization and hydrogen chloride absorption main system; 3. PAFC polymerization main system; 4. Miscellaneous salt recovery main system; 5. Sodium bisulfate auxiliary system; 6. Coal gangue activation auxiliary system;
[0104] 1-1, activated gangue hanging hopper; 1-2, acid hydrolysis leaching tank; 1-3, acid hydrolysis slurry pump; 1-4, acid hydrolysis plate and frame filter press; 1-5, acid hydrolysis silicon slag hopper; 1-6, washing water pump; 1-7, acid water tank;
[0105] 2-1, crystallization absorption tower; 2-2, absorption circulation tank; 2-3, absorption circulation pump; 2-4, absorption salt pump; 2-5, crystallization plate and frame filter press; 2-6, crystallization filter cake hopper; 2-7, hydraulic jet pump; 2-8, acidic water pump; 2-9, tail gas absorption circulation tank;
[0106] 3-1, aluminum chloride mother liquor tank; 3-2, aluminum chloride mother liquor pump; 3-3, PAFC polymerization kettle; 3-4, PAFC slurry buffer tank; 3-5, polymerization salt mining pump; 3-6, polymerization plate and frame filter press; 3-7, PAFC filter cake hopper; 3-8, belt dryer; 3-9, PAFC filtrate storage tank; 3-10, PAFC nanofiltration pump; 3-11, PAFC nanofiltration membrane; 3-12, PAFC buffer tank; 3-13, PAFC solution pump; 3-14, PAFC scraper thin film evaporation concentrator; 3-15, surface condenser; 3-16, vacuum pump;
[0107] 4-1, miscellaneous salt solution buffer tank; 4-2, miscellaneous salt solution pump; 4-3, calcium slag plate and frame filter press; 4-4, calcium slag filter cake hopper; 4-5, miscellaneous salt scraper film evaporation concentrator; 4-6, miscellaneous salt slurry tank; 4-7, miscellaneous salt slurry pump; 4-8, miscellaneous salt plate and frame filter press; 4-9, miscellaneous salt filter cake hopper;
[0108] 5-1, bucket elevator; 5-2, screw conveyor dryer; 5-3, Mannheim reactor; 5-4, discharge screw conveyor; 5-5, concentrated sulfuric acid high-level tank; 5-6, concentrated sulfuric acid storage tank; 5-7, concentrated sulfuric acid pump; 5-8, concentrated sulfuric acid unloading tank;
[0109] 6-1. Gangue hopper; 6-2. Gangue crusher; 6-3. Gangue belt conveyor; 6-4. Coal hopper in front of gangue furnace; 6-5. Gangue activation furnace; 6-6. Activated gangue crusher. DETAILED DESCRIPTION
[0110] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0111] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0112] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0113] Embodiment 1:
[0114] A method for producing crystalline aluminum chloride and PAFC using solid waste, the process flow is as follows: Figures 1 to 8 As shown, the following steps are included:
[0115] (1) solid waste salt sodium chloride (containing 3-5% water) is preheated to 140-150°C during drying, and reacts with 98% concentrated sulfuric acid in a Mannheim reactor to produce sodium bisulfate by exothermic reaction, with the reaction temperature controlled at 220-230°C, and hydrogen chloride gas is produced by the reaction; solid waste salt sodium chloride includes solid waste salt sodium chloride obtained from various sewage and wastewater treatment and chemical production;
[0116] (2) The gangue is placed in a gangue activation furnace and the furnace temperature is controlled to be 650-700°C for high-temperature activation. At the same time, deionized water is placed in the furnace to indirectly heat the gangue and the heat energy generated by the combustion of gas to produce 700-800 kPaG steam for system use; the high-temperature activated gangue is cooled and crushed to achieve further mechanical activation; the main components of gangue are Al2O3 and SiO2, and also contain small amounts of Fe2O3, CaO, MgO, TiO2, Na2O, K2O, etc.; the raw materials that can replace gangue are all substances containing aluminum or aluminum oxide;
[0117] (3) Adding activated coal gangue and hydrochloric acid mother liquor from the crystallization plate and frame filter press into the acidolysis leaching tank, and adding an appropriate amount of iron ore or iron oxide (for supplementing the iron content) in proportion for stirring and acidolysis leaching, the leaching time is about 0.8 to 1.2 hours, and the pH value is always controlled to be less than 4 to prevent the generated AlCl3 and FeCl3 from being hydrolyzed; after the acidolysis leaching is completed, the acidolysis slurry pump is started under stirring to transport all the materials (aluminum chloride solution and silicon slag) in the acidolysis leaching tank into the acidolysis plate and frame filter press for filtration, and the filtrate (aluminum chloride solution) is respectively entered into the aluminum chloride mother liquor tank and the absorption circulation tank for buffering in proportion; when the inlet pressure of the acidolysis plate and frame filter press reaches the rated pressure, the outlet flow of the filtrate is transferred to the tail gas absorption circulation tank, and the washing water pump is started to wash the filter residue with a rated amount of water, and the washing liquid enters the tail gas absorption circulation tank. After the washing is completed, the plate and frame are slag-proof, and the silicon slag enters the acidolysis silicon slag hopper for buffering; the silicon slag can be shipped and sold as building materials;
[0118] (4) The hydrogen chloride gas from the Mannheim reactor and the PAFC polymerization kettle enters the crystallization absorption tower, and the absorption circulation pump is started to circulate and absorb with the circulating mother liquor (the supplementary aluminum chloride solution of the absorption circulation tank comes from the acid hydrolysis plate and frame filter press), and crystalline aluminum chloride (AlCl3·6H2O) is precipitated. The crystallized aluminum chloride slurry transported by the absorption salt pump enters the crystallization plate and frame filter press for filtration, and the crystallized filter cake enters the crystallization filter cake hopper for buffering. A part of the crystallized aluminum chloride is packaged and sold, and the other part enters the PAFC polymerization kettle for re-saturation of the aluminum chloride solution. The hydrogen chloride tail gas from the crystallization absorption tower enters the hydraulic jet pump, and the acid water pump is started to absorb with acid water (the supplementary water of the absorption circulation tank comes from the acid washing water from the acid hydrolysis plate and frame filter press and the acid cold water of the surface condenser). The absorbed acid water returns to the tail gas absorption circulation tank, and the acid water flowing in the tail gas absorption circulation tank enters the absorption circulation tank.
[0119] (5) Add the crystallization filter cake buffered in the crystallization filter cake storage hopper and the aluminum chloride solution delivered by the aluminum chloride mother liquor pump into the PAFC polymerization kettle in a certain ratio. First, start the stirring to mix the materials evenly and make them heavy saturated, then pass 700-800kPaG steam into its jacket to heat and raise the temperature. When the temperature of the material in the kettle rises to 150-160°C, control the pressure in the kettle at 0.5-0.6MPaG for hydrolysis and polymerization, and control the polymerization time to 30-50 minutes; the hydrogen chloride gas generated during hydrolysis enters the crystallization absorption tower; after the polymerization is completed, the kettle is subjected to negative pressure flash evaporation, the acidic water vapor generated enters the surface condenser for condensation, and the solution in the kettle is reduced from 150-160°C to below 60°C. PAFC slurry and PAFC evaporation slurry from PAFC scraper membrane evaporation concentrator enter PAFC slurry buffer tank for buffering, and are transported by polymer salt pump into polymer plate and frame filter press for filtration. The wet material after filtration enters PAFC filter cake hopper for buffering. The PAFC wet material in PAFC filter cake hopper enters belt dryer for drying, and the dried PAFC is packaged. PAFC filtrate enters PAFC filtrate storage tank for buffering. PAFC filtrate in PAFC filtrate storage tank is transported by PAFC nanofiltration pump into PAFC nanofiltration for nanofiltration separation, PAFC solution enters PAFC buffer tank for storage, and impure salt solution enters impure salt solution buffer tank for buffering. PAFC solution in PAFC buffer tank is transported by PAFC solution pump into PAFC scraper membrane evaporation concentrator for evaporation and concentration, and PAFC evaporation slurry with solid-liquid ratio of 25-35% enters PAFC slurry buffer tank, and acidic water vapor enters surface condenser for condensation. The vacuum degree of the system is controlled at -85 to -90 kPaG through a vacuum pump and a surface condenser; the acidic water vapor from the PAFC scraper film evaporation concentrator and the water vapor evaporated from the mixed salt scraper film evaporation concentrator enter the surface condenser, and the acidic water vapor is condensed in the surface condenser using circulating water. Part of the condensed acidic condensed water enters the acidic water tank for washing silicon slag, and the other part enters the tail gas absorption circulation tank for absorbing the tail hydrogen chloride gas.
[0120] (6) Add an appropriate amount of soda ash to the mixed salt solution buffer tank for neutralization and removal of calcium and magnesium impurities, and control the pH value to 7.0-8.0. The mixed salt solution in the mixed salt solution buffer tank is transported by the mixed salt solution pump to the calcium slag plate and frame filter press for filtration, and the filter cake is sent to the calcium slag filter cake storage hopper for buffering and processed or utilized in batches. The mixed salt clear liquid is processed according to one of the following two schemes according to the potassium chloride content:
[0121] 1) The potassium chloride content is too high to meet the quality requirements of sodium bisulfate: the salt clear liquid enters the salt scraper thin film evaporation concentrator for evaporation and concentration, and the salt slurry with a solid-liquid ratio of 25-35% is obtained and enters the salt slurry tank. The salt slurry in the salt slurry tank is transported by the salt slurry pump to the salt plate and frame filter press for filtration, and the salt filter cake enters the salt filter cake hopper for buffering and packaging. The salt mother liquor after filtration enters the salt solution buffer tank for buffering.
[0122] 2) The potassium chloride content is low and can meet the requirements of qualified sodium bisulfate quality: the impure salt clear liquid is returned to the double salt evaporation and concentration process for recycling.
[0123] The design indicators of the above products are as follows:
[0124] 1. Sodium bisulfate product design indicators:
[0125] (I) Quality indicators of sodium bisulfate raw materials:
[0126] 1. Solid waste salt sodium chloride: (w / w%)
[0127] NaCl ≥ 95.0%, Na2SO4 ≤ 0.03%, Na2CO3 ≤ 0.07%, COD ≤ 0.02%, water-insoluble impurities ≤ 0.10%, moisture ≤ 5.0%;
[0128] 2. 98% sulfuric acid: (w / w%)
[0129] H2SO4≥98.0%, ash≤0.1%, moisture≤2.0%.
[0130] (II) Sodium bisulfate raw material consumption index:
[0131] 1. Solid waste salt sodium chloride: 515kg / t;
[0132] 2. 98% sulfuric acid: 835kg / t.
[0133] (III) Sodium bisulfate product quality indicators (w / w%):
[0134] NaHSO4≥98.0%, KHSO4≤0.50%, NaCl≤0.10%, KCl≤0.01%, COD≤0.01%, moisture≤0.10%.
[0135] 2. Design indicators of crystalline aluminum chloride products
[0136] (I) Raw material quality indicators:
[0137] 1. Hydrogen chloride gas (w / w%)
[0138] HCl ≥ 91.5%, CO2 ≤ 0.10%, water ≤ 8.5%;
[0139] 2. Coal gangue (w / w%)
[0140] Al2O3≥23.00%, Fe2O3≥2.40%, SiO2≤41.60%, SO2≤0.60%, K2O+Na2O≤2.00%,
[0141] CaO+MgO≤0.70%, TiO2≤0.80%, heavy metal≤0.01%, loss on ignition≤28.85%;
[0142] 3. Iron oxide (qualified): (w / w%)
[0143] Fe2O3≥98.5%, SiO2≤0.04%, CaO≤0.05%, Al2O3≤0.05%, MnO≤0.5%, SO4 2- ≤0.20%,
[0144] TaO≤0.02%, MgO≤0.05%
[0145] 4. Iron ore (hematite grade 1): (w / w%)
[0146] Fe2O3≥91.43% (Fe≥64.00%), SiO2≤8.00%, S≤0.10%, P≤0.10%, Cu≤0.20%, As
[0147] ≤0.10%
[0148] (II) Raw material consumption indicators:
[0149] 1. Hydrogen chloride gas (100%): 430kg / t;
[0150] 2. Coal gangue: 1600kg / t;
[0151] 3. Iron oxide: 15kg / t (or first grade hematite: 16.5kg / t).
[0152] (III) Product quality indicators (w / w%):
[0153] AlCl3·6H2O≥87.0%, FeCl3·6H2O≥8.5%, NaCl+NaCl≤0.30%, HCl≤1.20%, heavy metals
[0154] ≤0.01%, water-insoluble impurities ≤0.10%, free water ≤5.00%, pH = 1.4 ~ 1.7. (Only applicable to sewage treatment, the flocculation effect is better when AlCl3·6H2O and FeCl3·6H2O are hydrolyzed simultaneously)
[0155] 3. PAFC product design indicators
[0156] (I) Raw material quality indicators:
[0157] 1. Hydrogen chloride gas (w / w%)
[0158] HCl ≥ 91.5%, CO2 ≤ 0.10%, water ≤ 8.5%;
[0159] 2. Coal gangue (w / w%)
[0160] Al2O3≥23.00%, Fe2O3≥2.40%, SiO2≤41.60%, SO2≤0.60%, K2O+Na2O≤2.00%,
[0161] CaO+MgO≤0.70%, TiO2≤0.80%, heavy metal≤0.01%, loss on ignition≤28.85%;
[0162] 3. Iron oxide (qualified): (w / w%)
[0163] Fe2O3≥98.5%, SiO2≤0.04%, CaO≤0.05%, Al2O3≤0.05%, MnO≤0.5%, SO4 2- ≤0.20%,
[0164] TaO≤0.02%, MgO≤0.05%
[0165] 4. Iron ore (hematite grade 1): (w / w%)
[0166] Fe2O3≥91.43% (Fe≥64.00%), SiO2≤8.00%, S≤0.10%, P≤0.10%, Cu≤0.20%, As
[0167] ≤0.10%
[0168] (II) Raw material consumption indicators:
[0169] 1. Hydrogen chloride gas (100%): 570kg / t;
[0170] 2. Coal gangue: 1750kg / t;
[0171] 3. Iron oxide: 16.5kg / t (or first grade hematite: 18.5kg / t).
[0172] (III) Product quality indicators (w / w%):
[0173] PAFC≥98.5% (including Al2O3≥39.5%, Fe2O3≥5.0%), water-insoluble impurities≤0.75%, heavy metals≤0.30%, pH=4.5~5.5.
[0174] Embodiment 2:
[0175] An apparatus for the method for producing crystalline aluminum chloride and PAFC in Example 1, such as Figures 9 to 15 As shown. It includes four main systems and two auxiliary systems (such as Fig. 9 As shown), there are four main systems: coal gangue acid hydrolysis and leaching main system 1, aluminum chloride crystallization and hydrogen chloride absorption main system 2, PAFC polymerization main system 3 and impurity salt recovery main system 4; two subsidiary systems: sodium bisulfate subsidiary system 5 (mainly providing hydrogen chloride gas for aluminum chloride crystallization and hydrogen chloride absorption main system) and coal gangue activation subsidiary system 6 (mainly providing activated coal gangue for coal gangue acid hydrolysis and leaching main system, and also providing required steam for this system and the previous system).
[0176] In this embodiment (such as Fig.10 As shown), the main system 1 for acid hydrolysis and leaching of coal gangue includes an activated coal gangue hanging hopper 1-1, an acid hydrolysis leaching tank 1-2, an acid hydrolysis slurry pump 1-3, an acid hydrolysis plate and frame filter press 1-4, and an acid hydrolysis silicon slag hopper 1-5 which are connected in sequence;
[0177] The liquid inlet end of the acidolysis leaching tank 1-2 is connected to the crystallization plate-frame filter press 2-5 of the aluminum chloride crystallization and hydrogen chloride absorption main system 2;
[0178] The liquid outlet end of the acidolysis plate and frame filter press 1-4 is respectively connected to the absorption circulation tank 2-2 and the tail gas absorption circulation tank 2-9 of the aluminum chloride crystallization and hydrogen chloride absorption main system 2, and the aluminum chloride mother liquor tank 3-1 of the PAFC polymerization main system 3; the material outlet end of the acidolysis plate and frame filter press 1-4 is connected to the acidolysis silicon slag hopper 1-5; the acidolysis plate and frame filter press 1-4 is also connected to a washing water pump 1-6 and an acidic water tank 1-7.
[0179] In this embodiment (such as Fig.11 As shown), the main system 2 for aluminum chloride crystallization and hydrogen chloride absorption includes a crystallization absorption tower 2-1, an absorption circulation tank 2-2, an absorption circulation pump 2-3, an absorption salt pump 2-4, a crystallization plate and frame filter press 2-5, and a crystallization filter cake hopper 2-6 connected in sequence;
[0180] The air inlet end of the crystallization absorption tower 2-1 is connected to the Mannheim reactor 5-3 of the sodium bisulfate auxiliary system 5 and the PAFC polymerization kettle 3-3 of the PAFC polymerization main system 3 respectively; the air outlet end of the crystallization absorption tower 2-1 is connected to the hydraulic jet pump 2-7, and the hydraulic jet pump 2-7 is connected to the acid water pump 2-8 and the tail gas absorption circulation tank 2-9 in turn;
[0181] The liquid inlet end of the absorption circulation tank 2-2 is respectively connected to the tail gas absorption circulation tank 2-9, the crystallization absorption tower 2-1, and the acid hydrolysis plate-frame filter press 1-4 of the coal gangue acid hydrolysis and leaching main system 1;
[0182] The liquid outlet of the crystallization plate-frame filter press 2-5 is connected to the acid hydrolysis leaching tank 1-2 of the coal gangue acid hydrolysis leaching main system 1, and the material outlet of the crystallization plate-frame filter press 2-5 is connected to the crystallization filter cake hopper 2-6;
[0183] The discharge end of the crystallization filter cake hopper 2 - 6 is connected to the PAFC polymerization kettle 3 - 3 of the PAFC polymerization main system 3 .
[0184] In this embodiment (such as Fig.12 As shown), the PAFC polymerization main system 3 includes an aluminum chloride mother liquor tank 3-1, an aluminum chloride mother liquor pump 3-2, a PAFC polymerization kettle 3-3, a PAFC slurry buffer tank 3-4, a polymerization salt pump 3-5, and a polymerization plate and frame filter press 3-6, which are connected in sequence;
[0185] The discharge end of the polymer plate-frame filter press 3-6 is sequentially connected to a PAFC filter cake hopper 3-7 and a belt dryer 3-8; the liquid discharge end of the polymer plate-frame filter press 3-6 is sequentially connected to a PAFC filtrate storage tank 3-9, a PAFC nanofiltration pump 3-10, a PAFC nanofiltration membrane 3-11, a PAFC buffer tank 3-12, a PAFC solution pump 3-13, a PAFC scraper film evaporation concentrator 3-14, a surface condenser 3-15, and a vacuum pump 3-16;
[0186] The liquid inlet end of the aluminum chloride mother liquor tank 3-1 is connected to the acid hydrolysis plate-frame filter press 1-4 of the coal gangue acid hydrolysis and leaching main system 1;
[0187] The feed end of the PAFC polymerization kettle 3-3 is connected to the crystallization filter cake hopper 2-6 of the main system 2 for aluminum chloride crystallization and hydrogen chloride absorption; the liquid inlet end of the PAFC polymerization kettle 3-3 is connected to the liquid outlet end of the aluminum chloride mother liquor pump 3-2; the gas outlet end of the PAFC polymerization kettle 3-3 is respectively connected to the surface condenser 3-15 (opened when the pressure is reduced after the polymerization is completed, and closed during the polymerization reaction) and the crystallization absorption tower 2-1 of the main system 2 for aluminum chloride crystallization and hydrogen chloride absorption (opened during the polymerization reaction and the pressure in the kettle is adjusted, and closed when the pressure is reduced after the polymerization is completed);
[0188] The liquid inlet end of the PAFC slurry buffer tank 3-4 is connected to the PAFC polymerization kettle 3-3 and the PAFC scraper film evaporation concentrator 3-14 respectively.
[0189] In this embodiment (such as Fig.13As shown), the main system for recovering impurities salts 4 comprises an impurity salt solution buffer tank 4-1, an impurity salt solution pump 4-2, a calcium slag plate-frame filter press 4-3, a calcium slag filter cake hopper 4-4, an impurity salt scraper film evaporation concentrator 4-5, an impurity salt slurry tank 4-6, an impurity salt slurry pump 4-7, an impurity salt plate-frame filter press 4-8, and an impurity salt filter cake hopper 4-9, which are connected in sequence;
[0190] The liquid inlet end of the mixed salt solution buffer tank 4-1 is respectively connected to the PAFC nanofiltration membrane 3-11 of the PAFC polymerization main system 3 and the mixed salt plate and frame filter press 4-8;
[0191] The gas outlet end of the impure salt scraper thin film concentration evaporator 4 - 5 is connected to the surface condenser 3 - 15 of the PAFC polymerization main system 3 .
[0192] In this embodiment (such as Fig.14 As shown), the sodium bisulfate auxiliary system 5 includes a bucket elevator 5-1, a screw conveyor dryer 5-2, a Mannheim reactor 5-3, a discharge screw conveyor 5-4, a concentrated sulfuric acid high-level tank 5-5, a concentrated sulfuric acid storage tank 5-6, a concentrated sulfuric acid pump 5-7, and a concentrated sulfuric acid unloading tank 5-8 connected in sequence;
[0193] The gas outlet end of the Mannheim reactor 5 - 3 is connected to the crystallization absorption tower 2 - 1 of the aluminum chloride crystallization and hydrogen chloride absorption main system 2 .
[0194] In this embodiment (such as Fig.15 As shown), the gangue activation auxiliary system 6 includes a gangue lower hopper 6-1, a gangue crusher 6-2, a gangue belt conveyor 6-3, a gangue furnace coal hopper 6-4, a gangue activation furnace 6-5, and an activated gangue crusher 6-6 which are connected in sequence;
[0195] The steam output pipe of the gangue activation furnace 6-5 is connected to the PAFC polymerization kettle 3-3, the belt dryer 3-8, the PAFC scraper film evaporation concentrator 3-14 of the PAFC polymerization main system 3 and the scraper film evaporation concentrator 4-5 of the scraper salt recovery main system 4, and provides the required heat source for the PAFC polymerization kettle 3-3, the belt dryer 3-8, the PAFC scraper film evaporation concentrator 3-14 of the PAFC polymerization main system 3 and the scraper film evaporation concentrator 4-5 of the scraper salt recovery main system 4 and the double salt evaporation concentration process;
[0196] The activated gangue coming out of the discharge port of the gangue activation furnace 6-5 is placed in the activated gangue storage site for cooling, crushed by the activated gangue crusher 6-6, and then placed in the activated gangue storage site for material preparation, and finally loaded into the activated gangue hanging hopper 1-1 of the gangue acidolysis leaching main system 1.
Claims
1. A method for producing crystalline aluminum chloride and polyaluminum ferric chloride using solid waste, characterized in that: The following steps are involved: (1) Drying the solid waste salt sodium chloride at 140-150°C and preheating it, reacting it with concentrated sulfuric acid to generate sodium bisulfate and hydrogen chloride gas, and controlling the reaction temperature to rise to 220-230°C; (2) subjecting the gangue to high-temperature activation and mechanical activation to obtain activated gangue; the temperature of the high-temperature activation is 650-700°C; during the high-temperature activation, fuel gas is introduced into the activation furnace for combustion-aiding heating, and ion-free water is used to produce 700-800 kPaG steam, which is used for heating and raising the temperature of the hydrolysis and polymerization reactions in step (5); (3) mixing the activated coal gangue obtained in step (2) with hydrochloric acid and / or the hydrochloric acid mother liquor obtained in step (4), and adding iron ore or iron oxide for stirring and acid hydrolysis leaching to obtain an aluminum chloride solution containing ferric chloride and silicon slag; the stirring and acid hydrolysis leaching time is 0.8 to 1.2 hours, and the pH value is controlled to be less than 4 during the stirring and acid hydrolysis leaching; (4) allowing the aluminum chloride solution containing ferric chloride obtained in step (3) to absorb the hydrogen chloride gas obtained in step (1) and / or step (5) to precipitate crystalline aluminum chloride, and the obtained hydrochloric acid mother liquor is returned to step (3) for repeated utilization; (5) The aluminum chloride solution containing ferric chloride obtained in step (3) is mixed with the crystalline aluminum chloride obtained in step (4), and stirred to make it re-saturated. Hydrolysis and polymerization reaction are carried out at 150-160° C. and 0.5-0.6 MPaG for 30-50 min, and hydrogen chloride gas is released. The obtained polymer product is subjected to evaporation, crystallization, pressure filtration, and drying to obtain a polyaluminum ferric chloride (PAFC) product. The specific operation of the evaporation and crystallization is as follows: negative pressure flash evaporation is carried out in a PAFC polymerization kettle at a vacuum degree of -85 to -90 kPaG, and the generated acidic water vapor enters a surface condenser for condensation, and the solution in the kettle is cooled from 150-160° C. to below 60° C., and part of the condensed acidic condensed water enters an acidic water tank for washing silicon slag, and the other part enters a tail gas absorption circulation tank for absorbing the tail hydrogen chloride gas; and the slurry in the PAFC polymerization kettle is subjected to pressure filtration and drying to obtain a PAFC product; (6) The liquid remaining after evaporation and crystallization in step (5) is separated into a salt solution by nanofiltration, and a soda ash solution is added for neutralization and impurity removal before recycling; the recycling specifically comprises the following steps: when the potassium chloride content in the salt solution after impurity removal is high, the salt solution after impurity removal is evaporated and concentrated to obtain a salt slurry with a solid-liquid ratio of 25 to 35%, and then the salt is recycled after dehydration by plate and frame filter pressing; when the potassium chloride content in the salt solution after impurity removal is low, the salt solution after impurity removal is returned to step (5) and mixed with the aluminum chloride solution containing ferric chloride and the crystallized aluminum chloride for recycling.
2. The method according to claim 1, characterized in that In step (1), the solid waste salt sodium chloride is solid waste salt sodium chloride obtained from various sewage, wastewater treatment or chemical production, and its water content is 3-5%; the concentrated sulfuric acid is 98% concentrated sulfuric acid.
3. The method according to claim 1, characterized in that In step (2), the components of the coal gangue include multiple ones of Al2O3, SiO2, Fe2O3, CaO, MgO, TiO2, Na2O, and K2O; the specific operation of the mechanical activation is: crushing the coal gangue after high-temperature activation.
4. The method according to any one of claims 1 to 3, characterized in that In step (6), the impure salt is a mixed salt of any one or more of sodium chloride, potassium chloride, calcium chloride and magnesium chloride, and the impure salt is acidic.
5. A device for the method according to any one of claims 1 to 4, characterized in that: The device comprises a main system for acid hydrolysis and leaching of coal gangue (1), a main system for crystallization of aluminum chloride and absorption of hydrogen chloride (2), a main system for polymerization of PAFC (3), and a main system for recovery of impurities (4) which are connected in sequence. The device also comprises a sodium bisulfate auxiliary system (5) connected to the main system for crystallization of aluminum chloride and absorption of hydrogen chloride (2), and a coal gangue activation auxiliary system (6) connected to the main system for acid hydrolysis and leaching of coal gangue (1); The coal gangue acid leaching main system (1) comprises an activated coal gangue hanging hopper (1-1), an acid leaching tank (1-2), an acid slurry pump (1-3), an acid plate and frame filter press (1-4), and an acid silicon slag hopper (1-5) which are connected in sequence; The aluminum chloride crystallization and hydrogen chloride absorption main system (2) comprises a crystallization absorption tower (2-1), an absorption circulation tank (2-2), an absorption circulation pump (2-3), an absorption salt pump (2-4), a crystallization plate and frame filter press (2-5), and a crystallization filter cake hopper (2-6) which are connected in sequence; The PAFC polymerization main system (3) comprises an aluminum chloride mother liquor tank (3-1), an aluminum chloride mother liquor pump (3-2), a PAFC polymerization kettle (3-3), a PAFC slurry buffer tank (3-4), a polymerization salt extraction pump (3-5), and a polymerization plate and frame filter press (3-6) which are connected in sequence; The main system for recovering impure salts (4) comprises an impure salt solution buffer tank (4-1), an impure salt solution pump (4-2), a calcium slag plate-frame filter press (4-3), a calcium slag filter cake hopper (4-4), an impure salt scraper thin-film concentration evaporator (4-5), an impure salt slurry tank (4-6), an impure salt slurry pump (4-7), an impure salt plate-frame filter press (4-8), and an impure salt filter cake hopper (4-9) which are connected in sequence; The sodium bisulfate auxiliary system (5) comprises a bucket elevator (5-1), a screw conveyor dryer (5-2), a Mannheim reactor (5-3), a discharge screw conveyor (5-4), a concentrated sulfuric acid high-level tank (5-5), a concentrated sulfuric acid storage tank (5-6), a concentrated sulfuric acid pump (5-7), and a concentrated sulfuric acid unloading tank (5-8) which are connected in sequence; The gangue activation auxiliary system (6) comprises a gangue lower hopper (6-1), a gangue crusher (6-2), a gangue belt conveyor (6-3), a gangue furnace front coal hopper (6-4), a gangue activation furnace (6-5), and an activated gangue crusher (6-6) which are connected in sequence.
6. The device according to claim 5, characterized in that The liquid inlet end of the acid hydrolysis leaching tank (1-2) is connected to the crystallization plate-frame filter press (2-5) of the aluminum chloride crystallization and hydrogen chloride absorption main system (2); The liquid outlet end of the acid hydrolysis plate-frame filter press (1-4) is respectively connected to the absorption circulation tank (2-2) and tail gas absorption circulation tank (2-9) of the aluminum chloride crystallization and hydrogen chloride absorption main system (2), and the aluminum chloride mother liquor tank (3-1) of the PAFC polymerization main system (3); the material outlet end of the acid hydrolysis plate-frame filter press (1-4) is connected to the acid hydrolysis silicon slag hopper (1-5); the acid hydrolysis plate-frame filter press (1-4) is also connected to a washing water pump (1-6) and an acidic water tank (1-7).
7. The device according to claim 6, characterized in that The air inlet end of the crystallization absorption tower (2-1) is respectively connected to the Mannheim reactor (5-3) of the sodium bisulfate auxiliary system (5) and the PAFC polymerization kettle (3-3) of the PAFC polymerization main system (3); the air outlet end of the crystallization absorption tower (2-1) is connected to a hydraulic jet pump (2-7), and the hydraulic jet pump (2-7) is sequentially connected to an acidic water pump (2-8) and a tail gas absorption circulation tank (2-9); The liquid inlet end of the absorption circulation tank (2-2) is respectively connected to the tail gas absorption circulation tank (2-9), the crystallization absorption tower (2-1), and the acid hydrolysis plate-frame filter press (1-4) of the coal gangue acid hydrolysis and leaching main system (1); The liquid outlet end of the crystallization plate-frame filter press (2-5) is connected to the acid hydrolysis leaching tank (1-2) of the coal gangue acid hydrolysis leaching main system (1); the material outlet end of the crystallization plate-frame filter press (2-5) is connected to the crystallization filter cake hopper (2-6); The discharge end of the crystallization filter cake hopper (2-6) is connected to the PAFC polymerization kettle (3-3) of the PAFC polymerization main system (3).
8. The device according to claim 7, characterized in that The liquid inlet end of the aluminum chloride mother liquor tank (3-1) is connected to the acid hydrolysis plate-frame filter press (1-4) of the coal gangue acid hydrolysis and leaching main system (1); The feed end of the PAFC polymerization kettle (3-3) is connected to the crystallization filter cake hopper (2-6) of the aluminum chloride crystallization and hydrogen chloride absorption main system (2); the liquid inlet end of the PAFC polymerization kettle (3-3) is connected to the liquid outlet end of the aluminum chloride mother liquor pump (3-2); the gas outlet end of the PAFC polymerization kettle (3-3) is respectively connected to the surface condenser (3-15) and the crystallization absorption tower (2-1) of the aluminum chloride crystallization and hydrogen chloride absorption main system (2); The liquid inlet end of the PAFC slurry buffer tank (3-4) is respectively connected to the PAFC polymerization kettle (3-3) and the PAFC scraper film evaporation concentrator (3-14).
9. The device according to claim 8, characterized in that The material discharge end of the polymer plate and frame filter press (3-6) is connected in sequence to a PAFC filter cake hopper (3-7) and a belt dryer (3-8); the liquid discharge end of the polymer plate and frame filter press (3-6) is connected in sequence to a PAFC filtrate storage tank (3-9), a PAFC nanofiltration pump (3-10), a PAFC nanofiltration membrane (3-11), a PAFC buffer tank (3-12), a PAFC solution pump (3-13), a PAFC scraper film evaporation concentrator (3-14), a surface condenser (3-15), and a vacuum pump (3-16).
10. The device according to claim 9, characterized in that The liquid inlet end of the impure salt solution buffer tank (4-1) is respectively connected to the PAFC nanofiltration membrane (3-11) of the PAFC polymerization main system (3) and the impure salt plate and frame filter press (4-8); The gas outlet end of the impure salt scraper thin film concentration evaporator (4-5) is connected to the surface condenser (3-15) of the PAFC polymerization main system (3).
11. The device according to claim 10, characterized in that The gas outlet end of the Mannheim reactor (5-3) is connected to the crystallization absorption tower (2-1) of the aluminum chloride crystallization and hydrogen chloride absorption main system (2).
12. The device according to claim 11, characterized in that The steam output pipe of the gangue activation furnace (6-5) is connected to the PAFC polymerization kettle (3-3), the belt dryer (3-8), the PAFC scraper film evaporation concentrator (3-14) of the PAFC polymerization main system (3) and the impure salt scraper film evaporation concentrator (4-5) of the impure salt recovery main system 4.
13. The device according to any one of claims 5 to 12, characterized in that: Step (1) of the method is carried out in the sodium bisulfate auxiliary system (5), step (2) of the method is carried out in the gangue activation auxiliary system (6); step (3) of the method is carried out in the gangue acid hydrolysis and leaching main system (1); step (4) of the method is carried out in the aluminum chloride crystallization and hydrogen chloride absorption main system (2); step (5) of the method is carried out in the PAFC polymerization main system (3); and step (6) of the method is carried out in the impurity salt recovery main system (4).