pH and temperature dual-responsive Janus magnetic composite particles and their applications

By grafting PNIPAM and PAA on the surface of Fe3O4@SiO2 nanoparticles, Janus magnetic composite particles with dual responsiveness are prepared, which solves the limitations of existing materials in functional regulation and application, and realizes multifunctionalization and intelligence The integrated interface activity and adsorption performance have magnetic recovery functions, which enhances the application value of the materials.

CN116478349BInactive Publication Date: 2024-11-15GUANGDONG UNIV OF PETROCHEMICAL TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310517129.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing temperature and pH dual-responsive materials have limitations in functional regulation and application, especially in biomedical and interface activity, and lack of versatile and intelligent solutions.

Method used

By grafting polyN-isopropylacrylamide (PNIPAM) and polyacrylic acid (PAA) on the surface of Fe3O4@SiO2 nanoparticles, Janus magnetic composite particles with dual responsiveness were prepared and pyrolysis was used to treat high temperature and pH. The design of the core-shell structure realizes the multifunctionalization and magnetic properties of the material.

Benefits of technology

It realizes the control of responsive interface activity and adsorption performance for external temperature and pH, has magnetic recovery function, reduces usage costs, and demonstrates the application potential of multifunctional and intelligent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116478349B_ABST
    Figure CN116478349B_ABST
Patent Text Reader

Abstract

The present invention relates to pH and temperature dual-responsive Janus magnetic composite particles and applications. The preparation method of the pH and temperature dual-responsive Janus magnetic composite particles comprises: a) preparing Fe3O4 magnetic particles by high-temperature pyrolysis; b) preparing Fe3O4@SiO2 nanoparticles with a core-shell structure; c) grafting poly-N-isopropylacrylamide PNIPAM and polyacrylic acid PAA on one side of the surface of the Fe3O4@SiO2 nanoparticles with a core-shell structure to prepare pH and temperature dual-responsive Janus magnetic nanocomposite particles. The interface activity and adsorption performance of the pH and temperature dual-responsive Janus magnetic composite particles can respond to the external temperature and pH respectively, realizing the multifunctional and intelligent application of the composite particles, and at the same time, they also have magnetism and can be recycled and reused through an external magnetic field, saving the use cost and having good application economy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a Janus nano material, and in particular to a pH and temperature dual-responsive Janus magnetic composite particle and an application thereof. Background Art

[0002] Temperature and pH dual-responsive materials are a special type of smart materials that can respond to changes in temperature and pH at the same time and undergo corresponding changes in structure, performance or function. Under specific temperature and pH conditions, these materials will undergo phase change, gelation, swelling, ion adsorption and other phenomena, thereby achieving regulation of material properties. This dual responsiveness gives the material richer functional regulation and application potential. In the fields of biomedicine, environmental protection, chemical sensors, etc., temperature and pH dual-responsive materials have high application value.

[0003] Janus materials are composite materials with two or more regions of different properties, and their surfaces usually exhibit two or more different chemical or physical properties, such as hydrophilic / hydrophobic, oleophilic / oleophobic, charged / uncharged, etc. Amphiphilic Janus materials can self-assemble on the interface and have excellent performance in reducing interfacial tension and stabilizing interfacial films. Because of their unique properties, Janus materials have broad application prospects in interfacial activity.

[0004] On the basis of the temperature and pH dual-responsive material, it is further endowed with Janus characteristics and magnetism, making the composite material multifunctional, thus having huge application potential, which is of great significance for enriching the application of composite materials. Summary of the invention

[0005] One object of the present invention is to provide pH and temperature dual-responsive Janus magnetic composite particles. Based on temperature and pH dual-responsive materials, such pH and temperature dual-responsive Janus magnetic composite particles also have Janus properties and magnetism, thereby realizing the multifunctionalization of composite materials. Another object of the present invention is to provide applications of such pH and temperature dual-responsive Janus magnetic composite particles.

[0006] The technical solution adopted by the present invention to solve the technical problem is: the preparation method of the pH and temperature dual-responsive Janus magnetic composite particles is as follows:

[0007] a) Preparation of Fe3O4 magnetic particles by high temperature pyrolysis;

[0008] b) Preparation of core-shell structured Fe3O4@SiO2 nanoparticles:

[0009] 1.5-2.5 g of Fe3O4 magnetic nanoparticles were uniformly dispersed in 500 mL of a mixed solvent, and then 10 mL of ammonia water was added. 4-6 g of tetraethyl orthosilicate TEOS was added dropwise to the above dispersion, and the mixture was stirred and reacted at 60°C for 3 h. After the reaction, the core-shell structured Fe3O4@SiO2 nanoparticles were collected by a magnet, and washed alternately with ethanol and deionized water, and dried. The mixed solvent was prepared by ethanol and water in a ratio of 2:1.

[0010] c) Poly (N-isopropylacrylamide) PNIPAM and poly (acrylic acid) PAA were grafted on one side of the surface of Fe3O4@SiO2 nanoparticles with core-shell structure to prepare pH and temperature dual-responsive Janus magnetic nanocomposite particles:

[0011] At 75°C, 0.5-2.5 g of Fe3O4@SiO2 particles are dispersed in 3-5 g of liquid paraffin containing 0.5%-2% hexadecyltrimethylammonium bromide (CTAB), the mixture is dispersed in 15-25 mL of deionized water, and emulsified for 0.5 h using a high-speed stirrer. After the emulsification, the emulsion is immediately placed in an ice bath to cool the paraffin to solidify the paraffin. The surface of the solidified paraffin emulsion droplets is rinsed with deionized water to remove CTAB and unadsorbed Fe3O4@SiO2 particles, and the solidified paraffin emulsion droplets are vacuum dried.

[0012] 0.1 g of hexadecyltrimethylammonium bromide (CTAB), 0.3-0.6 g of N-isopropylacrylamide (NIPAM), 0.05-0.15 mL of acrylic acid (AA), and 0.02-0.04 g of N,N-methylenebisacrylamide were dissolved in 50 mL of deionized water, and the solidified paraffin emulsion droplets were dispersed into the above solution. 4-6 mL of 5% potassium persulfate (KPS) solution was added and reacted at 60 °C for 24 h to obtain pH and temperature dual-responsive Janus magnetic nanocomposite particles Fe3O4@SiO2 / PNIPAM / PAA.

[0013] The method for preparing Fe3O4 magnetic particles by high temperature pyrolysis in the above scheme is as follows:

[0014] Dissolve 1.5-2.5 g of ferric chloride hexahydrate FeCl3 and 3.5-5.5 g of anhydrous sodium acetate NaAc uniformly in 75-100 mL of ethylene glycol, place the solution in a reactor, react at 200 °C for 10 h, cool to room temperature after the reaction, collect black Fe3O4 magnetic particles with a magnet, and wash with anhydrous ethanol.

[0015] When preparing pH and temperature dual-responsive Janus magnetic nanocomposite particles in the above scheme, the controllable preparation of pH and temperature dual-responsive Janus magnetic composite particles is achieved by adjusting the burial depth of the core-shell structured Fe3O4@SiO2 nanoparticles in paraffin and the degree of polymerization of NIPAM and AA.

[0016] The application of pH and temperature dual-responsive Janus magnetic composite particles in the above scheme in the field of interfacial activity.

[0017] The application of pH and temperature dual-responsive Janus magnetic composite particles in the above scheme in the adsorption field.

[0018] When the pH and temperature dual-responsive Janus magnetic composite particles are used in the above scheme, the interface activity and adsorption performance of the Fe3O4@SiO2 / PNIPAM / PAA composite particles are controlled by changing the external temperature and pH, respectively, and the pH and temperature dual-responsive Janus magnetic composite particles are recycled and reused through the magnetic field. Beneficial Effects

[0019] 1. The present invention grafts poly (N-isopropylacrylamide) (PNIPAM) and poly (acrylic acid) (PAA) on one side of the surface of Fe3O4@SiO2 core-shell particles for the first time to prepare Janus magnetic composite particles with dual responsiveness to temperature and pH. The modification method is simple, low in cost and has good repeatability.

[0020] 2. The interfacial activity and adsorption performance of the pH and temperature dual-responsive Janus magnetic composite particles of the present invention can respond to the external temperature and pH respectively, thereby realizing the multifunctional and intelligent application of the composite particles.

[0021] 3. The present invention has magnetism and can be recycled and reused through an external magnetic field, thus saving use costs and having good application economy.

[0022] 4. The present invention belongs to a new type of pH and temperature dual-responsive Janus magnetic composite particles, which not only have pH and temperature dual-responsive characteristics, but also have surface activity and magnetism, so that it has multiple properties and realizes the multifunctionality of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The figure is a flow chart for the preparation of dual-responsive Janus magnetic composite particles;

[0024] Figure 2 Infrared spectra of Fe3O4, Fe3O4@SiO2, and dual-responsive Janus magnetic composite particles;

[0025] Figure 3This is a fluorescence microscope image of dual-responsive Janus magnetic composite particles;

[0026] Figure 4 The effect of temperature on the interfacial activity of dual-responsive Janus magnetic composite particles;

[0027] Figure 5 The effect of pH on the adsorption performance of dual-responsive Janus magnetic composite particles;

[0028] Figure 6 Hysteresis loops of Fe3O4, Fe3O4@SiO2, and dual-responsive Janus magnetic composite particles. DETAILED DESCRIPTION

[0029] The preparation method of the pH and temperature dual-responsive Janus magnetic composite particles is as follows:

[0030] a) Preparation of Fe3O4 magnetic particles by high temperature pyrolysis

[0031] Dissolve 1.5-2.5 g of ferric chloride hexahydrate (FeCl3) and 3.5-5.5 g of anhydrous sodium acetate (NaAc) uniformly in 75-100 mL of ethylene glycol, place the above solution in a reactor, react at 200°C for 10 h, cool to room temperature after the reaction, collect black Fe3O4 particles with a magnet, and wash with anhydrous ethanol.

[0032] b) Preparation of core-shell structured Fe3O4@SiO2 particles

[0033] 1.5-2.5g of Fe3O4 magnetic nanoparticles were uniformly dispersed in 500mL of mixed solvent (ethanol: water = 2:1), and then 10mL of ammonia water was added. 4-6g of tetraethyl orthosilicate (TEOS) was added dropwise to the above dispersion, and the mixture was stirred at 60°C for 3h. After the reaction, the Fe3O4@SiO2 nanoparticles were collected by magnet, washed alternately with ethanol and deionized water, and dried.

[0034] c) pH and temperature dual-responsive Janus magnetic composite particles were prepared, and the smart polymers poly (N-isopropylacrylamide) (PNIPAM) and poly (acrylic acid) (PAA) were grafted onto one side of the surface of Fe3O4@SiO2 particles with a core-shell structure. Their interfacial activity and adsorption properties can respond to the external temperature and pH, respectively.

[0035] At 75°C, 0.5-2.5 g of Fe3O4@SiO2 particles were dispersed in 3-5 g of liquid paraffin containing 0.5%-2% hexadecyltrimethylammonium bromide (CTAB). The mixture was dispersed in 15-25 mL of deionized water and emulsified for 0.5 h using a high-speed mixer. Immediately after the emulsification, the emulsion was cooled in an ice bath to solidify the paraffin. The surface of the solidified paraffin droplets was rinsed with deionized water to remove CTAB and unadsorbed Fe3O4@SiO2 particles, and the solidified paraffin droplets were vacuum dried.

[0036] 0.1 g of hexadecyltrimethylammonium bromide (CTAB), 0.3-0.6 g of N-isopropylacrylamide (NIPAM), 0.05-0.15 mL of acrylic acid (AA), and 0.02-0.04 g of N,N-methylenebisacrylamide were dissolved in 50 mL of deionized water, and the solidified paraffin emulsion was dispersed in the above solution. 4-6 mL of 5% potassium persulfate (KPS) solution was added and reacted at 60 °C for 24 h to obtain dual-responsive magnetic Janus nanoparticles (Fe3O4@SiO2 / PNIPAM / PAA). The preparation flow chart and infrared spectrum of pH and temperature dual-responsive Janus magnetic composite particles are shown in Figure 2. Figure 1 and Figure 2 .

[0037] In order to prove that the dual-responsive Janus magnetic composite particle surface has an asymmetric structure, the fluorescent agent fluorescein isothiocyanate (FITC) was grafted onto its surface. Since PNIPAM / PAA was grafted on one side, FITC could only be grafted on the other side of Fe3O4@SiO2 / PNIPAM / PAA. Therefore, the fluorescence on one side of the dual-responsive Janus magnetic composite particle surface grafted with FITC is significantly stronger than that on the other side.

[0038] The surface tension of the dual-responsive Janus magnetic composite particles at 30°C and 60°C was compared. The effect of temperature on the surface tension of the dual-responsive Janus magnetic composite particles is shown in Figure 4 .

[0039] The removal rate of methyl blue by dual-responsive Janus magnetic composite particles was compared in the pH range of 3 to 11. The effect of pH on the adsorption performance of dual-responsive Janus magnetic composite particles is shown in Figure 5 .

[0040] The hysteresis loops of Fe3O4, Fe3O4@SiO2 and dual-responsive Janus magnetic composite particles are shown in Figure 6 .

[0041] The present invention grafts poly N-isopropylacrylamide (PNIPAM) and polyacrylic acid (PAA) onto one side of the surface of Fe3O4@SiO2 core-shell particles, and the interfacial activity and adsorption performance can respond to the external temperature and pH respectively, thus realizing the multifunctionality and intelligence of the composite particles. In addition, the pH and temperature dual-responsive Janus magnetic composite particles can be recycled and reused through the external magnetic field, making them economical to use and having broad application prospects.

[0042] Based on the preparation of Fe3O4@SiO2 particles with a core-shell structure, the present invention adds poly-N-isopropylacrylamide (PNIPAm) and polyacrylic acid (PAA) to the side of the shell (silicon dioxide) surface to prepare pH and temperature dual-responsive Janus magnetic composite particles (Fe3O4@SiO2 / PNIPAM / PAA). By changing the external temperature and pH, the interfacial activity and adsorption performance of the Fe3O4@SiO2 / PNIPAM / PAA composite particles can be controlled respectively, and they can be recycled and reused through a magnetic field, which is of great significance to enriching the application of Janus composite materials. In view of the low price of raw materials, the recyclable and reusable products, the mature modification method, the easy operation and high repeatability, it is expected to achieve its industrial application.

Claims

1. A pH and temperature dual-responsive Janus magnetic composite particle, Features: The preparation method of the pH and temperature dual-responsive Janus magnetic composite particles is as follows: a) Preparation of Fe by high temperature pyrolysis 3 O 4 Magnetic particles; b) Preparation of core-shell structured Fe 3 O 4 @SiO 2 Nanoparticles: 1.5-2.5 g of Fe 3 O 4 The magnetic nanoparticles were evenly dispersed in 500 mL of mixed solvent, and 10 mL of ammonia water was added. 4-6 g of tetraethyl orthosilicate TEOS was added dropwise to the dispersion and stirred at 60 °C for 3 h. After the reaction was completed, the core-shell structure of Fe 3 O 4 @SiO 2 The nanoparticles were washed alternately with ethanol and deionized water and dried; the mixed solvent was prepared by mixing ethanol and water in a ratio of 2:1; c) In the core-shell structure of Fe 3 O 4 @SiO 2 One side of the nanoparticle surface was grafted with poly (N-isopropylacrylamide) PNIPAM and poly (acrylic acid) PAA to prepare pH and temperature dual-responsive Janus magnetic nanocomposite particles: At 75℃, 0.5-2.5g of Fe 3 O 4 @SiO 2 The particles were dispersed in 3-5 g of liquid paraffin containing 0.5%-2% hexadecyltrimethylammonium bromide (CTAB). The mixture was dispersed in 15-25 mL of deionized water and emulsified with a high-speed mixer for 0.5 h. After the emulsification, the emulsion was immediately placed in an ice bath to solidify the paraffin. The surface of the solidified paraffin droplets was rinsed with deionized water to remove CTAB and unadsorbed Fe. 3 O 4 @SiO 2 Particles, the solidified paraffin wax emulsion droplets are vacuum dried; 0.1 g of hexadecyltrimethylammonium bromide CTAB, 0.3-0.6 g of N-isopropylacrylamide NIPAM, 0.05-0.15 mL of acrylic acid AA, and 0.02-0.04 g of N,N-methylenebisacrylamide were dissolved in 50 mL of deionized water, and solidified paraffin emulsion droplets were dispersed into the above solution. 4-6 mL of 5% potassium persulfate KPS solution was added and reacted at 60 ° C for 24 h to obtain pH and temperature dual-responsive Janus magnetic nanocomposite particles Fe 3 O 4 @SiO 2 / PNIPAM / PAA.

2. The pH and temperature dual-responsive Janus magnetic composite particles according to claim 1, Features: The high temperature pyrolysis method is used to prepare Fe 3 O 4 The method for magnetic particles is as follows: 1.5-2.5 g of ferric chloride hexahydrate FeCl 3 and 3.5-5.5 g of anhydrous sodium acetate NaAc were uniformly dissolved in 75-100 mL of ethylene glycol. The above solution was placed in a reactor and reacted at 200 °C for 10 h. After the reaction was completed, it was cooled to room temperature and the black Fe 3 O 4 The magnetic particles were washed with anhydrous ethanol.

3. The pH and temperature dual responsive Janus magnetic composite particles according to claim 2, Features: When preparing the pH and temperature dual-responsive Janus magnetic nanocomposite particles, the Fe 3 O 4 @SiO 2 The burial depth of nanoparticles in paraffin and the degree of polymerization of NIPAM and AA enable the controllable preparation of pH and temperature dual-responsive Janus magnetic composite particles.

4. Use of the pH and temperature dual-responsive Janus magnetic composite particles according to claim 1, 2 or 3, Features: The application of the pH and temperature dual-responsive Janus magnetic composite particles in the field of interfacial activity.

5. Application of the pH and temperature dual responsive Janus magnetic composite particles according to claim 1, 2 or 3, Features: The application of the pH and temperature dual-responsive Janus magnetic composite particles in the adsorption field.

6. Use of the pH and temperature dual-responsive Janus magnetic composite particles according to claim 4, Features: After the pH and temperature dual-responsive Janus magnetic composite particles are used, the pH and temperature dual-responsive Janus magnetic composite particles are recovered and reused through a magnetic field.

7. Use of the pH and temperature dual-responsive Janus magnetic composite particles according to claim 5, Features: After the pH and temperature dual-responsive Janus magnetic composite particles are used, the pH and temperature dual-responsive Janus magnetic composite particles are recovered and reused through a magnetic field.