A kind of anti-erosion wear-resistant light-transmitting polymer coating and preparation method thereof
By applying a hard erosion-resistant coating on the polyurethane coating, the problem of erosion in aerospace and underwater glass in harsh environments is solved, and the corrosion resistance and wear resistance are improved, while maintaining light transmission. Significantly reduces wear of glass.
Patent Information
- Application Number
- CN202310411218.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Aerospace and underwater glass are susceptible to erosion in harsh environments, resulting in a decrease in light transmittance and reduced safety. The existing polyurethane coatings have weak erosion resistance and are difficult to effectively protect the glass surface.
Coated a hard erosion-resistant coating on the polyurethane coating, using polymethyl methacrylate or polycarbonate, improves erosion resistance through a multi-layer coating structure and drys at high temperatures for curing.
The corrosion resistance and wear resistance of the polymer coating are significantly improved, while maintaining the light transmittance of the glass, preventing the fragmentation and damage of the hard corrosion resistance layer, and significantly reducing the wear of the glass.
Smart Images

Figure HDA0004183269080000011 
Figure HDA0004183269080000012 
Figure HDA0004183269080000013
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer coatings, and specifically refers to a polymer coating having excellent erosion resistance and wear resistance and maintaining a certain light transmittance, and a preparation method thereof. Background Art
[0002] In aerospace and underwater environments, the service conditions of glass are relatively harsh, and erosion is a major challenge faced by glass in special service conditions. The reason why glass is eroded is that when the glass surface contacts external media (such as water, dust, sand, etc.) or other substances, it will be subjected to chemical or physical reactions to varying degrees, resulting in surface wear and corrosion. These media or substances will cause chemical erosion, electrochemical erosion, mechanical impact, etc. on the glass surface, causing surface wear and damage. Underwater glass is eroded mainly due to the impact and abrasion of various solid particles, seaweed, marine life, sea salt and other substances in the water on the glass surface. These substances may continuously hit the glass surface under the scouring of water flow, which will cause wear and tear while causing the glass transmittance to decrease. Aerospace glass will be hit by high-speed solid particles in the atmosphere during high-altitude flight, resulting in surface erosion. These solid particles mainly include dust, stones, ice crystals, etc., which have great impact energy on the surface of aerospace vehicles. These solid particles will form tiny pits and cracks when hitting the glass surface, and may be directly embedded in the glass. These problems will lead to increased roughness of the glass surface and reduced transparency, which will reduce the safety of the glass and further affect the field of view and safety performance of the spacecraft.
[0003] In order to ensure the safety and stability of glass and maintain its light transmittance, special treatment of the glass surface is usually required. Polymer coatings have good wear resistance and impact resistance, and can protect the substrate surface under mechanical impact and wear. Polyurethane coatings have good weather resistance, chemical corrosion resistance and wear resistance, and polyurethane coatings have excellent elasticity and toughness. However, the erosion resistance of polyurethane coatings is relatively weak, because the hardness and rigidity of polyurethane coatings themselves are relatively low, and they are easily damaged by impact. Summary of the invention
[0004] In order to solve the above problems of the prior art, the present invention provides an erosion-resistant, wear-resistant and light-transmitting polymer coating and a preparation method thereof. The present invention can improve the erosion resistance of the polymer coating and maintain the light transmittance of the coated glass.
[0005] The present invention is achieved through the following technical solutions:
[0006] A corrosion-resistant, wear-resistant and light-transmitting polymer coating comprises a polyurethane coating coated on a glass substrate and a hard corrosion-resistant coating coated on the polyurethane coating; the hard corrosion-resistant coating is a polymethyl methacrylate coating or a polycarbonate coating.
[0007] Preferably, the thickness of the polyurethane coating is 0.5-1 mm, and the thickness of the hard erosion-resistant coating is 0.1-0.5 mm.
[0008] Preferably, the elastic modulus of the polyurethane layer is 20-50 MPa.
[0009] The method for preparing the erosion-resistant, wear-resistant and light-transmitting polymer coating comprises the following steps:
[0010] Step 1: Preparation of polyurethane coating on glass substrate
[0011] Step 2, preparing a hard erosion-resistant coating on the polyurethane coating.
[0012] Preferably, step 2 is specifically:
[0013] 1) dissolving polymethyl methacrylate or polycarbonate in a solvent to obtain a solution;
[0014] 2) applying the dissolving solution onto the polyurethane coating;
[0015] 3) Drying the sample obtained in step 2) to obtain an anti-erosion, wear-resistant and light-transmitting polymer coating.
[0016] Furthermore, in step 1), the solvent is dichloromethane or tetrahydrofuran.
[0017] Furthermore, in step 3), the drying is performed at 60-80° C. for 2-4 hours.
[0018] Preferably, step 1 is specifically:
[0019] 1) taking a polyol and subjecting it to heat treatment under vacuum to remove moisture;
[0020] 2) Mix the polyol and diisocyanate from which water has been removed at 30-50°C, react under nitrogen protection for 1-2 hours, then heat to 80-90°C and continue to react for 4-5 hours to generate a polyurethane prepolymer;
[0021] 3) The polyurethane prepolymer and the chain extender are stirred and mixed, decompressed to remove bubbles, coated on the surface of the glass substrate, and cured at 60-100° C. for 10-12 hours to obtain a polyurethane coating.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention improves the erosion resistance of the polyurethane coating by compounding a hard erosion-resistant coating on the polyurethane coating, that is, by a multi-layer coating structure. The polymethyl methacrylate and polycarbonate in the hard erosion-resistant coating have good mechanical properties and light transmittance, especially polymethyl methacrylate has good impact crack resistance, and can be coated on the surface of polyurethane to prepare a wear-resistant composite coating with better erosion resistance, and will not affect the light transmittance of the glass substrate. The polyurethane coating has toughness, can absorb energy, improve the wear resistance of the coating, and prevent the hard erosion-resistant layer from breaking and damaging.
[0024] Furthermore, the molecular weight distributions of polymethyl methacrylate and polycarbonate are selected to be 30,000-50,000 and 10,000-20,000, respectively, so that they can be fully dissolved in the solvent. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of erosion-resistant and wear-resistant polymer coating.
[0026] Figure 2 Figure 2 shows the wear results of erosion-resistant and wear-resistant polymer coatings: (a) polycarbonate / polyurethane composite layer; (b) pure polyurethane layer.
[0027] Figure 3 This is a test chart of the mass loss of erosion-resistant and wear-resistant polymer coatings with wear.
[0028] Figure 4 This is a graph showing how the transmittance of the erosion-resistant and wear-resistant polymer coating changes with wear. DETAILED DESCRIPTION
[0029] In order to further understand the present invention, the present invention is described below in conjunction with embodiments. These descriptions are only to further explain the features and advantages of the present invention and are not intended to limit the claims of the present invention.
[0030] like Figure 1 The erosion-resistant, wear-resistant and light-transmitting polymer coating of the present invention comprises a polyurethane coating coated on a glass substrate and a hard erosion-resistant coating coated on the polyurethane coating. The hard erosion-resistant coating is a polymethyl methacrylate coating or a polycarbonate coating.
[0031] The thickness of the polyurethane coating is 0.5-1 mm, and the thickness of the hard anti-erosion coating is 0.1-0.5 mm.
[0032] The elastic modulus of the polyurethane layer is 20-50 MPa.
[0033] The method for preparing the erosion-resistant, wear-resistant and light-transmitting polymer coating of the present invention comprises the following steps:
[0034] Step 1: Preparation of polyurethane coating on glass substrate
[0035] 1) taking 20-40 parts (by mass, all parts of the following substances are by mass) of polyol, and heat treating it under vacuum to remove the moisture therein;
[0036] 2) Mix the polyol from which water has been removed at 30-50° C. with 10-20 parts of diisocyanate, react under nitrogen protection for 1-2 hours, then heat to 80-90° C. and continue to react for 4-5 hours to generate a polyurethane prepolymer;
[0037] 3) The polyurethane prepolymer is stirred and mixed with 3-5 parts of a chain extender, and the air bubbles are removed by decompression. The obtained coating is applied on the surface of a glass substrate, and cured at 60-100° C. for 10-12 hours to obtain a polyurethane coating.
[0038] Step 2: Preparation of erosion-resistant polymethyl methacrylate coating or polycarbonate coating
[0039] 1) dissolving polymethyl methacrylate or polycarbonate in dichloromethane or tetrahydrofuran to obtain a solution;
[0040] 2) Draw the dissolving liquid with a micro syringe, adjust the speed of the spin coater to 3000 r / min-4000 r / min, and use the spin coater to spin-coat polymethyl methacrylate or polycarbonate onto the polyurethane coating.
[0041] 3) Place the obtained film-containing sample in a vacuum oven and dry at 60-80°C for 2-4 hours.
[0042] The diisocyanate is one or two of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate; the polyol is one or two of polytetramethylene ether PTMG1000 and polytetramethylene ether PTMG2000; the chain extender is one or two of 3,3'-dichloro-4,4'-diaminodiphenylmethane, 3,5-dimethylthiotoluenediamine, 1,4-butanediol and ethylene glycol.
[0043] Example 1, Preparation of polyurethane coating
[0044] Take 20 parts of polyether polyol PTMG1000, put them in a container, heat to 100°C and evacuate for 3 hours to remove moisture, then cool the polyether polyol PTMG1000 to 50°C, mix evenly with 10 parts of toluene diisocyanate, react for 1 hour, then heat to 75°C and continue to react for 5 hours to generate a polyurethane prepolymer; cool the polyurethane prepolymer to 60°C and put it in a container, add 3 parts of 3,5-dimethylthiotoluenediamine, vacuum degas for 5 minutes, and then evenly coat it on the surface of a white glass substrate with a coating thickness of about 1 mm, and cure it at 80°C for 12 hours to obtain a polyurethane coating with an elastic modulus of 37 MPa.
[0045] Example 2, Preparation of polyurethane coating
[0046] Take 30 parts of polyoxypropylene glycol 1000, put it in a container, heat it to 100°C and evacuate it for 3 hours to remove moisture, then cool the polyoxypropylene glycol 1000 to 50°C, mix it evenly with 15 parts of toluene diisocyanate, react for 2 hours, then heat it to 75°C and continue to react for 4 hours to generate a polyurethane prepolymer; cool the polyurethane prepolymer to 60°C and put it in a container, add 4 parts of 3,5-dimethylthiotoluenediamine, vacuum degas for 5 minutes, and then evenly coat it on the surface of a glass substrate with a coating thickness of about 0.5 mm, and cure it at 80°C for 12 hours to obtain a polyurethane coating with an elastic modulus of 23 MPa.
[0047] Example 3, Preparation of polyurethane coating
[0048] Take 40 parts of polyether polyol PTMG1000, place them in a container, heat to 100°C and evacuate for 3 hours to remove moisture, then cool the polyether polyol PTMG1000 to 50°C, mix evenly with 20 parts of isophorone diisocyanate, react for 2 hours, then heat to 75°C and continue to react for 5 hours to generate a polyurethane prepolymer; cool the polyurethane prepolymer to 60°C and place it in a container, add 4 parts of 1,4-butanediol, vacuum degas for 5 minutes, and then evenly coat it on the surface of the glass substrate with a coating thickness of about 1 mm, cure at 80°C for 12 hours, and its elastic modulus is 42 MPa.
[0049] Example 4, Preparation of Hard Polymethyl Methacrylate Coating
[0050] Dissolve polymethyl methacrylate in tetrahydrofuran; extract the solution with a micro syringe, adjust the speed of the spin coater to 3000r / min, and use the spin coater to apply the solution to the polyurethane coating of Example 1, gradually add the solution dropwise, and test and control the thickness to be between 0.5mm. Put the obtained film-containing sample into a vacuum oven and dry it at 60°C for 2 hours to obtain a polymethyl methacrylate / polyurethane composite layer.
[0051] Example 5, Preparation of Hard Polymethyl Methacrylate Coating
[0052] Dissolve polymethyl methacrylate in tetrahydrofuran; extract the dissolving solution with a microsyringe, adjust the speed of the spin coater to 3500r / min, and use the spin coater to spin coat the dissolving solution onto the polyurethane coating of Example 1, gradually add the dissolving solution dropwise, and test and control the thickness to be between 0.3mm. Put the obtained film-containing sample into a vacuum oven and dry it at 80°C for 3 hours to obtain a polymethyl methacrylate / polyurethane composite layer.
[0053] Example 6, Preparation of hard polycarbonate coating
[0054] Dissolve polycarbonate in dichloromethane; extract the dissolving solution with a microsyringe, adjust the speed of the spin coater to 3200r / min, and use the spin coater to spin coat the dissolving solution onto the polyurethane coating of Example 1, gradually add the dissolving solution dropwise, and test and control the thickness to be between 0.5mm. Put the obtained film-containing sample into a vacuum oven and dry it at 70°C for 2 hours to obtain a polycarbonate / polyurethane composite layer.
[0055] Example 7, Preparation of hard polycarbonate coating
[0056] Dissolve polycarbonate in dichloromethane; extract the dissolving solution with a microsyringe, adjust the speed of the spin coater to 40000r / min, and use the spin coater to spin coat the dissolving solution onto the polyurethane coating of Example 1, gradually add the dissolving solution dropwise, and test and control the thickness to be between 0.3mm. Put the obtained film-containing sample into a vacuum oven and dry it at 70°C for 4 hours to obtain a polycarbonate / polyurethane composite layer.
[0057] Example 8, Example 6 Wear Test of Polycarbonate / Polyurethane Composite Layer
[0058] The polycarbonate / polyurethane composite layer of Example 6 was subjected to a wear test using a wear test machine, with the test machine rotating at 200 r / min. The mass loss of the sample was measured every 5 minutes. The results after ten minutes of wear are as follows: Figure 2 As shown, it can be seen that the wear of the polycarbonate / polyurethane composite layer (a) is significantly lighter than that of the pure polyurethane layer (b). Figure 3 is the mass loss result, from Figure 3 The results show that the mass loss of the polycarbonate / polyurethane composite layer is significantly smaller than that of the pure polyurethane layer, indicating that the wear resistance of the polycarbonate / polyurethane composite layer has been greatly improved.
[0059] Example 9, Example 6 Test on the change of light transmittance of polycarbonate / polyurethane composite layer with wear
[0060] The polycarbonate / polyurethane composite layer obtained in Example 6 was subjected to a wear test using a wear test machine, with the test machine rotating at 100 r / min. The transmittance was measured every 5 minutes, and the transmittance of the sample to 550nm visible light was tested using a transmittance meter. The results are as follows: Figure 4 As shown. Figure 4 The results show that the decrease in light transmittance of the polycarbonate / polyurethane composite layer with friction is significantly lower than that of the pure polyurethane coating.
Claims
1. An anti-erosion, wear-resistant and light-transmitting polymer coating, characterized in that: It comprises a polyurethane coating coated on a glass substrate, and a hard anti-erosion coating coated on the polyurethane coating; the hard anti-erosion coating is a polymethyl methacrylate coating or a polycarbonate coating; the elastic modulus of the polyurethane coating is 20-50MPa; the thickness of the polyurethane coating is 0.5-1mm, and the thickness of the hard anti-erosion coating is 0.1-0.5mm; The method for preparing the erosion-resistant, wear-resistant and light-transmitting polymer coating comprises the following steps: Step 1, preparing a polyurethane coating on a glass substrate; Step 2, preparing a hard anti-erosion coating on the polyurethane coating; Step 1 is as follows: 1.1) Take the polyol and heat treat it under vacuum to remove moisture; 1.2) Mix the polyol and diisocyanate from which water has been removed at 30-50°C, react under nitrogen protection for 1-2 hours, then heat to 80-90°C and continue to react for 4-5 hours to generate a polyurethane prepolymer; wherein the diisocyanate is one or two of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate; and the polyol is one or two of polytetramethylene ether PTMG1000 and polytetramethylene ether PTMG2000; 1.3) Mixing the polyurethane prepolymer and the chain extender, degassing under reduced pressure, coating the prepolymer on the surface of the glass substrate, and curing the prepolymer at 60-100° C. for 10-12 hours to obtain a polyurethane coating; wherein the chain extender is one or two of 3,3'-dichloro-4,4'-diaminodiphenylmethane, 3,5-dimethylthiotoluenediamine, 1,4-butanediol and ethylene glycol; Step 2 is as follows: 2.1) dissolving polymethyl methacrylate or polycarbonate in a solvent to obtain a solution; 2.2) applying the dissolving solution onto the polyurethane coating; 2.3) Drying the sample obtained in step 2.2) to obtain an anti-erosion, wear-resistant and light-transmitting polymer coating.
2. The method for preparing the erosion-resistant, wear-resistant and light-transmitting polymer coating according to claim 1, characterized in that: The following steps are involved: Step 1, preparing a polyurethane coating on a glass substrate; Step 2, preparing a hard erosion-resistant coating on the polyurethane coating; Step 1 is as follows: 1.1) Take the polyol and heat treat it under vacuum to remove moisture; 1.2) Mix the polyol and diisocyanate from which water has been removed at 30-50°C, react under nitrogen for 1-2 hours, then heat to 80-90°C and continue to react for 4-5 hours to generate a polyurethane prepolymer; 1.3) The polyurethane prepolymer and the chain extender are stirred and mixed, decompressed to remove bubbles, coated on the surface of the glass substrate, and cured at 60-100°C for 10-12h to obtain a polyurethane coating; Step 2 is as follows: 2.1) dissolving polymethyl methacrylate or polycarbonate in a solvent to obtain a solution; 2.2) applying the dissolving solution onto the polyurethane coating; 2.3) Drying the sample obtained in step 2.2) to obtain an anti-erosion, wear-resistant and light-transmitting polymer coating.
3. The method for preparing the erosion-resistant, wear-resistant and light-transmitting polymer coating according to claim 2, characterized in that: In step 2.1), the solvent is dichloromethane or tetrahydrofuran.
4. The method for preparing the erosion-resistant, wear-resistant and light-transmitting polymer coating according to claim 2, characterized in that: In step 2.3), the drying is specifically performed at 60-80° C. for 2-4 hours.
Citation Information
Patent Citations
Method for preparing self-cleaning polycarbonate film
CN101812184A
Weatherable & abrasion resistant coating systems for polymeric substrates
CN103492502A
Polyurethane coating agent, and preparation method and application thereof
CN111040602A
Antiglare hardcoat multilayer film
CN111741848A
Vehicular polymeric glazing
US20180236753A1