A method for preparing Y2O3 particle dispersion-strengthened copper-based composite material using metal yttrium salt
By using Y salt and Cu powder for mechanical alloying and calcination reduction, combined with discharge plasma sintering, the problem of dispersed phase agglomeration is solved, the performance of copper-based composite materials is improved, and the uniform distribution and purity of Y2O3 particles are achieved, which enhances the material conductive and mechanical properties.
Patent Information
- Application Number
- CN202310416392.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-13
AI Technical Summary
The agglomeration of the dispersed phase during the mechanical alloying process leads to a reduction in the performance of copper-based composite materials. The existing method is prone to doping with impurities during the ball milling process and the Y source powder particle size is large, which affects the material properties.
Y salt is used as the oxide source, ball milled with Cu powder through mechanical alloying process, in-situ reaction is used to prevent the agglomeration of the dispersed phase, and Y2O3 particle dispersion-strengthened copper-based composite materials are prepared through calcination reduction and discharge plasma sintering.
The uniform distribution of the dispersed phase is achieved, the electrical and thermal conductivity and mechanical properties of the copper-based material are improved, and the generation and agglomeration of impurities are avoided. The resulting Y2O3 particles are purer and smaller, and the densification of the material is enhanced.
Smart Images

Figure CN116479277B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of high-strength and high-conductivity copper-based composite materials, and in particular to a method for preparing Y2O3 particle dispersion-reinforced copper-based composite materials by using metal yttrium salts. Background Art
[0002] Oxide dispersion strengthened copper-based composites are composites with excellent mechanical properties and electrical and thermal conductivity obtained by dispersing a small amount of nano-oxide particles in the copper matrix to hinder the movement of dislocations within the grain boundaries. In the preparation of oxide dispersion strengthened copper-based composites, the mechanical alloying process has obvious advantages, because this method can combine materials that cannot be prepared by traditional smelting methods, and use appropriate powder processing conditions to obtain a well-dispersed second phase in the matrix. At the same time, mechanical alloying can make the powder have greater surface activity and promote element diffusion. Therefore, Y powder and CuO or Cu2O can be used as raw materials and oxidants to promote the non-equilibrium diffusion of oxygen elements during the mechanical alloying process, and dispersed strengthening phase Y2O3 particles are formed in situ. However, this method is easy to be doped with impurities during the ball milling process, which affects the performance of the material. In addition, the particle size of the Y source powder is large, all at the micron level. Without the addition of process control agents, the particle size of the particles after ball milling is large, at the millimeter level, which is not conducive to sintering densification.
[0003] In addition, there are literature reports that use Y salt as a raw material to obtain relatively pure Cu-Y2O3 composite powder by solid-liquid doping. Since Y salt is at the molecular level after being dissolved in deionized water, the composite powder particles obtained after drying are fine, and the average grain size of the composite material obtained is at the micron level. However, when the content of the dispersed phase Y2O3 in the copper matrix reaches a certain level, it will agglomerate, and many tiny flocculent particles will appear on the surface of the copper matrix, which indicates that the bond between Y2O3 and the copper matrix is not strong.
[0004] In view of the above phenomenon, the present invention adopts Y salt as Y source and uses mechanical alloying process to prepare high-strength and high-conductivity copper-based composite materials. Since Y salt does not react with Cu powder, no impurities are generated during the ball milling process, and Y salt is in a crystalline state, has high brittleness and low hardness, and is easily broken during the ball milling process, thereby achieving a uniform dispersion effect. When no process control agent is added, the ball milled particles still maintain the micron level, making the dispersed phase particles smaller and more evenly distributed, and finally obtaining a pure Y2O3 particle dispersion-strengthened copper-based composite material. Summary of the invention
[0005] The present invention proposes a method for preparing Y2O3 particle dispersion-reinforced copper-based composite materials using metal yttrium salts, which mainly solves the technical defect that the performance of the copper-based composite materials is reduced due to the agglomeration of the dispersed phase during the mechanical alloying process. Y salt is used as the source of oxide, and in-situ reaction and mechanical alloying process are used to prevent the agglomeration of the dispersed phase in the copper matrix, so that the dispersed phase is evenly distributed, thereby improving the electrical and thermal conductivity and mechanical properties of the copper-based material.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing Y2O3 particle dispersion-strengthened copper-based composite material using metal yttrium salt, wherein Y salt and Cu powder are directly subjected to mechanical alloying to obtain Cu-Y salt precursor powder, and then Y2O3 particle dispersion-strengthened copper-based composite powder is obtained by calcination reduction in a reducing atmosphere, and finally Y2O3 particle dispersion-strengthened copper-based composite material is obtained by spark plasma sintering.
[0008] Further improvement is that the preparation method specifically comprises the following steps:
[0009] (I) Mechanical alloying
[0010] Y(NO3)3·6H2O or Y2(CO3)3 is used as Y salt, Y salt powder and Cu powder are placed in a ball mill according to a weight ratio of 2.36-8:92-97.64, the ball mill is assembled under an argon atmosphere, and the ball mill is placed in a planetary ball mill for ball milling, and after the ball milling is completed, the ball mill is taken out and ground to obtain a precursor powder Cu-Y(NO3)3 or Cu-Y2(CO3)3;
[0011] (ii) Calcination reduction
[0012] The precursor powder is placed in a tube furnace, and Ar-H2 mixed gas with a H2 content of 10% is introduced for 30 minutes, and the air in the tube is exhausted. Then, the temperature is increased to 600°C at a heating rate of 10°C / min, and the temperature is kept for 2 hours and then cooled with the furnace to obtain Y2O3 particle dispersion strengthened copper-based composite powder;
[0013] (III) Spark plasma sintering
[0014] (1) Powder loading: The composite powder obtained in step (ii) is wrapped with carbon paper and loaded into a graphite mold. After pre-pressing, the mold is placed in a discharge plasma furnace and the furnace chamber is evacuated to a vacuum at room temperature;
[0015] (2) Exhaust: Set the pre-compression pressure to 10 MPa, raise the temperature to 600 °C and keep it for 5 min to exhaust the gas in the powder material;
[0016] (3) Sintering: The temperature is continuously raised to 900°C and kept at this temperature for 5 minutes. During the temperature raising process, the pressure is uniformly increased to a final pressure of 50 MPa. After the heat preservation is completed, the pressure is cooled to room temperature with the furnace to obtain a Y2O3 particle dispersion-strengthened copper-based composite material, in which the mass ratio of Y2O3 is 1.5-2.5%.
[0017] As a preferred technical solution of the present invention, in the preparation method, the ball-to-material ratio in step (i) is 7:3-4:1, the ball milling speed is 550-650 rpm, and the ball milling time is 32-48 hours. In step (iii), the heating rate is 100°C / min.
[0018] Compared with the prior art, the beneficial effects of the present invention are mainly manifested in:
[0019] First, since Y salt does not react with Cu powder, no impurities are generated during the ball milling process. During calcination and reduction, oxide gases such as C and N can be released at high temperatures, and finally a pure Y2O3 particle dispersion-strengthened copper-based composite material is obtained. In addition, during the ball milling process, Y salt can be used as a process control agent to inhibit the growth of copper grains. After ball milling, the particles remain at the micron level, making the dispersed phase particles smaller, more evenly distributed, and the sintering densification degree easier, thereby improving the electrical and thermal conductivity and mechanical properties of the copper matrix.
[0020] Second, compared with the method of using Y powder or Y2O3 powder to prepare Cu-Y2O3 composite powder, since the Y salt is in a crystalline state, it is brittle and has low hardness, and has better dispersibility when ball-milled with Cu powder. In addition, the Y salt has a smaller particle size than Y powder or Y2O3, and the dispersed phase particles obtained after ball milling are finer and more evenly dispersed, resulting in the final prepared Cu-Y2O3 composite material having better mechanical properties and conductive properties.
[0021] Third, compared with the method of using Y salt as a raw material to obtain a Cu-Y2O3 composite material by solid-liquid doping, the bonding between the copper matrix and Y2O3 is weak, and agglomeration occurs and a second phase similar to a mesh is formed at the copper grain boundary, which destroys the continuity of the copper matrix and is not conducive to the plasticity and conductivity of the sample. The mechanical alloying used in the present invention can be ball milled for a long time to weaken this phenomenon, so that the two are closely bonded, the strengthening phase is finely and evenly dispersed in the copper matrix, the mechanical properties of the copper composite material are improved, and the influence on the conductivity is minimized. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the XRD spectrum of the composite material Cu-Y2O3 prepared in Example 1.
[0023] Figure 2 This is a powder picture of the composite material Cu-Y2O3 obtained in Example 1 after ball milling.
[0024] Figure 3 This is a powder picture of the composite material Cu-Y2O3 prepared in Example 1 after ball milling.
[0025] Figure 4 This is the result obtained by energy spectrum analysis of the composite material Cu-Y2O3 prepared in Example 2.
[0026] Figure 5 This is the result obtained by energy spectrum analysis of the composite material Cu-Y2O3 prepared in Example 1.
[0027] Figure 6 This is the tensile curve of the composite material Cu-Y2O3 prepared in Example 2.
[0028] Figure 7 This is the tensile curve of the composite material Cu-Y2O3 prepared in Comparative Example 2. DETAILED DESCRIPTION
[0029] The preferred embodiments and comparative embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0030] Example 1
[0031] The Cu-Y2O3 composite material in this embodiment is made by mechanical alloying, calcination reduction and spark plasma sintering, wherein the purity of pure Cu powder is 99.5%, and the mass fraction of added yttrium carbonate (Y2(CO3)3) is 2.36%. The preparation method is as follows:
[0032] (1) Mechanical alloying: 48.82 g of pure Cu powder and 1.18 g of yttrium carbonate (Y2(CO3)3) were placed in a ball mill, and the ball mill was assembled under an argon atmosphere. After assembly, the ball mill was placed in a planetary ball mill for ball milling. The ball milling speed (rotation speed) was 550 rpm, the ball milling time was 32 h, and the ball-to-material ratio was 7:3. After the ball milling was completed, 50 g of Cu-Y2(CO3)3 precursor powder was obtained.
[0033] (2) Calcination reduction: The above-mentioned precursor powder is placed in a tubular furnace, and an Ar-H2 mixed gas with a H2 content of 10% is introduced for 30 minutes. The air in the tube is discharged, and the temperature is increased to 600°C at a rate of 10°C / min. After keeping the temperature for 2 hours, the mixture is cooled in the furnace to obtain a Cu-Y2O3 composite powder.
[0034] (3) Spark plasma sintering: 15 g of Cu-Y2O3 composite powder was wrapped with carbon paper and loaded into a graphite mold. After pre-pressing, the mold was placed in a spark plasma sintering furnace. The furnace chamber was evacuated to vacuum at room temperature. The pre-pressing pressure was set to 10 MPa, the heating rate was 100 °C / min, the temperature was raised to 600 °C and kept for 5 min, and then the temperature was continued to be raised to 900 °C and kept for 5 min. During the temperature increase process, the pressure was continuously increased to a final pressure of 50 MPa. After the insulation was completed, the temperature was cooled to room temperature with the furnace to obtain a Cu-Y2O3 composite material with a Y2O3 mass fraction of 1.5%.
[0035] Example 2
[0036] The Cu-Y2O3 composite material in this embodiment is made by mechanical alloying, calcination reduction and spark plasma sintering, wherein the purity of pure Cu powder is 99.5%, and the mass fraction of added yttrium nitrate (Y(NO3)3·6H2O) is 4.91%. The preparation method is as follows:
[0037] (1) Mechanical alloying: 47.545 g of pure Cu powder and 2.455 g of yttrium nitrate (Y(NO3)3·6H2O) were placed in a ball mill, and the ball mill was assembled under an argon atmosphere. After the assembly, the ball mill was placed in a planetary ball mill for ball milling. The ball milling speed (rotation speed) was 550 rpm, the ball milling time was 32 h, and the ball-to-material ratio was 7:3. After the ball milling was completed, 50 g of Cu-Y(NO3)3 precursor powder was obtained.
[0038] (2) Calcination reduction: The above-mentioned precursor powder is placed in a tubular furnace, and an Ar-H2 mixed gas with a H2 content of 10% is introduced for 30 minutes. The air in the tube is discharged, and the temperature is increased to 600°C at a rate of 10°C / min. After keeping the temperature for 2 hours, the mixture is cooled in the furnace to obtain a Cu-Y2O3 composite powder.
[0039] (3) Spark plasma sintering: 15 g of Cu-Y2O3 composite powder was wrapped with carbon paper and loaded into a graphite mold. After pre-pressing, the mold was placed in a spark plasma sintering furnace. The furnace chamber was evacuated to vacuum at room temperature. The pre-pressing pressure was set to 10 MPa, the heating rate was 100 °C / min, the temperature was raised to 600 °C and kept for 5 min, and then the temperature was continued to be raised to 900 °C and kept for 5 min. During the temperature increase process, the pressure was continuously increased to a final pressure of 50 MPa. After the insulation was completed, the temperature was cooled to room temperature with the furnace to obtain a Cu-Y2O3 composite material with a Y2O3 mass fraction of 1.5%.
[0040] Example 3
[0041] The Cu-Y2O3 composite material in this embodiment is made by mechanical alloying, calcination reduction and spark plasma sintering, wherein the purity of pure Cu powder is 99.5%, and the mass fraction of added yttrium nitrate (Y(NO3)3·6H2O) is 8%. The preparation method is as follows:
[0042] (1) Mechanical alloying: 46 g of pure Cu powder and 4 g of yttrium nitrate (Y(NO3)3·6H2O) were placed in a ball mill, and the ball mill was assembled under an argon atmosphere. After the assembly, the ball mill was placed in a planetary ball mill for ball milling. The ball milling speed (rotation speed) was 650 rpm, the ball milling time was 48 h, and the ball-to-material ratio was 4:1. After the ball milling was completed, 50 g of Cu-Y(NO3)3 precursor powder was obtained.
[0043] (2) Calcination reduction: The above-mentioned precursor powder is placed in a tubular furnace, and an Ar-H2 mixed gas with a H2 content of 10% is introduced for 30 minutes. The air in the tube is discharged, and the temperature is increased to 600°C at a rate of 10°C / min. After keeping the temperature for 2 hours, the mixture is cooled in the furnace to obtain a Cu-Y2O3 composite powder.
[0044] (3) Spark plasma sintering: 15 g of Cu-Y2O3 composite powder was wrapped with carbon paper and loaded into a graphite mold. After pre-pressing, the mold was placed in a spark plasma sintering furnace. The furnace chamber was evacuated to vacuum at room temperature. The pre-pressing pressure was set to 10 MPa, the heating rate was 100 °C / min, the temperature was raised to 600 °C and kept for 5 min, and then the temperature was continued to be raised to 900 °C and kept for 5 min. During the temperature increase process, the pressure was continuously increased to a final pressure of 50 MPa. After the insulation was completed, the furnace was cooled to room temperature to obtain a Cu-Y2O3 composite material with a Y2O3 mass fraction of 2.5%.
[0045] Comparative Example 1
[0046] The Cu-Y2O3 composite material in this embodiment is made by mechanical alloying, calcination reduction and spark plasma sintering, wherein CuO is used as the copper matrix and oxidant, and the mass fraction of pure Y powder added is 0.95%. The preparation method is as follows:
[0047] (1) Mechanical alloying: First, 49.525 g of CuO powder and 0.475 g of pure Y powder were placed in a ball mill, and the ball mill was assembled under an argon atmosphere. After the assembly, the ball mill was placed in a planetary ball mill for ball milling. The ball milling speed (rotation speed) was 550 rpm, the ball milling time was 32 h, and the ball-to-material ratio was 7:3. After the ball milling was completed, 50 g of CuO-Y2O3 precursor powder was obtained.
[0048] (2) Calcination and reduction: The precursor powder is placed in a high-temperature tubular furnace and calcined and reduced in a hydrogen atmosphere. During the reduction process, the temperature is raised from room temperature to 600°C at a rate of 10°C / min. After being kept at this temperature for 2 hours, the powder is cooled in the furnace to obtain a Cu-Y2O3 composite powder.
[0049] (3) Spark plasma sintering: 15 g of Cu-Y2O3 composite powder was wrapped with carbon paper and loaded into a graphite mold. After pre-pressing, the mold was placed in a spark plasma sintering furnace. The furnace chamber was evacuated to vacuum at room temperature. The pre-pressing pressure was set to 10 MPa, the heating rate was 100 °C / min, the temperature was raised to 600 °C and kept for 5 min, and then the temperature was continued to be raised to 900 °C and kept for 5 min. During the temperature increase process, the pressure was continuously increased to a final pressure of 50 MPa. After the insulation was completed, the temperature was cooled to room temperature with the furnace to obtain a Cu-Y2O3 composite material with a Y2O3 mass fraction of 1.5%.
[0050] Comparative Example 2
[0051] The Cu-Y2O3 composite material in this embodiment is made by solid-liquid doping, calcination reduction and spark plasma sintering, wherein the purity of pure Cu powder is 99.5%, and the mass fraction of added yttrium nitrate (Y(NO3)3·6H2O) is 4.91%. The preparation method is as follows:
[0052] (1) Solid-liquid doping: First, dissolve 2.455g Y(NO3)3·6H2O with an appropriate amount of plasma water, and then add 47.545g pure Cu powder. Place the beaker in a DF-1 magnetic stirrer and heat to 120°C for drying (add a rotor to the beaker to mix the powder evenly). After the water in the beaker evaporates, dry the precursor powder in a DHG-9070 oven at 140°C for 12 hours to obtain 50g Cu-Y(NO3)3 precursor powder.
[0053] (2) Calcination and reduction: The precursor powder is placed in a high-temperature tube furnace and calcined and reduced in a hydrogen atmosphere. During the reduction process, the temperature is raised from room temperature to 200°C at a rate of 10°C / min, kept at this temperature for 30 minutes, and then raised to 600°C at a rate of 10°C / min and kept at this temperature for 2 hours. After the insulation is completed, the temperature is lowered to 500°C at a rate of 5°C / min, and then cooled in the furnace to obtain a Cu-Y2O3 composite powder.
[0054] (3) Spark plasma sintering: 15 g of Cu-Y2O3 composite powder was wrapped with carbon paper and loaded into a graphite mold. After pre-pressing, the mold was placed in a spark plasma sintering furnace. The furnace chamber was evacuated to vacuum at room temperature. The pre-pressing pressure was set to 10 MPa, the heating rate was 100 °C / min, the temperature was raised to 600 °C and kept for 5 min, and then the temperature was continued to be raised to 900 °C and kept for 5 min. During the temperature increase process, the pressure was continuously increased to a final pressure of 50 MPa. After the insulation was completed, the temperature was cooled to room temperature with the furnace to obtain a Cu-Y2O3 composite material with a Y2O3 mass fraction of 1.5%.
[0055] Table 1 Performance test of Cu-Y2O3 composite materials prepared in Examples 1 to 3 and Comparative Examples 1 to 2.
[0056]
[0057] It can be seen from Table 1 that compared with the Cu-Y2O3 composite materials prepared by the method used in Comparative Examples 1 and 2, the composite materials prepared by mechanical alloying of Y salt and Cu powder in Examples 1, 2 and 3 have more excellent comprehensive properties.
[0058] Depend on Figure 1 , Figure 2 and Figure 3 It can be seen that after mechanical alloying with Y salt and Cu powder, the powder particles are finer, and no impurities remain after calcination and reduction, obtaining a pure Y2O3 particle dispersion-strengthened copper-based composite material.
[0059] Depend on Figure 4 and Figure 5 It can be seen that the Cu-Y2O3 composite material obtained by mechanical alloying, calcination reduction and spark plasma sintering of CuO and Y powder traditionally has dispersed phase Y2O3 agglomerated in the copper matrix, resulting in poor mechanical properties and electrical and thermal conductivity. The composite material Cu-Y2O3 obtained by mechanical alloying, calcination reduction and spark plasma sintering of Y salt and Cu powder has a more dispersed distribution of dispersed phase Y2O3 in the copper matrix, thus obtaining better comprehensive performance.
[0060] Depend on Figure 6 and Figure 7 It can be seen that compared with the precursor powder prepared by solid-liquid doping of Y salt and Cu powder, the composite material Cu-Y2O3 obtained by mechanical alloying of Y salt and Cu powder has better mechanical properties.
[0061] The above embodiments only illustrate specific implementations of the present disclosure, but the implementations of the present disclosure are not limited by the above contents. Any changes, modifications, substitutions, combinations, and simplifications made without substantially departing from the main idea and principle of the inventive concept of the present disclosure shall be equivalent replacement methods and shall be included in the scope of protection determined by the claims.
Claims
1. A method for preparing Y2O3 particle dispersion strengthened copper-based composite material using metal yttrium salt, characterized in that: The specific steps include: (1) Mechanical alloying: 48.82 g of pure Cu powder and 1.18 g of yttrium carbonate (Y2(CO3)3) were placed in a ball mill, and the ball mill was assembled under an argon atmosphere. After the assembly, the ball mill was placed in a planetary ball mill for ball milling; the ball milling speed was 550 rpm, the ball milling time was 32 h, and the ball-to-material ratio was 7:
3. After the milling was completed, 50 g of Cu-Y2(CO3)3 precursor powder was obtained; (2) Calcination reduction: The above-mentioned precursor powder was placed in a tube furnace, and Ar-H2 mixed gas with a H2 content of 10% was introduced for 30 minutes. The air in the tube was exhausted, and the temperature was raised to 600°C at a rate of 10°C / min. After keeping the temperature for 2 hours, the mixture was cooled in the furnace to obtain Cu-Y2O3 composite powder; (3) Spark plasma sintering: 15 g of Cu-Y2O3 composite powder was wrapped with carbon paper and loaded into a graphite mold. After pre-pressing, the mold was placed in a spark plasma sintering furnace. The furnace chamber was evacuated to vacuum at room temperature. The pre-pressing pressure was set to 10 MPa, the heating rate was 100 °C / min, the temperature was raised to 600 °C and kept for 5 min, and then the temperature was continued to be raised to 900 °C and kept for 5 min. During the temperature increase process, the pressure was continuously increased to a final pressure of 50 MPa. After the insulation was completed, the Cu-Y2O3 composite material was cooled to room temperature with the furnace to obtain a Y2O3 mass fraction of 1.5%, a conductivity of 89.6% IACS, a Vickers hardness of 97.4 HV, and a tensile strength of 325 MPa.
Citation Information
Patent Citations
Preparation method of high-strength and high-conductivity copper alloy
CN113337747A