A self-transforming modified flaky zinc oxide and its preparation method and application

By grafting phosphorylcholine and trimethoxysiloxane groups on the surface of flaky zinc oxide, the adaptive dispersion and biocompatibility of modified zinc oxide in water and oil phases were achieved, solving the current problem. There is a problem that modified zinc oxide is only suitable for a single phase, which improves the application characteristics of cosmetics.

CN116492231BActive Publication Date: 2024-10-29GUANGDONG UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310352613.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-29
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

Existing modified zinc oxide is only suitable for single oil phase or single water phase cosmetics, cannot adapt to both water and oil phases in cosmetics, and has insufficient biocompatibility.

Method used

A copolymer containing siloxane groups was synthesized through free radical reaction, and phosphorylcholine hydrophilic groups and trimethoxysiloxane hydrophobic groups were grafted on the surface of flaky zinc oxide, so that they can self-generate under the action of thermodynamics. transformation to adapt to the microstructure distribution of different phases, resulting in good dispersion in both water and oil phases.

Benefits of technology

It achieves adaptive dispersion of modified flake zinc oxide in water and oil phases, enhances biocompatibility, simplifies the preparation process, reduces raw material costs, and has good cosmetic application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116492231B_ABST
    Figure CN116492231B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of cosmetic raw material preparation, and discloses a self-transforming modified flaky zinc oxide, a preparation method thereof and its application. The modified flaky zinc oxide is a mixture of 2-methacryloyloxyethyl phosphorylcholine, 3-(isobutyleneoxy)propyltrimethoxysilane, azobisisobutyronitrile and ethanol A, and stirred at 70-80°C for reaction; after cooling, precipitation and filtration are performed to obtain a phospholipid-silane copolymer; a mixed solution of flaky zinc oxide, phospholipid-silane copolymer, ethanol B, water and ammonia is ultrasonically treated, an organic tin catalyst is added, stirred at room temperature, filtered, washed and dried to obtain. The surface of the modified flaky zinc oxide is simultaneously grafted with a hydrophobic group and a hydrophilic group, and when in different phases, self-transformation occurs under the action of thermodynamics, so that the modified flaky zinc oxide has good dispersibility in both the aqueous phase and the oil phase. At the same time, it has good biocompatibility, and its process is simple, green and environmentally friendly, and can be applied in cosmetics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cosmetic raw material preparation, and in particular relates to a self-transforming modified flaky zinc oxide and a preparation method and application thereof. Background Art

[0002] Sunscreen products applied to the human skin will cause makeup to collapse after mixing with the oil and sweat secreted by the human body. Therefore, sunscreen needs to adapt to the changes in human skin, otherwise it will appear dull and greasy. Zinc oxide is an important and widely used physical sunscreen in cosmetics. In addition, zinc oxide can also adsorb oil on the skin surface. Therefore, in order to prolong the makeup effect, people usually add zinc oxide to cosmetic powder or add hydrophobic zinc oxide to the oil phase to inhibit oil secretion and makeup collapse.

[0003] Phosphocholine (PC) is the main lipid component of the outer layer of human cell membranes, with excellent properties such as high hydrophilicity, non-toxicity and stability at physiological pH. 2-Methacryloyloxyethyl phosphorylcholine (MPC) is an organic monomer containing phosphorylcholine, which has similar properties to the outer layer of human cell membranes. MPC polymer can significantly increase the biocompatibility of materials by modifying the surface of materials to mimic the outer layer of cell membranes. 3-(Isomethacryloyloxy)propyltrimethoxysilane (KH-570) is a silane coupling agent, which is often used for surface treatment of inorganic fillers to improve adhesion to inorganic materials and increase water resistance.

[0004] Therefore, in recent years, in order to obtain modified zinc oxide with excellent properties, some patents describe the technology of modified zinc oxide and its application in cosmetics. Chinese patent CN110613625A "Spherical zinc oxide powder coated with natural substances, its manufacturing method and cosmetic composition containing it" provides a spherical zinc oxide powder coated with natural substances, a TEOS coating layer on the surface of the spherical zinc oxide powder, and a lecithin natural substance coating layer uniformly coated on the surface of the TEOS coating layer. The prepared zinc oxide powder has a good ultraviolet isolation effect. Chinese patent CN112390282A "A hydrophilic zinc oxide quantum dot and its preparation method and use" uses zinc acetate and 3-aminopropyltriethoxysilane (APTES) as raw materials to modify zinc oxide under alkaline conditions. The obtained modified zinc oxide has good water solubility and antibacterial effect, which is suitable for the field of daily cosmetics. Chinese patent CN108524309B "A waterproof sunscreen cosmetic and preparation method" uses a titanate coupling agent to modify zinc oxide, and then loads isooctyl methoxycinnamate and 3-(4-methylbenzylidene) camphor on the modified zinc oxide to prepare a composite sunscreen, which not only has good waterproof properties and can be used in underwater environments, but also can achieve ultraviolet absorption effects. However, the modified zinc oxide prepared in the above patent is only suitable for single oil phase or single water phase cosmetics, and its application in cosmetics is greatly limited. Therefore, it is of great significance to develop a modified zinc oxide that can be applied to both water phase and oil phase cosmetic components and has good biocompatibility. Summary of the invention

[0005] In order to solve the above-mentioned deficiencies and shortcomings of the prior art, the primary purpose of the present invention is to provide a self-transforming modified flaky zinc oxide. The surface of the modified flaky zinc oxide is simultaneously connected with a hydrophobic group and a hydrophilic group. When in different phases, the microstructure distribution of the hydrophilic group and the hydrophobic group on the surface will undergo self-transformation under the action of thermodynamics, so that the modified flaky zinc oxide can adapt to different phases and has good dispersibility in both the water phase and the oil phase.

[0006] Another object of the present invention is to provide a method for preparing the self-transforming modified flaky zinc oxide obtained by the above method. The method synthesizes a copolymer containing siloxane groups by free radical reaction, and the hydroxyl groups of the siloxane groups in the copolymer undergo a dehydration condensation reaction with the hydroxyl groups on the surface of the flaky zinc oxide under the action of a catalyst, thereby simultaneously grafting hydrophilic groups and hydrophobic groups on the surface of the flaky zinc oxide.

[0007] Another object of the present invention is to provide an application of the self-transforming modified flaky zinc oxide.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] The invention discloses a self-transforming modified flaky zinc oxide. The modified flaky zinc oxide comprises the following steps: 2-methacryloyloxyethyl phosphorylcholine, 3-(isobutyleneoxy)propyltrimethoxysilane, azobisisobutyronitrile and ethanol A are mixed, dry nitrogen is used to blow the obtained solution, and the mixture is stirred at 70-80 DEG C for reaction; the reaction mixture is cooled to room temperature, then put into deionized water for precipitation and filtration, and washed with deionized water for multiple times to obtain a phospholipid-silane copolymer; a mixed solution of flaky zinc oxide, phospholipid-silane copolymer, ethanol B, water and ammonia water is ultrasonically treated, an organic tin catalyst is added, and the mixture is stirred at room temperature; the obtained product is filtered, washed with anhydrous ethanol and deionized water for multiple times, and dried at 40-50 DEG C overnight to obtain the obtained product.

[0010] Preferably, the molar ratio of the 2-methacryloyloxyethyl phosphorylcholine and 3-(isomethacryloyloxy)propyltrimethoxysilane is (1-8):(3-8); the volume ratio of ethanol A to the total mass ratio of 2-methacryloyloxyethyl phosphorylcholine and 3-(isomethacryloyloxy)propyltrimethoxysilane is (1-4) mL:1 g; the mass ratio of the 2-methacryloyloxyethyl phosphorylcholine and azobisisobutyronitrile is (100-500):1.

[0011] Preferably, the mass ratio of the flaky zinc oxide and the phospholipid-silane copolymer is (5-10):1; the volume ratio of the total mass of the mixed solution of flaky zinc oxide, phospholipid-silane copolymer, water and ammonia water to ethanol B is 3g:(100-200)mL; the volume ratio of the mixed solution of water and ammonia water to ethanol B is 1:(10-20), and the volume ratio of water and ammonia water is (3-10):1; the concentration of ammonia is 25-50wt%; and the organic tin catalyst is dibutyltin dilaurate, stannous octoate or dibutyltin diacetate.

[0012] Preferably, the surface of the modified flaky zinc oxide is grafted with both phosphorylcholine hydrophilic groups and trimethoxysiloxane hydrophobic groups.

[0013] The method for preparing the self-transforming modified flaky zinc oxide comprises the following steps:

[0014] S1. 2-methacryloyloxyethyl phosphorylcholine, 3-(isobutyleneoxy)propyltrimethoxysilane, azobisisobutyronitrile and ethanol are mixed, and the resulting solution is blown with dry nitrogen gas, and stirred at 70-80° C. for reaction; the reaction mixture is cooled to room temperature, and then placed in deionized water for precipitation and filtration, and washed with deionized water for multiple times to obtain a phospholipid-silane copolymer;

[0015] S2. Ultrasonic treatment of a mixed solution of flaky zinc oxide, phospholipid-silane copolymer, ethanol, water and ammonia water, adding an organic tin catalyst, and stirring at room temperature; filtering the resulting product and washing it with anhydrous ethanol and deionized water for multiple times, respectively, and drying it at 40-50°C overnight to obtain a self-transforming modified flaky zinc oxide.

[0016] Preferably, the reaction time in step S1 is 2 to 3 hours; the ultrasonic time in step S2 is 30 to 60 minutes, the reaction time is 24 to 48 hours, and the stirring rate is 200 to 500 rpm / min.

[0017] Application of the modified flaky zinc oxide in the field of cosmetics.

[0018] The method of the present invention synthesizes an amphiphilic copolymer, and then grafts the amphiphilic copolymer onto the surface of flaky zinc oxide. The surface of the prepared modified flaky zinc oxide is simultaneously connected with a hydrophobic group and a hydrophilic group, so when the modified flaky zinc oxide is in different phases, the microstructure distribution of the hydrophilic group and the hydrophobic group on its surface will undergo self-transformation under the action of thermodynamics, so that the modified flaky zinc oxide adapts to different phases and has good dispersibility in both the aqueous phase and the oil phase. The microstructure distribution of the hydrophilic group and the hydrophobic group on the surface of the modified flaky zinc oxide will undergo self-transformation in the aqueous phase and the oil phase. In the aqueous phase, the thermodynamic action minimizes the interaction between the hydrophilic group on the surface of the modified flaky zinc oxide and water, and the hydrophilic group is exposed to contact with water; in the oil phase, the thermodynamic action minimizes the interaction between the hydrophobic group on the surface of the modified flaky zinc oxide and oil, and the hydrophobic group is exposed to contact with oil, and the prepared modified flaky zinc oxide has good dispersibility in both the aqueous phase and the oil phase. The application of the amphiphilic phospholipid-silane copolymer, modified flaky zinc oxide and self-transformed microstructure synthesized by the present invention can give the modified flaky zinc oxide of the present invention the application characteristics required in the field of cosmetics.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The modified flaky zinc oxide self-transforms microstructure of the present invention. The composite microstructure is conducive to self-adaptation to different phases, has good dispersibility in different phases, and is suitable for different cosmetic formulations. The microstructures of the phosphorylcholine hydrophilic group and the trimethoxysiloxane hydrophobic group in different phases will self-transform, so that the modified flaky zinc oxide can adapt to different phases and has good dispersibility in both the water phase and the oil phase.

[0021] 2. The present invention synthesizes a copolymer containing siloxane groups through a free radical reaction, and the hydroxyl groups after hydrolysis of the siloxane groups in the copolymer react with the hydroxyl groups on the surface of the flaky zinc oxide under the action of a catalyst to undergo a dehydration condensation reaction, thereby simultaneously grafting the phosphorylcholine hydrophilic group and the trimethoxysiloxane hydrophobic group on the surface of the flaky zinc oxide. The preparation method is simple and practical, and the raw materials used are low in cost, abundant in source and easily available, and easy to promote.

[0022] 3. The modified flaky zinc oxide prepared by the present invention has good biocompatibility, and its process is simple, green and environmentally friendly, and has good potential for cosmetic applications. Since phosphorylcholine has similar properties to the phospholipid bilayer of human skin, the biocompatibility is enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Schematic diagram of the synthetic chemical formula of the phospholipid-silane copolymer of the present invention;

[0024] Figure 2 The present invention is a flow chart for preparing the modified flaky zinc oxide;

[0025] Figure 3 This is the infrared spectrum of the phospholipid-silane copolymer and the modified flaky zinc oxide in Example 1;

[0026] Figure 4 This is the NMR spectrum of the phospholipid-silane copolymer of Example 2;

[0027] Figure 5 This is an optical photograph of the dispersion of modified flaky zinc oxide in Example 3;

[0028] Figure 6 Schematic diagram of the dispersibility mechanism of the modified flaky zinc oxide of the present invention. DETAILED DESCRIPTION

[0029] The content of the present invention is further described below in conjunction with specific examples, but it should not be construed as limiting the present invention. If not specifically indicated, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0030] Example 1

[0031] Figure 1 This is a schematic diagram of the synthetic chemical formula of phospholipid-silane copolymer; Figure 2 A method for preparing a self-transforming modified flaky zinc oxide, such as Figure 1 and 2 As shown, the following steps are included:

[0032] 1. Weigh 2-methacryloyloxyethyl phosphorylcholine (0.4mmol, 0.118g) and 3-(isobutyleneoxy)propyltrimethoxysilane (2mmol, 0.745g) and 2mL of anhydrous ethanol into a thumb bottle, and slowly blow the resulting solution with dry nitrogen for 10min. Then transfer the thumb bottle to an oil bath at 80°C, and then weigh 0.001g of azobisisobutyronitrile (AIBN) and dissolve it in 1mL of anhydrous ethanol, and slowly drop it into the thumb bottle, stir and react for 3h, and after the reaction is completed, cool the reaction mixture to room temperature, put the reaction mixture into deionized water for precipitation, filter the product, and wash it with deionized water for several times to obtain a white viscous phospholipid-silane copolymer.

[0033] 2. Weigh 3g of flaky zinc oxide and 100mL of anhydrous ethanol and add them to a round-bottom flask, weigh 0.3g of phospholipid-silane copolymer and fully dissolve it, and finally add a mixed solution of 6mL of water and 2mL of ammonia water (25wt%). Ultrasonicate the above mixture for 30min to make it fully dispersed, add the catalyst di-n-butyltin dilaurate, place the round-bottom flask on a magnetic stirrer, and stir the above mixed system at room temperature for 48h at a stirring speed of 500rpm. Filter and wash the obtained product with anhydrous ethanol and deionized water for multiple times, respectively, place the loaded product filter paper in a vacuum drying oven, dry it overnight at 40℃, and grind the dried product into powder with a mortar to obtain self-transforming modified flaky zinc oxide.

[0034] Figure 3 is the infrared spectrum of the phospholipid-silane copolymer, 3-(isobutyleneoxy)propyltrimethoxysilane, flaky zinc oxide and modified flaky zinc oxide in Example 1. Figure 3 It can be seen that the phospholipid silane polymer and modified flake zinc oxide 2900cm -1 Multiple bands of tertiary amine N(CH3) appeared at 1387cm -1 The absorption peak of P=O appears at 1228cm -1 The absorption peak of (P)-OC appears at , indicating that the phospholipid silane polymer and modified flake zinc oxide were successfully prepared.

[0035] Example 2

[0036] 1. Weigh 2-methacryloyloxyethyl phosphorylcholine (2mmol, 0.944g) and 3-(isobutyleneoxy)propyltrimethoxysilane (0.4mmol, 0.093g) and 4mL of anhydrous ethanol into a thumb bottle, and slowly blow the resulting solution with dry nitrogen for 10min. Then transfer the thumb bottle to an oil bath at 80°C, and then weigh 0.001g of azobisisobutyronitrile (AIBN) and dissolve it in 1mL of anhydrous ethanol, slowly add it dropwise to the thumb bottle, and stir the reaction for 3h. After the reaction, cool the reaction mixture to room temperature, put the reaction mixture into deionized water for precipitation, filter the product, and wash it with deionized water several times to obtain a phospholipid-silane copolymer of a white viscous substance.

[0037] 2. Weigh 3g of flaky zinc oxide and 100mL of anhydrous ethanol and add them to a round-bottom flask, weigh 0.3g of phospholipid-silane copolymer and fully dissolve it, and finally add a mixed solution of 6mL of water and 2mL of ammonia water (25wt%). Ultrasonicate the above mixture for 30min to make it fully dispersed, add the catalyst di-n-butyltin dilaurate, place the round-bottom flask on a magnetic stirrer, and stir the above mixed system at 500rpm at room temperature for 48h. Filter and wash the obtained product with anhydrous ethanol and deionized water for multiple times, place the loaded product filter paper in a vacuum drying oven, dry it overnight at 40℃, and grind the dried product into powder with a mortar to obtain self-transforming modified flaky zinc oxide.

[0038] Figure 4 is the NMR spectrum of the phospholipid-silane copolymer in Example 2. Figure 4 It can be seen that δ H =0.62-0.75ppm peak corresponds to -CH2Si-,δ H =3.14-3.45ppm peak corresponds to -N(CH3), δ H =4.20-4.50ppm peak corresponds to -POCH2, indicating that the phospholipid silane polymer was successfully prepared.

[0039] Example 3

[0040] 1. Weigh 2-methacryloyloxyethyl phosphorylcholine (1mmol, 0.295g) and 3-(isobutyleneoxy)propyltrimethoxysilane (1mmol, 0.373g) and 2mL of anhydrous ethanol into a thumb bottle, and slowly blow the resulting solution with dry nitrogen for 10min. Then transfer the thumb bottle to an oil bath at 80°C, and then weigh 0.001g of azobisisobutyronitrile (AIBN) and dissolve it in 1mL of anhydrous ethanol, slowly add it dropwise to the thumb bottle, and stir the reaction for 3h. After the reaction, cool the reaction mixture to room temperature, put the reaction mixture into deionized water for precipitation, filter the product, and wash it with deionized water several times to obtain a white viscous phospholipid-silane copolymer.

[0041] 2. Weigh 3g of flaky zinc oxide and 100mL of anhydrous ethanol and add them to a round-bottom flask, weigh 0.3g of phospholipid-silane copolymer and fully dissolve it, and finally add a mixed solution of 6mL of water and 2mL of ammonia water (25wt%). Ultrasonicate the above mixture for 30min to make it fully dispersed, add di-n-butyltin dilaurate as a catalyst, place the round-bottom flask on a magnetic stirrer, and stir the above mixed system at 500rpm at room temperature for 48h. Filter and wash the obtained product with anhydrous ethanol and deionized water for multiple times, respectively, place the loaded product filter paper in a vacuum drying oven, dry it overnight at 40℃, and grind the dried product into powder with a mortar to obtain self-transforming modified flaky zinc oxide.

[0042] Figure 5 The optical photos of the dispersion stability test of flaky zinc oxide (①) and modified flaky zinc oxide (②) in deionized water (a) and white oil (b) in Example 3 are shown in Figure 3. Take 4 thumb bottles of the same specifications, weigh the same mass of flaky zinc oxide and modified flaky zinc oxide, and measure the same volume of deionized water and white oil, respectively, ultrasonicate for 30 minutes, and then let it stand. Figure 5 It can be seen that, with deionized water as the solvent, the flaky zinc oxide suspension precipitated after standing for 1 hour, and the modified flaky zinc oxide suspension still maintained good dispersibility after standing for 12 hours; with white oil as the solvent, the flaky zinc oxide aggregated in the white oil after standing for 2 hours, and the modified flaky zinc oxide suspension still maintained good dispersibility after standing for 2 hours, indicating that the modified flaky zinc oxide can undergo self-transformation to adapt to the aqueous phase and the oil phase, and can maintain good dispersion stability in both the aqueous phase and the oil phase. This is because the microstructures of the hydrophilic groups of phosphorylcholine and the hydrophobic groups of trimethoxysiloxane in different phases will undergo self-transformation, allowing the modified flaky zinc oxide to adapt to different phases and have good dispersibility in both the aqueous phase and the oil phase, such as Figure 6 shown.

[0043] Comparative Example 1

[0044] Weigh 3g of flaky zinc oxide and 100mL of anhydrous ethanol into a round-bottom flask, and add a mixed solution of 6mL of water and 2mL of ammonia water (25wt%). Ultrasonicate the mixture for 30min to fully disperse it, place the round-bottom flask on a magnetic stirrer, and stir the mixed system at 500rpm at room temperature for 48h. Filter and wash the obtained product with anhydrous ethanol and deionized water for multiple times, place the loaded product filter paper in a vacuum drying oven, dry it overnight at 40℃, and grind the dried product into powder with a mortar to obtain flaky zinc oxide, the particle size of which is the same as that of the modified flaky zinc oxide.

[0045] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A self-transforming modified flaky zinc oxide, characterized in that: The modified flaky zinc oxide is prepared by mixing 2-methacryloyloxyethyl phosphorylcholine, 3-(isobutyleneoxy)propyltrimethoxysilane, azobisisobutyronitrile and ethanol A, blowing the obtained solution with dry nitrogen, and stirring the reaction at 70-80°C; cooling the reaction mixture to room temperature, then putting it into deionized water for precipitation and filtration, and washing it with deionized water to obtain a phospholipid-silane copolymer; ultrasonically treating a mixed solution of flaky zinc oxide, phospholipid-silane copolymer, ethanol B, water and ammonia water, adding an organic tin catalyst, stirring at room temperature, filtering the obtained product, washing it with anhydrous ethanol and deionized water respectively, and drying it at 40-50°C overnight to obtain the obtained product.

2. The self-transforming modified flaky zinc oxide according to claim 1, characterized in that: The molar ratio of the 2-methacryloyloxyethyl phosphorylcholine to 3-(isomethacryloyloxy)propyltrimethoxysilane is (1-8):(3-8); the volume ratio of ethanol A to the total mass ratio of 2-methacryloyloxyethyl phosphorylcholine and 3-(isomethacryloyloxy)propyltrimethoxysilane is (1-4) mL:1 g; the mass ratio of the 2-methacryloyloxyethyl phosphorylcholine to azobisisobutyronitrile is (100-500):

1.

3. The self-transforming modified flaky zinc oxide according to claim 1, characterized in that: The mass ratio of the flaky zinc oxide and the phospholipid-silane copolymer is (5-10):1; the volume ratio of the total mass of the mixed solution of the flaky zinc oxide, the phospholipid-silane copolymer, water and ammonia water to ethanol B is 4g:(100-200)mL; the volume ratio of the mixed solution of water and ammonia water to ethanol B is 1:(10-20), and the volume ratio of water to ammonia water is (3-10):1; the concentration of the ammonia water is 25-50wt%; and the organic tin catalyst is dibutyltin dilaurate, stannous octoate or dibutyltin diacetate.

4. The method for preparing the self-transforming modified flaky zinc oxide according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. 2-methacryloyloxyethyl phosphorylcholine, 3-(isobutyleneoxy)propyltrimethoxysilane, azobisisobutyronitrile and ethanol are mixed, and the resulting solution is blown with dry nitrogen gas, and stirred at 70-80° C. for reaction; the reaction mixture is cooled to room temperature, and then placed in deionized water for precipitation and filtration, and washed with deionized water to obtain a phospholipid-silane copolymer; S2. A mixed solution of flaky zinc oxide, phospholipid-silane copolymer, ethanol, water and ammonia water is ultrasonically treated, an organic tin catalyst is added, and the mixture is stirred at room temperature; the obtained product is filtered and washed with anhydrous ethanol and deionized water respectively, and dried at 40-50° C. overnight to obtain a self-transforming modified flaky zinc oxide.

5. The method for preparing the self-transforming modified flaky zinc oxide according to claim 4, characterized in that: The reaction time in step S1 is 2-3 hours; the ultrasonic time in step S2 is 30-60 minutes, the stirring time is 24-48 hours, and the stirring rate is 200-500 rpm / min.

6. Use of the modified flaky zinc oxide according to any one of claims 1 to 3 in the field of cosmetics.

Citation Information

Patent Citations

  • A waterproof sunscreen cosmetic and its preparation method

    CN108524309B

  • Spherical zink oxide powder coated with natural materials, manufacturing method thereof, and cosmetic comprising the same

    CN110613625A

  • Hydrophilic zinc oxide quantum dot and preparation method and application thereof

    CN112390282A

  • Organic and inorganic composite powder used to block ultraviolet light, and cosmetic composition including same

    CN103505376A

  • Phosphorylcholine group and silicone group-containing copolymer, powder coated with said copolymer and production method therefor, and use of said copolymer and said powder in cosmetics

    CN111868121A