A kind of desulfurization and denitrification activated carbon with adjustable CaS content and its preparation method and application
By adjusting the CaS content and adding a binder, the problem of high preparation cost and unstable performance of activated carbon in the non-electricity industry was solved. Highly active and high-performance desulfurization and denitrification activated carbon was prepared, which promoted the integrated dry activated carbon flue gas purification. Industrial application of technology.
Patent Information
- Application Number
- CN202310317187.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Among the existing technologies, low-temperature flue gas treatment technology in the non-electricity industry has problems such as high dependence on specific coal types, high cost of activated carbon preparation, and unstable performance. Moreover, the mature technology of thermal power plants cannot be promoted in the non-electricity industry, resulting in low cost. High-performance activated carbon is difficult to prepare.
By detecting the content of pyrite and calcite in raw coal, adjusting the mass ratio of CaS, adding a binder and performing hot pressing molding, carbonization and activation treatments, a desulfurization and denitrification activated carbon with adjustable CaS content was prepared, optimizing the molding performance of the activated carbon. and preparation process.
It has reduced the dependence on unique coal types, reduced the cost of activated carbon preparation, obtained highly active and high-performance desulfurization and denitrification activated carbon, and promoted the industrial application of activated carbon dry integrated flue gas purification technology in non-electricity industries.
Smart Images

Figure CN116495730B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of desulfurization and denitrification activated carbon, and specifically relates to a desulfurization and denitrification activated carbon with adjustable CaS content, and a preparation method and application thereof. Background Art
[0002] Industrial production will emit a large amount of sulfur oxides (SO x ) and nitrogen oxides (NO x ), which will not only cause environmental problems such as ozone layer depletion and acid rain, but also pose a serious threat to the human respiratory system. In response to this, the country has introduced strict ultra-low emission standards: NO x <50mg·Nm -3 ;SO x <35mg·Nm -3 . At present, thermal power plants have basically completed ultra-low emission transformation and the technology is mature. However, due to the low flue gas temperature (<250℃) of non-electric industries represented by coking, sintering, and kilns, the mature flue gas treatment technology of thermal power plants cannot be promoted in non-electric industries. In recent years, the activated carbon dry integrated desulfurization and denitrification technology has received widespread attention due to its advantages such as high low-temperature activity, no water consumption, easy regeneration, and basically no secondary pollution. At present, coal-based desulfurization and denitrification activated carbon has been widely used in low-temperature flue gas treatment in non-electric industries.
[0003] Scientific research and production practice show that the preparation process conditions of activated carbon and the composition of raw coal determine its desulfurization and denitrification activity and application potential. In the actual production process, due to the extensive management mode of activated carbon plants in my country, coal selection and blending are currently mainly based on experience, resulting in dependence on inherent coal types, which is not conducive to the preparation of low-cost and high-performance activated carbon. Coal is mainly composed of carbon organic matter and inorganic minerals. Although the content of inorganic minerals is relatively small, its influence on the activity of activated carbon is huge. Patent literature (publication number CN115557496A) discloses a method for preparing high desulfurization and denitrification activated carbon by blending coal using the mineral catalytic index of coal. Pyrite and calcite are the most important inorganic minerals for activated carbon in coal, and their contents can reach 3% and 8% of the coal sample respectively. Patent literature (publication number CN113808679A) discloses that the presence of pyrite and calcite alone in coal will enhance the low-temperature desulfurization and denitrification activity of activated carbon. However, inorganic substances in coal usually exist together in coal. Previous studies have shown that calcium sulfide (CaS) will be generated when pyrite and calcite exist simultaneously in coal.
[0004] In view of the fact that the above-mentioned coal preparation and blending are highly dependent on specific coal types, and the activated carbon prepared has high cost and unstable performance, it is urgent to find reasonable, scientific and accurate indicators / parameters to guide the preparation of high-performance activated carbon. Summary of the invention
[0005] In order to solve the technical problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a desulfurization and denitrification activated carbon with adjustable CaS content and a preparation method and application thereof.
[0006] To achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing desulfurization and denitrification activated carbon with adjustable CaS content, the preparation method comprising the following steps:
[0008] Step 1: Select different types of raw coal and detect the content of pyrite and calcite in each raw coal;
[0009] Step 2: Based on the mass ratio of pyrite to calcite, the content of CaS is adjusted and the raw coals are compounded;
[0010] Step 3: Add a binder to the mixed coal obtained by compounding, and obtain the desulfurization and denitrification activated carbon through hot pressing, carbonization and activation treatment.
[0011] Preferably, the mass ratio of pyrite to calcite is 0.8 to 1.2 to ensure maximum generation of CaS.
[0012] Preferably, the binder includes but is not limited to coal tar and asphalt. Since the main body of coal is a non-polar hydrocarbon, a binder needs to be added during the preparation process to improve the molding performance of the coal sample. Coal tar and asphalt can increase the viscosity and surface tension of the coal sample exponentially, greatly enhance the interaction between particles, and greatly enhance the plasticity of the mixed sample.
[0013] Preferably, the mass percentage of the binder is 20% to 30% based on the mass of the mixed coal, so as to ensure the molding performance of the activated carbon and the economy of preparing the activated carbon.
[0014] Preferably, the conditions for the hot pressing molding are: a pressure of 25 to 35 MPa, a temperature of 50 to 85° C., and a time of 4 to 10 min, so that the prepared activated carbon has better anti-wear strength.
[0015] Preferably, the carbonization conditions are: carbonization temperature is 450-750° C., and carbonization time is 40-100 min, so as to obtain a precursor with initially developed structural pores.
[0016] Preferably, the activation conditions are as follows: the activation medium is water vapor, the activation temperature is 800-950°C, the flow rate of water vapor is 0.03-0.08 mL / min·g, and the water vapor introduction time is 20-90 min, so as to obtain activated carbon with a developed pore structure and a higher yield.
[0017] In a second aspect, the present invention provides a desulfurization and denitrification activated carbon, which is prepared according to the aforementioned preparation method.
[0018] In a third aspect, the present invention provides the application of the aforementioned desulfurization and denitrification activated carbon in desulfurization and denitrification, and the application includes application in flue gas treatment in non-electricity industries.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The present invention prepares desulfurization and denitrification activated carbon by regulating the CaS content, provides a scientific and reasonable basis for coal selection and coal blending, reduces the dependence on special coal types and the preparation cost of activated carbon, and the obtained desulfurization and denitrification activated carbon has high activity;
[0021] (2) The present invention can provide scientific, reasonable and accurate guidance for the preparation of low-cost, high-performance activated carbon using high-inorganic sulfur / calcium / iron coal, and further promote the industrial application of activated carbon dry integrated flue gas purification technology in non-electricity industries, with extremely high market prospects and practical utilization value. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The trend diagram of sulfur capacity change of activated carbon with different CaS content at 120℃ for single desulfurization;
[0023] Figure 2 This is a graph showing the change trend of denitrification rate of activated carbon with different CaS contents at 120°C;
[0024] Figure 3 This is a trend chart of the changes in the desulfurization, denitrification and denitrification rates of activated carbon with different CaS contents at 120°C. DETAILED DESCRIPTION
[0025] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0026] Example 1
[0027] A method for preparing desulfurization and denitrification activated carbon with adjustable CaS content, specifically comprising the following steps:
[0028] (1) Zhundong high-speed railway general coal and Inner Mongolia high-calcium Shangwan coal were selected as raw coal to prepare activated carbon. The contents of pyrite and calcite in each raw coal were obtained by X-ray fluorescence spectrometer (XRF), X-ray diffractometer (XRD) and eva siroquant quantitative software, as shown in Table 1;
[0029] Table 1
[0030]
[0031] (2) The Zhundong high-speed railway general coal and the Inner Mongolia high-calcium Shangwan coal were compounded in mass ratios of 1:0, 1:1, 1:2, 1:3 and 0:1, respectively, and mixed evenly. The mass ratio of pyrite to calcite in the compounded mixed coal is shown in Table 2;
[0032] (3) Add 23 wt.% (based on the mass of the mixed coal) of a binder (a mixture of asphalt and coal tar) to the mixed coal obtained by the above compounding and mix them thoroughly. After hot pressing (constant temperature and pressure at 75°C and 25 MPa for 5 minutes), carbonize at 600°C for 1 hour to obtain a precursor. The precursor is crushed into 20-40 meshes, and 10 g of the precursor is activated in a water vapor (water intake: 0.06 mL / min·g, 900°C) atmosphere for 80 minutes to obtain the desulfurization and denitrification activated carbon.
[0033] (4) The CaS content in the desulfurization and denitrification activated carbon was measured using an X-ray diffractometer (XRD) and eva siroquant quantitative software (see Table 2), and the desulfurization and denitrification activated carbon was named AC-XCaS, where X is the CaS content.
[0034] Table 2
[0035]
[0036] Example 2
[0037] The activated carbon prepared in Example 1 was tested for desulfurization activity in the following simulated flue gas. The simulated flue gas composition was: 1500ppm SO2, 10vol.% water vapor, 5vol.% O2 and nitrogen as the balance gas. The total gas flow rate was 200mL / min and the space velocity was 4000h -1 , the temperature is 120°C. The sulfur capacity (S, mg / g) is calculated by the following formula:
[0038] S=FC in t q / M
[0039]
[0040] Where, F is the total flow rate of simulated flue gas (mL / min); M is the mass of activated carbon (g); t q is the stoichiometric time of adsorption. In this embodiment, t q 60min; C in , C out are the inlet and outlet concentrations of SO2, respectively.
[0041] The desulfurization activity test results are shown in Table 3 and Figure 1 .
[0042] Table 3
[0043]
[0044]
[0045] Example 3
[0046] The activated carbon prepared in Example 1 was tested for denitrification activity in the following simulated flue gas, the simulated flue gas composition was: 500ppm NO, 500ppm NH3, 5Vol.% O2 and nitrogen as the balance gas, the total gas flow rate was 200mL / min, the space velocity was 4000h -1 , the temperature is 120℃. The denitrification rate (Re, %) is calculated by the following formula:
[0047]
[0048] Among them, C in , C out are the inlet and outlet concentrations of NO, respectively.
[0049] The results of the denitrification activity test are shown in Table 4 and Figure 2 .
[0050] Table 4
[0051]
[0052] Example 4
[0053] The activated carbon prepared in Example 1 was tested for denitrification activity in the following simulated flue gas. The simulated flue gas composition was: 1500ppm SO2, 5Vol.% O2, 500ppm NO, 500ppm NH3, 5Vol.% O2 and nitrogen as the balance gas. The total gas flow rate was 200mL / min and the air velocity was 4000h -1 , the temperature is 120℃. The denitrification activity test results are shown in Table 5 and Figure 3 .
[0054] Table 5
[0055]
[0056]
[0057] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0058] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing desulfurization and denitrification activated carbon with adjustable CaS content, characterized in that: The following steps are involved: Step 1: Select different types of raw coal and detect the content of pyrite and calcite in each raw coal; Step 2: Based on the mass ratio of pyrite to calcite, the content of CaS is adjusted and the raw coals are compounded; Step 3: adding a binder to the mixed coal obtained by compounding, and subjecting the mixture to hot pressing, carbonization and activation treatment to obtain the desulfurization and denitrification activated carbon; The mass ratio of the pyrite to the calcite is 0.8-1.
2.
2. The method for preparing a desulfurization and denitrification activated carbon with adjustable CaS content according to claim 1, characterized in that: The binder includes coal tar and asphalt.
3. The method for preparing a desulfurization and denitrification activated carbon with adjustable CaS content according to claim 1, characterized in that: The mass percentage of the binder is 20% to 30% based on the mass of the mixed coal.
4. The method for preparing a desulfurization and denitrification activated carbon with adjustable CaS content according to claim 1, characterized in that: The conditions for the hot pressing molding are: pressure of 25-35 MPa, temperature of 50-85° C., and time of 4-10 min.
5. The method for preparing a desulfurization and denitrification activated carbon with adjustable CaS content according to claim 1, characterized in that: The carbonization conditions are as follows: the carbonization temperature is 450-750° C., and the carbonization time is 40-100 min.
6. The method for preparing a desulfurization and denitrification activated carbon with adjustable CaS content according to claim 1, characterized in that: The activation conditions are as follows: the activation medium is water vapor, the activation temperature is 800-950° C., the flow rate of water vapor is 0.03-0.08 mL / (min•g), and the introduction time of water vapor is 20-90 min.
7. A desulfurization and denitrification activated carbon prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the desulfurization and denitrification activated carbon as claimed in claim 7 in desulfurization and denitrification.
9. The use of desulfurization and denitrification activated carbon according to claim 8, characterized in that: Applied to flue gas treatment in non-electrical industries.
Citation Information
Cited By
Blast furnace injection coal blending method using sintering desulfurization and denitrification activated carbon and flux