A high-toughness fiber water-stable phosphogypsum regeneration base material and preparation method thereof
Through the use of high-tough fiber water-stable phosphogypsum regeneration base material, combined with low-temperature plasma treatment and modifiers, the problems of phosphogypsum recycling and poor stability of road base are solved, and efficient recycling of road structures and environmental protection are achieved.
Patent Information
- Application Number
- CN202310391627.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-13
AI Technical Summary
The prior art is difficult to effectively recycle and utilize industrial solid waste phosphogypsum and road base materials, resulting in groundwater pollution and poor road structure stability.
The high-tough fiber water-stable phosphate gypsum is used to regenerate the base material. The combination of basalt fibers and modifiers treated with low temperature plasma can improve the performance of phosphate gypsum, increase the toughness and stability of the cement base, and reduce impurities through stabilizers. Influence.
It improves the toughness and crack resistance of road base materials, extends the service life of the road, reduces the mining of natural resources and pollutant emissions, and achieves economic and environmental benefits.
Smart Images

Figure BDA0004175987590000021 
Figure BDA0004175987590000071 
Figure BDA0004175987590000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of recycled road base materials, and in particular to a high-toughness fiber water-stable phosphogypsum recycled base material and a preparation method thereof. Background Art
[0002] Industrial wet phosphorus production produces a large amount of industrial solid waste phosphogypsum, the main component of which is calcium sulfate dihydrate, and contains some impurities such as soluble phosphoric acid and fluoride. Therefore, phosphogypsum is prone to seepage during storage and disposal, causing phosphorus or fluoride pollution in groundwater. If it is recycled and applied in road engineering, its water swelling characteristics will cause cracking of the road. Therefore, the development of a regeneration road technology that takes into account the recycling of phosphogypsum and avoids the influence of its impurities is imminent.
[0003] In the past, road bases were mostly made of lime-stabilized soil or cement-stabilized soil. When roads were renovated or expanded, a large amount of inorganic binder-stabilized soil milling materials were produced. This type of milling material has no gradation and poor structural stability. If it is directly recycled in the road without treatment, it will have a great impact on the structural stability. Basalt fiber is a fiber made by continuously drawing basalt after high-temperature melting. It is often used in cement-based materials to enhance its toughness and structural stability, and can be used in cement-stabilized regenerated bases. However, due to the poor hydrophilicity of basalt fiber, it is easy to disperse unevenly in cement-based materials, forming clumps and bundles, which greatly limits the improvement of material performance and even has a negative impact.
[0004] Therefore, if a new formula of recycled base material can be developed, phosphogypsum can be modified and recycled, the impact of impurities can be greatly reduced; and the stability of inorganic binder stabilized soil when recycled and applied to the base layer and the uniformity of basalt fiber dispersion in cement-based materials can be ensured. Not only can industrial waste and road waste be recycled and reused in roads, reducing the exploitation and waste of natural resources; it can also prevent phosphorus-containing impurities from polluting groundwater and protect water resources; and the toughness of recycled base materials can be greatly improved, extending the service life of roads, with good economic and environmental benefits. Summary of the invention
[0005] The purpose of the present invention is to overcome at least one of the defects of the above-mentioned prior art and to provide a high-toughness fiber water-stabilized phosphogypsum regenerated base material and a preparation method thereof, which increases the recycling rate of waste asphalt pavement materials and industrial waste phosphogypsum, improves the toughness of cement cold regenerated base, reduces the formation of reflective cracks, and extends the service life of regenerated roads.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A high-tenacity fiber water-stable phosphogypsum regeneration base material, the base material comprises the following components by weight:
[0008] 100 parts of recycled asphalt pavement materials, including 45-75 parts of recycled asphalt mixture materials and 25-55 parts of inorganic recycled materials;
[0009]
[0010] Furthermore, the base material includes the following components in parts by weight: 50-70 parts of recycled asphalt mixture, 30-40 parts of inorganic recycled material, 40-50 parts of phosphogypsum, 12-13.5 parts of cement, 0.15-0.2 parts of fiber, 1.5-2 parts of modifier, and 2-3 parts of stabilizer.
[0011] Furthermore, the asphalt mixture recycled material is asphalt pavement surface milling material;
[0012] The inorganic recycled material is lime stabilized soil, cement stabilized soil or lime fly ash stabilized soil, preferably lime stabilized soil;
[0013] The cement is ordinary Portland cement with a strength grade of 42.5 and a fineness of ≤10%.
[0014] Furthermore, the phosphogypsum has a passing rate through a 200 μm sieve hole of greater than or equal to 80%, a content of calcium sulfate dihydrate of ≥90%, a pH value of ≥5, and an adhesion moisture content of ≤15%.
[0015] Furthermore, the fiber is BSⅡ type basalt fiber treated with low temperature plasma, with a fiber length of 16 mm and a tensile strength of ≥3500 MPa.
[0016] Furthermore, the low-temperature plasma treatment method is: using a low-temperature plasma surface processor, the output power is 200W, and the nozzle distance is 20mm to surface treat the BSⅡ type basalt fiber for 120s.
[0017] Furthermore, the modifier consists of tris(hydroxymethyl)aminomethane, sodium ricinoleate, calcium hydroxide and konjac mannan; the mass ratio of tris(hydroxymethyl)aminomethane, sodium ricinoleate, calcium hydroxide and konjac mannan is 2:3:2:3.
[0018] Furthermore, the stabilizer consists of aluminum pillared montmorillonite, zeolite powder and sodium gluconate; the mass ratio of aluminum pillared montmorillonite, zeolite powder and sodium gluconate is 1:1:2.
[0019] The material used in the present invention is low-temperature plasma treated BSⅡ basalt fiber. BSⅡ basalt fiber has strong alkali corrosion resistance and excellent tensile properties, which can effectively improve the toughness of the base material. After low-temperature plasma surface treatment, the roughness of the fiber surface increases, the bonding effect between the fiber and cement hydration products increases, and the bridging effect is enhanced; and the hydrophilicity of the fiber surface is improved to avoid agglomeration and bundle formation, and the dispersion in the base material is more uniform, which can significantly improve the material's crack resistance.
[0020] As for the modifier, sodium ricinoleate is an anionic surfactant that can adapt to a wide range of pH environments. It can be used as a collector to specifically adsorb and wrap phosphorus-containing impurities such as P2O5, effectively reducing the wrapping effect of phosphorus-containing impurities on cement stone, increasing the degree of freedom of hydration nuclei, and enhancing the compatibility of phosphogypsum and cement. Tris(hydroxymethyl)aminomethane and calcium hydroxide have hydroxyl or amino groups with excellent fluoride removal capabilities, which can reduce the content of soluble fluorine impurities in phosphogypsum, and calcium hydroxide can enhance the alkalinity of the material environment, which can further improve the performance of phosphogypsum. The calcium ions it provides can also react with free fluoride ions to generate fine calcium fluoride particles. Konjac mannan is a heat-resistant gel-like substance. When added to the mixture, it can effectively adsorb and wrap phosphorus-containing and fluorine-containing impurities such as calcium fluoride, and still maintain good structural stability under hydration exothermic conditions, greatly reducing the impact of impurities in phosphogypsum on cement hydration.
[0021] As for stabilizers, aluminum-pillared montmorillonite and zeolite powder have large interlayer spacing and good heat resistance. They can absorb and isolate phosphogypsum impurities and their solidified products in the interlayer by adsorption, thereby promoting cement hydration, greatly reducing the seepage of harmful substances, and reducing the pollution of phosphogypsum to the environment. In addition, aluminum-pillared montmorillonite can also provide some aluminum ions through ion exchange, promote the positive hydration reaction, fill the tiny pores inside the material, and improve the ability to resist frost heave. Sodium gluconate is a cost-effective water reducer that can reduce the unit water consumption of the material, weaken the water swelling reaction of phosphogypsum, and reduce the temperature shrinkage and dry-wet shrinkage of cement, which can effectively avoid the formation of cracks in the curing stage.
[0022] A method for preparing the high-tenacity fiber water-stable phosphogypsum regeneration base material as described above, the method comprising the following steps:
[0023] Dry mix part of the asphalt pavement recycling material, part of the phosphogypsum and part of the cement and mix them evenly;
[0024] Add the fiber and continue stirring until it is evenly mixed;
[0025] Add the remaining asphalt pavement recycling materials, phosphogypsum, cement, modifier and water and mix quickly;
[0026] Add the stabilizer and mix evenly to obtain the high-tenacity fiber water-stabilized phosphogypsum recycled base material.
[0027] Or the preparation method comprises the following steps:
[0028] (1) Dry mix part of the asphalt pavement recycled material, part of the phosphogypsum and part of the cement and mix them evenly;
[0029] (2) Add fiber and continue stirring until it is evenly mixed;
[0030] (3) Add the remaining asphalt pavement recycled material, phosphogypsum, cement, modifier and water and mix quickly;
[0031] (4) Add stabilizer and mix evenly;
[0032] (5) Conduct indoor compaction tests according to the Test Code for Stabilized Materials with Inorganic Binders for Highway Engineering (JTG E51-2009) to determine the optimum moisture content and maximum dry density, and then decide on the amount of water to be added;
[0033] (6) Repeat the above steps (1) to (4) according to the optimum moisture content to obtain a high-tenacity fiber-type water-stable phosphogypsum recycled base material.
[0034] In the first four steps, the amount of water added is arbitrary. When the amount of water added in step (5) is determined, the first four steps are repeated to obtain a formal sample. The specific amount of water added can be referred to Table 1.
[0035] Furthermore, the amount of water added is determined based on the optimal moisture content and the maximum dry density determined by indoor compaction tests; the dry mixing time is 1-2 minutes, the continued mixing time is 1-2 minutes, and the rapid mixing time is 0.5 minutes.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The present invention has high economic benefits and can recycle a large amount of phosphogypsum, road surface milling materials and inorganic binder stabilized soil, thereby reducing the construction cost;
[0038] (2) The present invention is green, energy-saving and environmentally friendly, reduces the exploitation of natural resources, reduces the infiltration of phosphorus and fluorine-containing pollutants, and protects groundwater resources;
[0039] (3) The high-toughness fiber water-stable phosphogypsum recycled base material of the present invention has high toughness and excellent crack resistance, thereby reducing the generation of reflective cracks in the pavement structure layer and extending the service life of the road. DETAILED DESCRIPTION
[0040] The following is a detailed description of an embodiment of the present invention. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiment.
[0041] A high-tenacity fiber water-stabilized phosphogypsum regeneration base material and a preparation method thereof, the purpose of which is to increase the recycling rate of waste asphalt pavement materials and industrial waste phosphogypsum, and to improve the toughness of cement cold regeneration base, reduce the generation of reflective cracks, and extend the service life of the regenerated road. The raw materials include the following components by weight: 100 parts of asphalt pavement recycled materials, 30-50 parts of phosphogypsum, 12-16 parts of cement, 0.1-0.3 parts of low-temperature plasma treated BSⅡ basalt fiber, 1-3 parts of modifier, and 1.5-3 parts of stabilizer: in the asphalt pavement recycled materials, 60-80 parts of asphalt mixture recycled materials and 20-40 parts of inorganic recycled materials. The asphalt mixture recycled materials are asphalt pavement surface milling materials. The inorganic recycled materials can be lime stabilized soil, cement stabilized soil or lime fly ash stabilized soil.
[0042] The passing rate of phosphogypsum through a 200μm sieve is greater than or equal to 80%, the content of calcium sulfate dihydrate is ≥90%, the pH value is ≥5, and the adhesion moisture content is ≤15%. The cement is ordinary Portland cement, the cement strength grade is 42.5, and the fineness is ≤10%.
[0043] The fiber is BSⅡ basalt fiber treated with low temperature plasma. The basalt fiber used is BSⅡ basalt fiber with a fiber length of 16mm and a tensile strength of ≥3500MPa. The specific preparation method is to use a low temperature plasma surface processor with an output power of 200W and a nozzle distance of 20mm to surface treat the BSⅡ basalt fiber for 120s.
[0044] The modifier is prepared by mixing tris(hydroxymethyl)aminomethane, sodium ricinoleate, calcium hydroxide and konjac mannan in a mass ratio of 2:3:2:3. The stabilizer is prepared by mixing aluminum pillared montmorillonite, zeolite powder and sodium gluconate, and the specific preparation method is to prepare the stabilizer by ultrasonic emulsification in a mass ratio of 1:1:2 and then drying.
[0045] The specific preparation method is:
[0046] (1) Dry mix part of the asphalt pavement recycled material, part of the phosphogypsum and part of the cement and mix them evenly;
[0047] (2) Add fiber and continue stirring until it is evenly mixed;
[0048] (3) Add the remaining asphalt pavement recycled material, phosphogypsum, cement, modifier and water and mix quickly;
[0049] (4) Add stabilizer and mix evenly;
[0050] (5) Conduct indoor compaction tests according to the Test Code for Stabilized Materials with Inorganic Binders for Highway Engineering (JTG E51-2009) to determine the optimum moisture content and maximum dry density, and then decide on the amount of water to be added;
[0051] (6) Repeat the above steps (1) to (4) according to the optimum moisture content to obtain a high-tenacity fiber-type water-stable phosphogypsum recycled base material.
[0052] Example 1
[0053] A high-tenacity fiber water-stabilized phosphogypsum recycled base material and a preparation method thereof, wherein the components are distributed according to the mass ratio as follows: 100 parts of asphalt pavement recycled material, including 60 parts of asphalt surface layer recycled material, 40 parts of lime-stabilized soil recycled material, 40 parts of phosphogypsum, 12 parts of cement, 0.15 parts of fiber, 1.5 parts of modifier, and 2 parts of stabilizer. The specific preparation method is as follows:
[0054] S1: Dry mix half of the asphalt pavement recycled material, half of the phosphogypsum and half of the cement for 2 minutes and mix them evenly;
[0055] S2: Add the fiber and continue stirring for 2 minutes until it is evenly mixed;
[0056] S3: Add the remaining asphalt pavement recycled materials, phosphogypsum and cement, modifier and water and mix quickly for 0.5min;
[0057] S4: Finally, add the stabilizer and mix evenly;
[0058] S5: According to the "Testing Procedures for Stabilized Materials with Inorganic Binders for Highway Engineering" (JTG E51-2009), indoor compaction tests are conducted to determine the optimum moisture content and maximum dry density, and then the amount of water to be added is determined;
[0059] S6: According to the amount of water added determined by the optimum moisture content, the above S1-S4 are repeated to obtain a high-tenacity fiber water-stable phosphogypsum recycled base material.
[0060] The specific test method is as follows:
[0061] 7d unconfined compressive strength test: According to the method in the "Testing Procedure for Inorganic Binder Stabilized Materials for Highway Engineering" (JTGE51-2009), a cylindrical specimen of 150mm×150mm×100mm was formed, and the 7d unconfined compressive strength test was carried out according to the above procedure. The test was carried out using a TYE-2000B press, and the loading mode was selected as 1mm / min displacement loading control.
[0062] Temperature shrinkage and drying shrinkage test: According to the method in "Test Code for Stabilized Materials of Inorganic Binders for Highway Engineering" (JTG E51-2009), a 100mm×100mm×400mm beam-shaped specimen was formed. The temperature shrinkage performance of the mixture was tested by the strain gauge method according to the above regulations. The area to be tested was smoothed with epoxy resin, and the strain gauge was pasted. The temperature change area of the high and low temperature alternating box was set to 45℃~-5℃, and maintained for 6 hours every time the temperature changed by 10℃, and the relevant data of temperature shrinkage performance were recorded; the drying shrinkage performance of the mixture was tested by the vertical column test method according to the above regulations.
[0063] Bending toughness test: According to the method in the "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" (JTG E51-2009), a beam-shaped specimen of 100mm×100mm×400mm was formed. After demoulding, the formed beam-shaped specimen was cured in a curing box under standard curing conditions for 28 days. After curing, the specimen was placed in a water tank and soaked in water for 1 day. The specimen was taken out and the surface moisture was dried with a towel for bending toughness test. The four-point bending test was carried out using the MTS universal tester. After the specimen was placed on the loading platform, a 100N pressure was applied to pre-press until the pressure head and the specimen were in full contact. Finally, a displacement loading rate of 1mm / min was used to directly destroy the specimen. The data was recorded to draw the load-deflection curve and the bending toughness was calculated according to the following formula.
[0064]
[0065] is the equivalent bending-tensile strength ratio when the characteristic deflection is L / a, where a can be 150 or 600; L, b, d are the length, width and height of the specimen respectively; f1 is the peak load strength; It is the integral of the load-deflection curve when the characteristic deflection is L / a, where a can be 150 or 600.
[0066] Example 2
[0067] A high-tenacity fiber water-stabilized phosphogypsum recycled base material and a preparation method thereof, wherein the components are distributed according to mass proportion as follows: 100 parts of asphalt pavement recycled material, including 50 parts of asphalt surface layer recycled material, 50 parts of lime-stabilized soil recycled material, 50 parts of phosphogypsum, 13.5 parts of cement, 0.25 parts of fiber, 2 parts of modifier, and 3 parts of stabilizer. The specific preparation method and experimental method are consistent with those in Example 1.
[0068] Example 3
[0069] A high-tenacity fiber water-stabilized phosphogypsum recycled base material and a preparation method thereof, wherein the components are distributed according to mass proportion as follows: 100 parts of asphalt pavement recycled material, including 60 parts of asphalt surface layer recycled material, 40 parts of lime-stabilized soil recycled material, 50 parts of phosphogypsum, 12.5 parts of cement, 0.23 parts of fiber, 2 parts of modifier, and 2.5 parts of stabilizer. The specific preparation method and experimental method are consistent with those in Example 1.
[0070] Example 4
[0071] A high-tenacity fiber water-stabilized phosphogypsum recycled base material and a preparation method thereof, wherein the components are distributed according to mass proportion as follows: 100 parts of asphalt pavement recycled material, including 70 parts of asphalt surface layer recycled material, 30 parts of lime-stabilized soil recycled material, 50 parts of phosphogypsum, 12 parts of cement, 0.2 parts of fiber, 2 parts of modifier, and 2 parts of stabilizer. The specific preparation method and experimental method are consistent with those in Example 1.
[0072] Comparative Example 1
[0073] A recycled base material and a preparation method thereof, wherein the components are distributed according to mass proportion as follows: 100 parts of asphalt pavement recycled material, including 60 parts of asphalt surface layer recycled material, 40 parts of lime-stabilized soil recycled material, 40 parts of phosphogypsum, and 12 parts of cement. The specific preparation method and experimental method are consistent with those in Example 1.
[0074] Comparative Example 2
[0075] A recycled base material and a preparation method thereof, wherein the components are distributed according to mass proportion as follows: 100 parts of asphalt pavement recycled material, including 60 parts of asphalt surface layer recycled material, 40 parts of lime-stabilized soil recycled material, 40 parts of phosphogypsum, 12 parts of cement, and 0.15 parts of fiber. The specific preparation method and experimental method are consistent with those in Example 1.
[0076] Comparative Example 3
[0077] A recycled base material and a preparation method thereof, wherein the components are distributed according to the mass ratio as follows: 100 parts of asphalt pavement recycled material, including 60 parts of asphalt surface layer recycled material, 40 parts of lime-stabilized soil recycled material, 40 parts of phosphogypsum, 12 parts of cement, 0.15 parts of fiber, and 1.5 parts of modifier. The specific preparation method and experimental method are consistent with those in Example 1.
[0078] Comparative Example 4
[0079] A recycled base material and a preparation method thereof, wherein the components are distributed according to the mass ratio as follows: 100 parts of asphalt pavement recycled material, including 60 parts of asphalt surface layer recycled material, 40 parts of lime stabilized soil recycled material, 40 parts of phosphogypsum, 12 parts of cement, 0.15 parts of fiber, and 2 parts of stabilizer. The specific preparation method and experimental method are consistent with those in Example 1.
[0080] Table 1 High-tenacity fiber water-stable phosphogypsum regeneration base material comparative examples and examples material composition
[0081]
[0082] Table 2 Experimental results of high-tenacity fiber water-stable phosphogypsum recycled base material case
[0083]
[0084] Note: “ / ” indicates that the specimen was damaged just when it reached or before reaching this condition.
[0085] By comparing Comparative Examples 1-4 and Examples 1-4 in Table 1, it can be seen that the optimal moisture content of the high-toughness fiber water-stable phosphogypsum regeneration base material of the present invention is relatively low. The specific comparison is as follows:
[0086] By comparing Example 1 and Comparative Example 3, it can be seen that the addition of the stabilizer can effectively reduce the water consumption of the material, mainly because the stabilizer contains sodium gluconate, which can ensure the construction and workability of the cement-based material while effectively reducing the amount of water.
[0087] Comparative Example 4 lacks a modifier compared to Example 1, resulting in a decrease in 7d unconfined compressive strength and bending toughness, and an increase in average temperature shrinkage coefficient and dry shrinkage coefficient. This is because the sodium ricinoleate contained in the modifier can capture phosphorus-containing impurities in a targeted manner and optimize the performance of phosphogypsum; tris(hydroxymethyl)aminomethane and calcium hydroxide in the modifier component can also remove fluorine-containing impurities in phosphogypsum, reduce the wrapping of cement stone by impurities, and improve hydration efficiency; and the konjac mannan in the modifier has good heat resistance, can remain stable under hydration conditions, and further adsorbs impurities in a gel-like structure. Thus, the compressive strength of the material can be greatly improved, and the bending toughness and shrinkage resistance are also improved to a certain extent, that is, the modifier contributes more to the compressive strength.
[0088] Compared with Example 1, Comparative Example 3 lacks a stabilizer, resulting in a decrease in the 7d unconfined compressive strength and flexural toughness, an increase in the average thermal shrinkage coefficient and the dry shrinkage coefficient, and the range of change is different from that of Comparative Example 4. The stabilizer has a stronger contribution to the shrinkage resistance. This is because the aluminum-pillared montmorillonite and zeolite powder in the stabilizer can adsorb the free impurity particles after solidification, which is conducive to the formation of material strength; in addition, the aluminum-pillared montmorillonite can also provide part of the aluminum ions through ion exchange, promote the hydration reaction, reduce the free water content in the material, and further fill the fine cracks inside the material; the sodium gluconate in the stabilizer takes into account the effects of slow setting and water reduction at the same time, greatly reduces the water consumption of cement-based materials, and can effectively enhance the shrinkage resistance and flexural toughness of the material, that is, the stabilizer mainly contributes to the shrinkage resistance, and also has a certain contribution to the compressive strength.
[0089] Compared with Example 2, Example 1 lacks the low-temperature plasma BSⅡ basalt fiber, resulting in a decrease in the 7d unconfined compressive strength and flexural toughness, and an increase in the average thermal shrinkage coefficient and dry shrinkage coefficient. This is because BSⅡ basalt fiber is a high-strength basalt fiber with excellent tensile resistance, which can improve the overall flexural and tensile resistance of the material through bridging effect; and after low-temperature plasma treatment, the hydrophilicity of the fiber is enhanced, and the dispersion uniformity in the cement base is greatly improved, avoiding the influence of fiber agglomeration and hydrophobicity caused by fine bubbles on the strength; in addition, low-temperature plasma can enhance the roughness of the fiber surface, greatly increase the friction between the fiber and cement stone, phosphogypsum and pavement recycled materials, thereby effectively improving the flexural toughness of the mixture, that is, the fiber mainly improves the flexural toughness.
[0090] It can be seen from Table 2 that the high-tenacity fiber water-stable phosphogypsum recycled base material of the present invention has a shrinkage coefficient and an average temperature shrinkage coefficient that are 20-30% lower than those of the comparative case, has a strong anti-shrinkage ability, can effectively reduce the generation of internal microcracks, and avoid the material from cracking under the influence of multiple factors such as phosphogypsum water swelling, temperature, and dry and wet shrinkage; from the bending toughness test results, it can be seen that the high-tenacity fiber water-stable phosphogypsum recycled base material of the present invention has a higher equivalent flexural tensile strength ratio, can still have a strong bearing capacity even with a large deformation, can greatly improve the toughness of the base material, thereby enhancing its anti-destruction ability under shrinkage and load.
[0091] Further comparison of the test results of Comparative Example 4 and Example 2 shows that the high-tenacity fiber water-stable phosphogypsum regeneration base material of the present invention can improve the recycling rate of stabilized soil and phosphogypsum while ensuring that the material has excellent anti-shrinkage performance and toughness. The 7d unconfined compressive strength test results show that the high-tenacity fiber water-stable phosphogypsum regeneration base material of the present invention also has excellent compressive performance, and can meet the requirements of the "Highway Asphalt Pavement Regeneration Specification" (JTG / T 5521-2019) for the 7d unconfined compressive strength of the base layer under heavy traffic ≥3MPa and there is still surplus, so the high-tenacity fiber water-stable phosphogypsum regeneration base material of the present invention can be directly applied to the base or subbase of heavy-load traffic highways.
[0092] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A high-tenacity fiber water-stable phosphogypsum regeneration base material, characterized in that: The base material comprises the following components by weight: 100 parts of recycled asphalt pavement materials, including 45-75 parts of recycled asphalt mixture materials and 25-55 parts of inorganic recycled materials; The modifier is composed of tris(hydroxymethyl)aminomethane, sodium ricinoleate, calcium hydroxide and konjac mannan, and the mass ratio of tris(hydroxymethyl)aminomethane, sodium ricinoleate, calcium hydroxide and konjac mannan is 2:3:2:3; The stabilizer is composed of aluminum pillared montmorillonite, zeolite powder and sodium gluconate, and the mass ratio of aluminum pillared montmorillonite, zeolite powder and sodium gluconate is 1:1:2; The asphalt mixture recycled material is the asphalt pavement surface milling material; The inorganic recycled material is lime stabilized soil, cement stabilized soil or lime fly ash stabilized soil.
2. A high-tenacity fiber water-stable phosphogypsum regeneration base material according to claim 1, characterized in that: The base material comprises the following components by weight: 50-70 parts of asphalt mixture recycled material, 30-40 parts of inorganic recycled material, 40-50 parts of phosphogypsum, 12-13.5 parts of cement, 0.15-0.2 parts of fiber, 1.5-2 parts of modifier, and 2-3 parts of stabilizer.
3. A high-tenacity fiber water-stable phosphogypsum regeneration base material according to claim 1, characterized in that: The inorganic recycled material is lime-stabilized soil; The cement is ordinary Portland cement with a strength grade of 42.5 and a fineness of ≤10%.
4. The high-tenacity fiber water-stable phosphogypsum regeneration base material according to claim 1, characterized in that: The passing rate of the phosphogypsum through a 200 μm sieve hole is greater than or equal to 80%, the content of calcium sulfate dihydrate is greater than or equal to 90%, the pH value is greater than or equal to 5, and the adhesion moisture content is less than or equal to 15%.
5. The high-tenacity fiber water-stable phosphogypsum regeneration base material according to claim 1, characterized in that: The fiber is BSⅡ type basalt fiber treated with low temperature plasma, with a fiber length of 16 mm and a tensile strength of ≥3500 MPa.
6. A high-tenacity fiber water-stable phosphogypsum regeneration base material according to claim 5, characterized in that: The method of low-temperature plasma treatment is: using a low-temperature plasma surface processor, the output power is 200W, and the nozzle distance is 20mm to perform surface treatment on the BSⅡ type basalt fiber for 120s.
7. A method for preparing the high-tenacity fiber water-stable phosphogypsum regeneration base material as claimed in any one of claims 1 to 6, characterized in that: The method comprises the following steps: Dry mix part of the asphalt pavement recycling material, part of the phosphogypsum and part of the cement and mix them evenly; Add the fiber and continue stirring until it is evenly mixed; Add the remaining asphalt pavement recycling materials, phosphogypsum, cement, modifier and water and mix quickly; Add the stabilizer and mix evenly to obtain the high-tenacity fiber water-stabilized phosphogypsum recycled base material.
8. The method for preparing a high-tenacity fiber water-stable phosphogypsum regeneration base material according to claim 7, characterized in that: The amount of water added is determined based on the optimal moisture content and maximum dry density determined by indoor compaction tests; the dry mixing time is 1-2 minutes, the continued mixing time is 1-2 minutes, and the rapid mixing time is 0.5 minutes.
Citation Information
Patent Citations
Cement phosphogypsum stabilized macadam material for road base and preparation method and usage of cement phosphogypsum stabilized macadam material
CN110304884A
Road as well as water-stable layer and preparation process thereof
CN113716928A
Modified ardealite stabilized macadam as well as preparation method and application thereof
CN113754398A
Method for efficiently purifying ardealite and application
CN114906868A
Preparation method of phosphogypsum pavement base water-stable material
CN115594455A