A desulfurized gypsum-based composite building material and its preparation method and application

By combining desulfurization gypsum, lime, naphthalene water reducer, sulfaluminate cement and mycelium fiber materials, and through specific culture and stirring treatment, the strength, water resistance and bending resistance of desulfurization gypsum in the construction industry is solved. The problem of insufficient folding ability significantly improves its mechanical properties and water resistance.

CN116496062BActive Publication Date: 2024-11-15BIJIE VOCATIONAL & TECH COLLEGE (BIJIE AGRI SCHOOL GUIZHOU PROVINCE)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310492404.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-15
Estimated Expiration
2043-05-04

AI Technical Summary

Technical Problem

The application of desulfurization gypsum in the construction industry is limited by its insufficient strength, water resistance and bending resistance, and the existing technology has limited effectiveness in improving performance.

Method used

Desulfurization gypsum, lime, naphthalene water reducer, sulfur aluminate cement and mycelium fiber materials are used to prepare excellent performance desulfurization gypsum-based composite building materials through specific mixing and culture methods, including mixing wood chips and basalt fibers. Later, Yunzhi and oyster mushrooms were inoculated, cultivated to form a mycelium-base composite, dried and crushed to obtain mycelium fiber material, and stirred with lime and other raw materials to form.

Benefits of technology

The compressive strength, flexural strength and water resistance of desulfurized gypsum-based composite building materials have been significantly improved, the water absorption rate is reduced, the softening coefficient is improved, the mechanical properties and water resistance are significantly improved, and there is good application prospect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004212938690000071
    Figure BDA0004212938690000071
  • Figure BDA0004212938690000081
    Figure BDA0004212938690000081
Patent Text Reader

Abstract

The present invention provides a desulfurized gypsum-based composite building material and a preparation method and application thereof, belonging to the technical field of building materials. The present invention overcomes the problem of insufficient performance of desulfurized gypsum-based composite materials in the prior art by adding specific mycelium fiber materials. The desulfurized gypsum-based composite building material provided by the present invention has excellent performance, a compressive strength of up to 36.69 MPa, a flexural strength of up to 7.31 MPa, a water absorption rate reduced to 12.28% relative to the non-mycelium treatment, and an anti-softening coefficient of up to 0.74, achieving an improvement in the desulfurized gypsum-based composite material, having strong mechanical properties and water resistance, and having good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of building materials, and in particular to a desulfurized gypsum-based composite building material and a preparation method and application thereof. Background Art

[0002] In the context of vigorously preventing and controlling the atmospheric pollutant SO2, desulfurized gypsum came into being. It is an industrial by-product gypsum produced by wet flue gas desulfurization. In recent years, the large-scale storage of desulfurized gypsum has brought great challenges to the ecological environment. It is difficult for the original desulfurized gypsum to produce strength when used alone. When it is calcined at high temperature into semi-hydrated desulfurized gypsum or anhydrous desulfurized gypsum, although its strength can be improved, the energy consumption is high and secondary pollution is generated, which is not conducive to the large-scale promotion and application of desulfurized gypsum in the construction industry. At the same time, desulfurized gypsum has the problems of poor water resistance and poor bending resistance, which limits its application.

[0003] Untreated desulfurized gypsum does not have self-hardening gelling properties and cannot form strength by itself. Although the strength of semi-hydrated desulfurized gypsum calcined from original desulfurized gypsum has been improved, its water resistance is very poor, mainly because water molecules have a destructive effect on dihydrate gypsum crystals, resulting in its softening coefficient being only about 0.2, making it difficult to directly apply it to the building materials industry. The prior art has a variety of schemes for preparing desulfurized gypsum-based composite cementitious materials by mixing admixtures such as mineral powder, cement, fly ash, silica fume, quicklime, and admixtures such as water reducers and retarders into desulfurized gypsum, which can improve the physical and mechanical properties and water resistance of desulfurized gypsum to a certain extent, and the addition of different admixtures and admixtures makes the various properties of desulfurized gypsum-based composite cementitious materials different, but the current materials are limited, and the effect of improving performance cannot meet actual needs. Summary of the invention

[0004] The object of the present invention is to provide a desulfurized gypsum-based composite building material and a preparation method and application thereof, so as to solve the problem of insufficient performance of desulfurized gypsum-based composite materials in the prior art.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a desulfurized gypsum-based composite building material, comprising the following raw materials in parts by weight:

[0007] 70-80 parts of desulfurized gypsum, 3-8 parts of lime, 0.3-0.8 parts of naphthalene water reducer, 9-10 parts of sulphoaluminate cement, 8-12 parts of mycelium fiber material and 53-58 parts of water;

[0008] The preparation method of the mycelium fiber material comprises the following steps:

[0009] Mix wood chips, basalt fibers and water to obtain a base material;

[0010] Inoculating Coriolus versicolor and Pleurotus ostreatus into the base material and culturing the base material to obtain a mycelium-base material complex;

[0011] The mycelium-base material complex is dried and crushed to obtain mycelium fiber material.

[0012] Preferably, the weight ratio of the wood chips to the basalt fibers is 6.5-7.5:2.5-3.5.

[0013] Preferably, the water content of the base material is 55-65%.

[0014] Preferably, the inoculation amount of Coriolus versicolor is 0.7-1.3%;

[0015] The inoculation amount of the Pleurotus ostreatus is 1.7-2.3%;

[0016] The culture temperature is 24-26°C;

[0017] The culture time is 30 to 40 days.

[0018] Preferably, the wood chips and basalt fibers are sterilized before being mixed with water;

[0019] The sterilization temperature is 120-122°C;

[0020] The sterilization time is 20 to 40 minutes.

[0021] Preferably, the drying temperature is 70-80°C;

[0022] The drying time is 12 to 36 minutes;

[0023] The particle size of the mycelium fiber material is 18 to 22 mm.

[0024] The present invention also provides a method for preparing the above-mentioned desulfurized gypsum-based composite building material, comprising the following steps:

[0025] Mix the lime and water and stir for the first time to obtain a lime suspension;

[0026] The lime suspension is mixed with other raw materials and stirred for a second time to obtain a mixed material;

[0027] The mixed material is placed in a mold and solidified to obtain a semi-finished product;

[0028] The desulfurized gypsum-based composite building material is obtained by subjecting the semi-finished product to a first curing and a second curing.

[0029] Preferably, the rotation speeds of the first stirring and the second stirring are independently 2000-3000 r / h;

[0030] The time of the first stirring and the second stirring are independently 1 to 2.5 hours.

[0031] Preferably, the temperature of the first curing is 48-52°C;

[0032] The humidity of the first curing is above 85%;

[0033] The first curing time is 5 to 7 hours;

[0034] The temperature of the second curing is 25-27°C;

[0035] The second curing time is 5 to 7 days.

[0036] The present invention also provides the use of the above desulfurized gypsum-based composite building material as a building material, wherein the building material includes a structural material and / or a waterproof material.

[0037] Technical effects and advantages of the present invention:

[0038] The desulfurized gypsum-based composite building material provided by the present invention has excellent performance, a compressive strength of up to 36.69 MPa, a flexural strength of up to 7.31 MPa, a water absorption rate reduced to 12.28% relative to the sterile silk treatment, and an anti-softening coefficient of up to 0.74, thereby achieving an improvement in the desulfurized gypsum-based composite material, having strong mechanical properties and water resistance, and having good application prospects. DETAILED DESCRIPTION

[0039] The present invention provides a desulfurized gypsum-based composite building material, comprising the following raw materials in parts by weight: 70-80 parts of desulfurized gypsum, 3-8 parts of lime, 0.3-0.8 parts of naphthalene-based water reducer, 9-10 parts of sulphoaluminate cement, 8-12 parts of mycelium fiber material and 53-58 parts of water; the raw materials of the desulfurized gypsum-based composite building material of the present invention include 70-80 parts of desulfurized gypsum, preferably 73-76 parts, the raw materials of the desulfurized gypsum-based composite building material include 3-8 parts of lime, preferably 4-6 parts, the raw materials of the desulfurized gypsum-based composite building material include 0.3-0.8 parts of naphthalene-based water reducer, preferably 0.4-0.6 parts, the desulfurized The raw materials of the gypsum-based composite building material include 9 to 10 parts of sulphoaluminate cement, preferably 9.3 to 9.7 parts, the raw materials of the desulfurized gypsum-based composite building material include 53 to 58 parts of water, preferably 54 to 56 parts, the raw materials of the desulfurized gypsum-based composite building material include 8 to 12 parts of mycelium fiber material, preferably 9 to 11 parts, and the preparation method of the mycelium fiber material includes the following steps: mixing sawdust, basalt fiber and water to obtain a base material; inoculating versicolor and oyster mushroom into the base material and culturing to obtain a mycelium-base material complex; drying and crushing the mycelium-base material complex to obtain a mycelium fiber material, the weight of the sawdust and basalt fiber is 200 grams, and the weight of the sawdust and basalt fiber is 200 grams. The amount ratio is preferably 6.5-7.5:2.5-3.5, more preferably 6.8-7.2:2.8-3.2, the water content of the base material is preferably 55-65%, more preferably 58-62%; the inoculation amount of the coriolus versicolor is preferably 0.7-1.3%, more preferably 0.8-1.1%; the inoculation amount of the oyster mushroom is preferably 1.7-2.3%, more preferably 1.8-2.1%, the coriolus versicolor and oyster mushroom refer to the primary species of the corresponding strains; the culture temperature is preferably 24-26°C, more preferably 24.5-25.5°C; the culture time is preferably 30-4 0 days, more preferably 33 to 37 days; the sawdust and basalt fiber are preferably sterilized before mixing with water; the sterilization temperature is preferably 120 to 122°C, more preferably 120.5 to 121.5°C; the sterilization time is preferably 20 to 40 minutes, more preferably 25 to 35 minutes; the drying temperature is preferably 70 to 80°C, more preferably 73 to 77°C; the drying time is preferably 12 to 36 minutes, more preferably 15 to 20 minutes; the particle size of the mycelium fiber material is preferably 18 to 22 mm, more preferably 19 to 21 mm.

[0040] The present invention also provides a method for preparing the above-mentioned desulfurized gypsum-based composite building material, comprising the following steps: mixing lime and water, performing a first stirring to obtain a lime suspension; mixing the lime suspension with other raw materials, performing a second stirring to obtain a mixed material; placing the mixed material into a mold, and obtaining a semi-finished product after solidification; performing a first curing and a second curing on the semi-finished product to obtain a desulfurized gypsum-based composite building material; the speed of the first stirring is preferably 2000-3000r / h, more preferably 2300-2700r / h; the time of the first stirring is preferably 1-2.5h, more preferably 1.8-2.2h; the speed of the second stirring is preferably 2000 ~3000r / h, more preferably 2400~2600r / h; the time of the second stirring is preferably 1~2.5h, more preferably 1.2~1.5h; the temperature of the first curing is preferably 48~52℃, more preferably 49~51℃; the humidity of the first curing is preferably above 85%, more preferably above 90%; the time of the first curing is preferably 5~7h, more preferably 5.5~6.5h; the temperature of the second curing is preferably 25~27℃, more preferably 25.5~26.5℃; the time of the second curing is preferably 5~7 days, more preferably 5.5~6.5 days.

[0041] The present invention also provides the use of the above desulfurized gypsum-based composite building material as a building material, wherein the building material includes a structural material and / or a waterproof material.

[0042] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0043] Trametes versicolor (Trametes versicolor, Trametes versicolor) ATCC48424, purchased from ATCC American Type Culture Collection;

[0044] Pleurotus ostreatus, Bio-52347, purchased from Biobw strain bank;

[0045] Naphthalene-based water reducer was purchased from Shanghai Chenqi Chemical Technology Co., Ltd.;

[0046] The desulfurized gypsum was purchased from Chongqing Muchuan Gypsum Building Materials Co., Ltd. It is light yellow in color and has gelling properties after being mixed with water. The physical performance indicators are as follows:

[0047] The 2h compressive strength is 7.02MPa; the 2h flexural strength is 3.46MPa; the 7d compressive strength is 6.44MPa; the 7d flexural strength is 2.86MPa; the softening coefficient is 0.45; the moisture content is 28.7%; and the water absorption rate is 32.6%.

[0048] Example 1

[0049] The wood chips and basalt fibers sterilized by high pressure (121°C, 30 min) were mixed in a weight ratio of 7:3, sterile water was added until the water content was 60%, and the first-grade species of Coriolus versicolor were inoculated at an inoculation rate of 1% of the weight of the base material, and the first-grade species of Pleurotus ostreatus were inoculated at an inoculation rate of 2% of the base material, mixed well, and cultured at 24°C for 35 days to allow the base material to be covered with mycelium;

[0050] The base material covered with mycelium was taken out, dried at 75°C for 24 hours, and then crushed into 20 mm particle size for later use;

[0051] Prepare materials: 75 parts of desulfurized gypsum, 5 parts of lime, 0.5 parts of naphthalene-based water reducer, 9.5 parts of sulphoaluminate cement, 10 parts of mycelium material and 55 parts of water.

[0052] Mix lime and water, stir them in a mixer at a speed of 2500r / h for 2h, add the remaining materials, stir them evenly at the same speed for 1h, put them into a mold to shape them, put them in a curing box with a temperature of 52°C and a humidity of more than 95% after shaping, take them out after 5h, and place them indoors at 26°C for 7 days to obtain a desulfurized gypsum-based composite building material.

[0053] Example 2

[0054] The wood chips and basalt fibers sterilized by high pressure (121°C, 30 min) were mixed in a weight ratio of 7.5:2.5, sterile water was added until the water content was 55%, and the first-grade species of Coriolus versicolor were inoculated at an inoculation rate of 0.7% of the weight of the base material, and the first-grade species of Pleurotus ostreatus were inoculated at an inoculation rate of 2.3% of the base material, mixed well, and cultured at 25°C for 40 days to allow the base material to be covered with mycelium;

[0055] The base material covered with mycelium was taken out, dried at 70°C for 12 hours, and then crushed into 18 mm particle size for later use;

[0056] Prepare materials: 70 parts of desulfurized gypsum, 3 parts of lime, 0.8 parts of naphthalene-based water reducer, 9 parts of sulphoaluminate cement, 12 parts of mycelium material and 53 parts of water.

[0057] Mix lime and water, stir them in a mixer at a speed of 2000r / h for 1.5h, add the remaining materials, stir them evenly at the same speed for 1h, put them into a mold to shape them, put them in a curing box with a temperature of 50℃ and a humidity of more than 90% after shaping, take them out after 7h, and place them indoors at 25℃ for 6 days to obtain desulfurized gypsum-based composite building materials.

[0058] Example 3

[0059] The wood chips and basalt fibers sterilized by high pressure (121°C, 30 min) were mixed in a weight ratio of 6.5:3.5, sterile water was added until the water content was 65%, and the first-grade species of Coriolus versicolor were inoculated at an inoculation rate of 1.3% of the weight of the base material, and the first-grade species of Pleurotus ostreatus were inoculated at an inoculation rate of 1.7% of the base material, mixed well, and cultured at 26°C for 30 days to allow the base material to be covered with mycelium;

[0060] The base material covered with mycelium was taken out, dried at 80°C for 36 hours, and then crushed into 22mm particle size for later use;

[0061] Prepare materials: 80 parts of desulfurized gypsum, 8 parts of lime, 0.3 parts of naphthalene-based water reducer, 10 parts of sulphoaluminate cement, 8 parts of mycelium material and 58 parts of water.

[0062] Mix lime and water, stir them in a mixer at a speed of 3000r / h for 2.5h, add the remaining materials, stir them evenly at the same speed for 1h, put them into a mold to shape them, put them in a curing box with a temperature of 48°C and a humidity of more than 85% after shaping, take them out after 6h, and place them indoors at 27°C for 5 days to obtain desulfurized gypsum-based composite building materials.

[0063] Comparative Example 1

[0064] Prepare materials: 75 parts of desulfurized gypsum, 5 parts of lime, 0.5 parts of naphthalene-based water reducer, 9.5 parts of sulphoaluminate cement, 10 parts of basalt fiber and 55 parts of water.

[0065] Mix lime and water, stir them in a mixer at a speed of 2500r / h for 2h, add the remaining materials, stir them evenly at the same speed for 1h, put them into a mold to shape them, put them in a curing box with a temperature of 52°C and a humidity of more than 95% after shaping, take them out after 5h, and place them indoors at 26°C for 7 days to obtain a desulfurized gypsum-based composite building material.

[0066] Comparative Example 2

[0067] The wood chips and basalt fibers sterilized by high pressure (121°C, 30 min) were mixed in a weight ratio of 7:3, sterile water was added until the water content was 60%, and the first-grade species of Coriolus versicolor were inoculated at an inoculum amount of 3% of the weight of the base material, mixed well, and cultured at 24°C for 35 days to allow the base material to be covered with hyphae;

[0068] The base material covered with mycelium was taken out, dried at 75°C for 24 hours, and then crushed into 20 mm particle size for later use;

[0069] Prepare materials: 75 parts of desulfurized gypsum, 5 parts of lime, 0.5 parts of naphthalene-based water reducer, 9.5 parts of sulphoaluminate cement, 10 parts of mycelium material and 55 parts of water.

[0070] Mix lime and water, stir them in a mixer at a speed of 2500r / h for 2h, add the remaining materials, stir them evenly at the same speed for 1h, put them into a mold to shape them, put them in a curing box with a temperature of 52°C and a humidity of more than 95% after shaping, take them out after 5h, and place them indoors at 26°C for 7 days to obtain a desulfurized gypsum-based composite building material.

[0071] Comparative Example 3

[0072] The wood chips and basalt fibers sterilized by high pressure (121°C, 30 min) were mixed in a weight ratio of 7:3, sterile water was added until the water content was 60%, and the first-grade species of Pleurotus ostreatus were inoculated at an inoculum amount of 3% of the weight of the base material, mixed well, and cultured at 24°C for 35 days to allow the base material to be covered with mycelium;

[0073] The base material covered with mycelium was taken out, dried at 75°C for 24 hours, and then crushed into 20 mm particle size for later use;

[0074] Prepare materials: 75 parts of desulfurized gypsum, 5 parts of lime, 0.5 parts of naphthalene-based water reducer, 9.5 parts of sulphoaluminate cement, 10 parts of mycelium material and 55 parts of water.

[0075] Mix lime and water, stir them in a mixer at a speed of 2500r / h for 2h, add the remaining materials, stir them evenly at the same speed for 1h, put them into a mold to shape them, put them in a curing box with a temperature of 52°C and a humidity of more than 95% after shaping, take them out after 5h, and place them indoors at 26°C for 7 days to obtain a desulfurized gypsum-based composite building material.

[0076] Comparative Example 4

[0077] Sterile water was added to the sawdust after high-pressure sterilization (121°C, 30 min) until the water content was 60%, and the first-grade species of Coriolus versicolor was inoculated at an inoculation rate of 1% of the weight of the base material, and the first-grade species of Pleurotus ostreatus was inoculated at an inoculation rate of 2% of the base material, mixed well, and cultured at 24°C for 35 days to allow the base material to be covered with mycelium;

[0078] The base material covered with mycelium was taken out, dried at 75°C for 24 hours, and then crushed into 20 mm particle size for later use;

[0079] Prepare materials: 75 parts of desulfurized gypsum, 5 parts of lime, 0.5 parts of naphthalene-based water reducer, 9.5 parts of sulphoaluminate cement, 5 parts of mycelium material, 5 parts of basalt fiber and 55 parts of water.

[0080] Mix lime and water, stir them in a mixer at a speed of 2500r / h for 2h, add the remaining materials, stir them evenly at the same speed for 1h, put them into a mold to shape them, put them in a curing box with a temperature of 52°C and a humidity of more than 95% after shaping, take them out after 5h, and place them indoors at 26°C for 7 days to obtain a desulfurized gypsum-based composite building material.

[0081] Experimental Example 1

[0082] The performance of the desulfurized gypsum-based composite building materials prepared in Example 1 and Comparative Examples 1 to 4 was measured respectively. The flexural strength, compressive strength and gypsum hardness were measured in accordance with the "Measurement of Mechanical Properties of Building Gypsum GB / T 17669.3-1999", and the water resistance was measured in accordance with the "Gypsum Block JC / T698-2010". The results are shown in Table 1 below:

[0083] Table 1 Desulfurization gypsum-based composite building materials performance test results

[0084]

[0085]

[0086] The results show that the desulfurized gypsum-based composite building material provided by the present invention has excellent performance, with a compressive strength of up to 36.69 MPa, a flexural strength of up to 7.31 MPa, a water absorption rate reduced to 12.28% relative to the sterile silk treatment, and an anti-softening coefficient of up to 0.74, which achieves an improvement in the desulfurized gypsum-based composite material, has strong mechanical properties and water resistance, and has good application prospects.

[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A desulfurized gypsum-based composite building material, characterized in that: The invention comprises the following raw materials in parts by weight: 70-80 parts of desulfurized gypsum, 3-8 parts of lime, 0.3-0.8 parts of naphthalene water reducer, 9-10 parts of sulphoaluminate cement, 8-12 parts of mycelium fiber material and 53-58 parts of water; The preparation method of the mycelium fiber material comprises the following steps: Mix wood chips, basalt fibers and water to obtain a base material; Inoculating Coriolus versicolor and Pleurotus ostreatus into the base material and culturing the base material to obtain a mycelium-base material complex; The mycelium-base material complex is dried and crushed to obtain mycelium fiber material.

2. The desulfurized gypsum-based composite building material according to claim 1, characterized in that: The weight ratio of the wood chips to the basalt fibers is 6.5-7.5:2.5-3.

5.

3. The desulfurized gypsum-based composite building material according to claim 2, characterized in that: The water content of the base material is 55-65%.

4. The desulfurized gypsum-based composite building material according to claim 3, characterized in that: The inoculation amount of Coriolus versicolor is 0.7-1.3%; The inoculation amount of the Pleurotus ostreatus is 1.7-2.3%; The culture temperature is 24-26°C; The culture time is 30 to 40 days.

5. The desulfurized gypsum-based composite building material according to claim 4, characterized in that: The sawdust and basalt fibers are sterilized before being mixed with water; The sterilization temperature is 120-122°C; The sterilization time is 20 to 40 minutes.

6. The desulfurized gypsum-based composite building material according to claim 5, characterized in that: The drying temperature is 70-80°C; The drying time is 12 to 36 minutes; The particle size of the mycelium fiber material is 18 to 22 mm.

7. The method for preparing the desulfurized gypsum-based composite building material according to any one of claims 1 to 6, characterized in that: The following steps are involved: Mix the lime and water and stir for the first time to obtain a lime suspension; The lime suspension is mixed with other raw materials and stirred for a second time to obtain a mixed material; The mixed material is placed in a mold and solidified to obtain a semi-finished product; The desulfurized gypsum-based composite building material is obtained by subjecting the semi-finished product to a first curing and a second curing.

8. The method for preparing the desulfurized gypsum-based composite building material according to claim 7, characterized in that: The rotation speeds of the first stirring and the second stirring are independently 2000-3000 r / h; The time of the first stirring and the second stirring are independently 1 to 2.5 hours.

9. The method for preparing the desulfurized gypsum-based composite building material according to claim 8, characterized in that: The temperature of the first curing is 48-52°C; The humidity of the first curing is above 85%; The first curing time is 5 to 7 hours; The temperature of the second curing is 25-27°C; The second curing time is 5 to 7 days.

10. Use of the desulfurized gypsum-based composite building material according to any one of claims 1 to 6 or the desulfurized gypsum-based composite building material obtained by the preparation method according to claim 7 as a building material, characterized in that: The building materials include structural materials and / or waterproof materials.