Production process of high bulk coated white cardboard
Through the high-volume thickness coating of white paper paper, the fiber binding force is improved by using all wood pulp and chemical mechanical pulp, the problem of insufficient appearance and smoothness of existing paper is solved, and the improvement of high whiteness and fold resistance is achieved, satisfying the satisfaction of The use of high-end paper jams has been reduced, and power consumption and chemical medicine use have been reduced.
Patent Information
- Application Number
- CN202310649224.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-06-02
AI Technical Summary
The existing single-sided coated gray-base white coated paper has shortcomings in appearance, smoothness and uniformity, and cannot meet the needs of high-end paper jams.
The high-volume thickness coating white cardboard production process is used to slurry the surface layer, core layer and bottom layer through the paper machine pulping system, and then slurry after flowing and screening and purification in the wet part of the paper machine. The three-layer slurry is dehydrated and molded and combined. Two pressing and front-to-back drying, finally hard calendering modification and coating were used, using whole wood pulp raw materials and chemical mechanical pulp to improve fiber binding and paper-forming strength.
It achieves high whiteness, good stiffness and fold resistance, while improving the uniformity of the paper and printing surface strength, meeting the use requirements of high-end paper jams, reducing the power consumption of paper machines, and reducing the use of chemical drugs.
Smart Images

Figure CN116516726B_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of papermaking, in particular to a production process of high-bulk coated white cardboard. Background technology:
[0002] The existing single-sided coated gray-bottomed white coated paper is made of 4 layers, which are divided into surface, lining, core and bottom. The 4 layers of pulp are screened and purified before being put on the net for forming, and then go through 2 presses and light pressing before entering the front drying section, and after sizing, it goes into the back drying section and 4 coatings, and finally is wound and rewound to complete the entire papermaking process.
[0003] Single-sided coated gray-bottom white coated paper belongs to the category of packaging paper, and is mainly used for single-sided color printing to make packaging boxes. Coated white board paper has high whiteness, good ink absorption and printing gloss, and good stiffness and folding resistance.
[0004] Single-sided coated gray-bottomed white coated paper uses only waste paper as its raw material, among which the raw material ratio is: surface layer: 100% domestic waste flower paper; lining layer: 100% domestic waste flower paper; core layer: 40% domestic waste paper skin AB grade + 60% domestic waste paper skin CD grade; bottom layer: 90% domestic waste flower paper + 10% domestic waste paper skin AB grade.
[0005] The single-sided coated gray-bottom white coated paper made from the above raw materials has certain deficiencies in appearance, smoothness and uniformity, and cannot meet the needs of high-end cardboard applications such as business card printing, invitations, certificates, trademarks and packaging decoration.
[0006] In view of this, the inventor proposes the following technical solution. Summary of the invention:
[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a high-bulk coated white cardboard production process.
[0008] In order to solve the above technical problems, the present invention adopts the following technical scheme: the production process of high bulk coated white cardboard is as follows: first, the paper machine pulping system prepares the pulp for the face layer, the core layer and the bottom layer, the three layers of pulp are sent to the head box for sizing after being screened and purified in the wet part of the paper machine, the three layers of pulp are respectively dehydrated to form wet paper webs and then compounded together and enter the pressing part, and the pressing part is further dehydrated after two presses, and the paper surface is modified to form a paper sheet without light pressing; after the paper sheet leaves the pressing part, it enters the front drying section of the paper machine for pre-drying, and the moisture content of the paper sheet when it leaves the front drying section is between 5.3-8.0%; then, the sizing machine is used for sizing, and then it enters the post-drying section for post-drying, and after hard calendering modification, it enters the coating section, wherein the three passes on the front side of the paper sheet are Coating, one coating on the back; after the paper sheets are coated, they are soft calendered and modified before curling, and finally rewound into storage to make high-bulk coated white cardboard; among them, when pulping, the raw material ratio of each layer is: 75% sulfate bleached hardwood pulp + 25% sulfate bleached coniferous pulp; the raw material ratio of the core layer is: 95% chemical mechanical pulp + 5% sulfate bleached coniferous pulp; the raw material ratio of the bottom layer is: 75% sulfate bleached hardwood pulp + 25% sulfate bleached coniferous pulp; among them, the freeness of the sulfate bleached coniferous pulp used in the core layer is 170csf; when the core layer pulp is screened and purified in the wet end of the paper machine, the filter aid used for the core layer pulp is silica sol, which increases the dehydration of the core layer and improves the uniformity of the finished paper.
[0009] Furthermore, in the above technical solution, when the three layers of slurry are sizing through the flow box, the concentration of each layer of slurry is: the sizing concentration of the surface layer is 0.1-0.5%, and the pH value of the surface layer slurry is 7.5±0.5; the sizing concentration of the core layer is 1.0-1.8%, and the pH value of the core layer slurry is 7.0±0.5; the concentration of the bottom layer slurry is 0.1-0.5%, and the pH value of the bottom layer slurry is 7.5±0.5.
[0010] Furthermore, in the above technical solution, the PAC dosage of the surface layer slurry and the bottom layer slurry is 8.0Kg / T; the PAC dosage of the core layer slurry is 6Kg / T, the dry strength agent dosage of the core layer slurry is 0-8Kg / T, and a certain amount of ASA is added to the core layer according to the water absorption value.
[0011] Furthermore, in the above technical solution, the bleached coniferous pulp used in the core layer is refined by a double-disc mill to form a refined pulp with a freeness of 170 csf. The refined pulp fully fibrils the fibers, and the chemical mechanical pulp adheres to the refined pulp fibers to strengthen the bonding between the fibers and improve the strength and bonding force of the finished paper.
[0012] Furthermore, in the above technical solution, when the pressing section is working, the first shoe press in the pressing section provides the maximum dehydration, the pressure of the first shoe press is 550-600KN / M, and the dehydration amount is 60-70%, and the second shoe press takes into account partial dehydration while modifying the paper surface, and the second shoe press pressure is 750-790KN / M; the soft calendering pressure is <25KN / M.
[0013] Furthermore, in the above technical solution, the bulk thickness of the chemical mechanical pulp is ≥2.6 cm 3 / g, freeness ≥420±20csf, tensile index>18N.m / g.
[0014] Furthermore, in the above technical solution, in the front and rear drying sections, the steam low pressure is 5 bar, the low pressure temperature is 175-200°C, and the steam high pressure is 15 bar, the high pressure temperature is 185-210°C.
[0015] Furthermore, in the above technical solution, when the sizing machine is applying glue, the amount of glue applied on the front side is increased to 4-7g, and the solid content of the surface glue is increased to 15-18%, so as to increase the printing surface strength of the finished paper to above 2.3.
[0016] Furthermore, in the above technical solution, the total coating amount of the four-coating of the paper sheet is 45-55g; the wet-end dyes do not use red, black and yellow dyes, but royal blue and magenta violet dyes, and royal blue and magenta violet are added at 10-20ppm according to the hue and coverage.
[0017] Furthermore, in the above technical solution, when the paper sheet is formed and enters the front drying section, the first 1-4 groups of dry networks in the front drying section adopt a spiral dry network, and the surface of the spiral dry network is a plane, wherein the spiral dry network has multiple columns of first carriers and second carriers that are staggered, and the upper end surfaces of the first carriers and the second carriers are both planes and on the same horizontal line; the first carriers in each column are distributed in parallel, and the second carriers in each column are distributed in parallel, the first carriers and the second carriers are distributed obliquely to each other, and the end of the second carrier is embedded between the ends of two adjacent first carriers in the same column, so that a gap is formed between the two adjacent first carriers in the same column, and the end of the first carrier is embedded between the ends of two adjacent second carriers in the same column, so that a gap is formed between the two adjacent second carriers in the same column.
[0018] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0019] 1. The present invention stops using waste paper as raw material paper and adopts full wood pulp raw material. The surface layer and the bottom layer adopt kraft wood pulp (i.e. kraft bleached coniferous wood pulp and kraft bleached broadleaf wood pulp); the core layer mainly adopts chemical mechanical pulp, so that it retains a certain fiber strength while having a higher yield.
[0020] 2. In order to improve the binding force of paper, the present invention adopts a refining process to beat the freeness of the bleached coniferous pulp used in the core layer to 170csf, fully make the fibers filamentary, and adhere to the refined pulp fibers (refined bleached coniferous pulp of the kraft process) in the chemical mechanical pulp fibers, strengthen the bonding between the fibers, and improve the strength and binding force of the paper. Specifically, the bleached coniferous pulp used in the core layer is refined by a double disc mill to form a refined pulp with a freeness of 170csf, the refined pulp fully makes the fibers filamentary, and the chemical mechanical pulp adheres to the refined pulp fibers, strengthens the bonding between the fibers, and improves the strength and binding force of the paper.
[0021] 3. The existing gray-bottom white board paper machine is designed with four-layer sizing, two shoe presses and light pressing. When making white card paper, the present invention stops the original surface sizing and changes the original lining sizing to the surface sizing of the white card paper, realizing three-layer sizing to make white card paper, thereby helping the gray-bottom white board paper machine to transform into a white card paper machine.
[0022] 4. The filter aid used in the core layer slurry is silica sol. Silica sol increases the dehydration of the core layer and improves the uniformity of the white cardboard. The principle is: the action principle of silica sol is charge neutralization, and it reacts with the cationic groups exposed in the flocs after shearing. The large and fluffy flocs are connected in series into small and compact flocs, which improves the water filtration speed and the formation and uniformity of the paper sheets.
[0023] 5. In addition, the pressing section of the present invention performs two-pass pressing and does not perform light pressing, which can not only reduce the power consumption of the paper machine, but also meet the high bulk thickness requirement of white cardboard, that is, increase the bulk thickness of the finished paper. Description of the drawings:
[0024] Figure 1 It is a process flow chart of the present invention;
[0025] Figure 2 1 is a structural diagram (partial) of the spiral dryer net used in the present invention. Specific implementation method:
[0026] The present invention is further described below in conjunction with specific embodiments and drawings.
[0027] like Figure 1As shown, the present invention is a high bulk thickness coated white cardboard production process, the process is: firstly, the paper machine pulping system is used to prepare pulp for the face layer, the core layer and the bottom layer, wherein, when preparing pulp, the raw material ratio of each layer is: 75% kraft bleached hardwood pulp + 25% kraft bleached coniferous pulp; the raw material ratio of the core layer is: 95% chemical mechanical pulp + 5% kraft bleached coniferous pulp; the raw material ratio of the bottom layer is: 75% kraft bleached hardwood pulp + 25% kraft bleached coniferous pulp; wherein, the freeness of the kraft bleached coniferous pulp used in the core layer is 170csf; the three-layer pulp is sent to the headstock box for sizing after being screened and purified in the wet part of the paper machine, wherein, when the core layer pulp is screened and purified in the wet part of the paper machine, the filter aid used in the core layer pulp is silica sol, and the silica sol increases The core layer is dehydrated to improve the uniformity of the paper; the three layers of pulp are dehydrated and formed into wet paper webs, and then compounded together and enter the pressing section, and are further dehydrated after two presses in the pressing section, and the paper surface is modified to form a paper sheet without light pressing; after the paper sheet leaves the pressing section, it enters the front drying section of the paper machine for pre-drying, and the moisture content of the paper sheet when it leaves the front drying section is between 5.3-8.0%; it is then sizing by the sizing machine and then enters the post-drying section for post-drying, and enters the coating section after hard calendering and modification, wherein the front side of the paper sheet is coated three times and the back side is coated once. The main components of the coating are kaolin, calcium carbonate, and latex, and the main ratio is 25% kaolin, 75% calcium carbonate and 12 parts of latex; after the coating of the paper sheet is completed, it is soft calendered and modified before entering the curling, and finally rewound into storage to make high-bulk coated white cardboard. That is to say, the present invention stops using waste paper as the raw material paper type, and uses full wood pulp raw material. The surface layer and the bottom layer use sulfate wood pulp (i.e., sulfate bleached conifer pulp and sulfate bleached broadleaf pulp); the core layer mainly uses chemical mechanical pulp, so that it retains a certain fiber strength while having a higher yield. In order to improve the paper bonding strength, the present invention uses a refined pulping process to beat the freeness of the sulfate bleached conifer pulp used in the core layer to 170csf, fully make the fibers filamentary, and the refined pulp fibers (finely ground sulfate bleached conifer pulp) are attached to the chemical mechanical pulp fibers to strengthen the bonding between the fibers and improve the paper strength and bonding strength. Specifically, the sulfate bleached conifer pulp used in the core layer is refined by a double disc mill to form a refined pulp with a freeness of 170csf. The refined pulp fully makes the fibers filamentary, and the chemical mechanical pulp is attached to the refined pulp fibers to strengthen the bonding between the fibers and improve the paper strength and bonding strength. The existing gray-bottom white board paper machine is designed with four-layer sizing, two shoe presses and light pressing. When making white card paper, the present invention stops the original surface sizing and changes the original lining sizing to the surface sizing of the white card paper, realizing three-layer sizing to make white card paper, thereby helping the gray-bottom white board paper machine to transform into a white card paper machine.The filter aid used in the core layer slurry is silica sol, which increases the dehydration of the core layer and improves the uniformity of the white cardboard. The principle is: the action principle of silica sol is charge neutralization, and it reacts with the cationic groups exposed in the flocs after shearing, and the large and fluffy flocs are connected in series into small and compact flocs, which improves the water filtration speed and the paper sheet formation and uniformity. In addition, the press section of the present invention performs two presses without light pressing, which can not only reduce the power consumption of the paper machine, but also meet the high bulk thickness required by white cardboard, that is, improve the bulk thickness of the finished paper.
[0028] In order to make the surface layer more delicate, the overall design of the surface screen is optimized, and more surface lines are added to the surface screen to retain the same air permeability, improve the uniformity of the paper, and improve the mechanical retention capacity of the formed fibers. While improving retention, it also improves the fineness of the finished paper.
[0029] The present invention uses full wood pulp, improves product safety, and can be used for food packaging. At the same time, the pulp is clean, and the pollution and damage to the net are small. The net pressing part felt cloth cleaning agent and the net cleaning agent are stopped, the bacterial content is low, the wet part bactericide is stopped, the types and amounts of chemical drugs are reduced, and the manufacturing cost is reduced to a certain extent.
[0030] When the three layers of slurry are sizing through the headbox, the concentration of each layer of slurry is: the sizing concentration of the surface layer is 0.1-0.5%, and the pH value of the surface layer slurry is 7.5±0.5; the sizing concentration of the core layer is 1.0-1.8%, and the pH value of the core layer slurry is 7.0±0.5; the concentration of the bottom layer slurry is 0.1-0.5%, and the pH value of the bottom layer slurry is 7.5±0.5.
[0031] The PAC dosage of the surface layer slurry and the bottom layer slurry is 8.0Kg / T; the PAC dosage of the core layer slurry is 6Kg / T, the dry strength agent dosage of the core layer slurry is 0-8Kg / T, and the core layer also adds a certain amount of ASA according to the water absorption value. Specifically, the core layer also adds 0.5-1kg / t of ASA according to the water absorption value, and the water absorption value is controlled to be <50 on the front side and <60 on the back side.
[0032] When the pressing section is working, the first shoe press in the pressing section provides the maximum dehydration. The pressure of the first shoe press is 550-600KN / M, and the dehydration amount is 60-70%. The second shoe press is to modify the paper surface while taking into account partial dehydration, and the second shoe press pressure is 750-790KN / M; the soft calendering pressure is <25KN / M.
[0033] The present invention adopts three-layer papermaking, in which the core layer accounts for about 53%-67% at most. The paper is required to have high bulk thickness, that is, the chemical mechanical pulp is required to have high bulk thickness while maintaining good strength indicators. Therefore, higher requirements are put forward for raw material indicators. The chemical mechanical pulp standard is as follows: the bulk thickness of the chemical mechanical pulp is ≥2.6cm 3 / g, freeness ≥420±20csf, tensile index>18N.m / g.
[0034] The OBA (fluorescent brightener) of the surface, core and bottom layers is adjusted according to the whiteness of the finished paper. Core layer filler: 80Kg / T, composed of calcium carbonate, added before the pulping pump.
[0035] In the front and rear drying sections, the low-pressure steam pressure is 5 bar, and the low-pressure temperature is 175-200°C; the high-pressure steam pressure is 15 bar, and the high-pressure temperature is 185-210°C. The front and rear drying steam pressures and temperatures meet the requirements of paper drying.
[0036] White cardboard has extremely high requirements for the printing surface strength of the finished paper. In order to improve the printing surface strength of the finished paper, when the sizing machine is applying glue, the amount of glue applied on the front side is increased to 4-7g, and the solid content of the surface glue is increased to 15-18%, so as to increase the printing surface strength of the finished paper to above 2.3.
[0037] In order to achieve high flatness, the coating amount is increased, and the total coating amount of the paper sheet after four coatings is 45-55g; the wet-end dyes do not use red, black and yellow dyes, but royal blue and royal violet dyes, and royal blue and royal violet are added at 10-20ppm depending on the hue and coverage.
[0038] When the paper sheets are formed and enter the front drying section, the first 1-4 groups of drying nets in the front drying section use spiral drying nets 10. The surface of the spiral drying net 10 is flat. The spiral drying net 10 can reduce the air permeability of the drying net, which has a vital impact on the final shaping of the paper sheets and can improve the flatness of the paper. In addition, the spiral drying net has the best surface treatment performance at high speed, reduces stretching, and has a longer life.
[0039] Specifically, combined Figure 2 As shown, the spiral dry net 10 has a plurality of columns of staggeredly distributed first carriers 101 and second carriers 102, and the upper end surfaces of the first carriers 101 and the second carriers 102 are both planes and on the same horizontal line; the first carriers 101 in each column are distributed in parallel, and the second carriers 102 in each column are distributed in parallel, the first carriers 101 and the second carriers 102 are distributed obliquely to each other, and the end of the second carrier 102 is embedded between the ends of two adjacent first carriers 101 in the same column, so that a gap is formed between the two adjacent first carriers 101 in the same column, and the end of the first carrier 101 is embedded between the ends of two adjacent second carriers 102 in the same column, so that a gap is formed between the two adjacent second carriers 102 in the same column.
[0040] The parameters of the high bulk coated white cardboard finally prepared by the present invention are as follows: strength: RI printing times ≥3 times, surface printing strength IGT ≥2.3, folding endurance ≥23 times, internal bonding strength ≥150 J / ㎡, bulk ≥1.60, stiffness CD / MD ≥9 / 19 g.cm, paper whiteness ≥86.5% ISO, gloss ≥42%, ink absorption of 16-19, roughness ≤1um, water absorption (front / back) 35-45 / 40-45 g / ㎡.
[0041] In summary, the present invention stops using waste paper as the raw material paper type, and uses full wood pulp raw material. The surface layer and the bottom layer use sulfate wood pulp (i.e., sulfate bleached conifer pulp and sulfate bleached broadleaf pulp); the core layer mainly uses chemical mechanical pulp, so that it retains a certain fiber strength while having a higher yield. In order to improve the paper bonding strength, the present invention uses a refined pulping process to beat the freeness of the sulfate bleached conifer pulp used in the core layer to 170csf, fully make the fibers filamentary, and the refined pulp fibers (finely ground sulfate bleached conifer pulp) are attached to the chemical mechanical pulp fibers to strengthen the bonding between the fibers and improve the paper strength and bonding strength. Specifically, the sulfate bleached conifer pulp used in the core layer is refined by a double disc mill to form a refined pulp with a freeness of 170csf. The refined pulp fully makes the fibers filamentary, and the chemical mechanical pulp is attached to the refined pulp fibers to strengthen the bonding between the fibers and improve the paper strength and bonding strength. The existing gray-bottom white board paper machine is designed with four layers of sizing, two shoe presses and light pressing. When making white cardboard, the present invention stops the original surface sizing and changes the original lining sizing to the surface sizing of the white cardboard to achieve three layers of sizing to make white cardboard, which helps the gray-bottom white board paper machine to transform into a white cardboard paper machine. The filter aid used in the core layer slurry is silica sol. Silica sol increases the dehydration of the core layer and improves the uniformity of the white cardboard. The principle is: the action principle of silica sol is charge neutralization, and it reacts with the cationic groups exposed in the flocs after shearing. The large and fluffy flocs are connected in series to small and compact flocs, which improves the water filtration speed and the formation and uniformity of the paper sheets. In addition, the pressing section of the present invention performs two presses without light pressing, which can not only reduce the power consumption of the paper machine, but also meet the high bulk thickness requirements of white cardboard, that is, improve the bulk thickness of the finished paper.
[0042] Of course, the above description is only a specific embodiment of the present invention and is not intended to limit the scope of implementation of the present invention. All equivalent changes or modifications made according to the structure, characteristics and principles described in the patent application scope of the present invention should be included in the patent application scope of the present invention.
Claims
1. High bulk coated white cardboard production process, characterized by: The process is as follows: first, the paper machine pulping system prepares the face layer, core layer and bottom layer, and the three layers of pulp are sent to the headbox for sizing after being screened and purified in the wet section of the paper machine. The three layers of pulp are respectively dehydrated to form wet paper webs and then compounded together before entering the pressing section, and are further dehydrated after two presses in the pressing section, and the paper surface is modified to form a paper sheet without light pressing; after the paper sheet leaves the pressing section, it enters the front drying section of the paper machine for pre-drying, and the moisture content of the paper sheet when it leaves the front drying section is between 5.3-8.0%; then, it is sizing by the sizing machine and then enters the post-drying section for post-drying, and after hard calendering and modification, it enters the coating section, where the front side of the paper sheet is coated three times and the back side is coated once; after the coating of the paper sheet is completed, it is soft calendered and modified before entering the curling section, and finally rewound into the warehouse to make high-bulk coated white cardboard; Among them, when pulping, the raw material ratio of each layer is: 75% kraft bleached hardwood pulp + 25% kraft bleached coniferous pulp; the raw material ratio of the core layer is: 95% chemical mechanical pulp + 5% kraft bleached coniferous pulp; the raw material ratio of the bottom layer is: 75% kraft bleached hardwood pulp + 25% kraft bleached coniferous pulp; among them, the freeness of the kraft bleached coniferous pulp used in the core layer is 170csf; When the core layer slurry is screened and purified in the wet section of the paper machine, the filter aid used for the core layer slurry is silica sol, which increases the dehydration of the core layer and improves the uniformity of the finished paper; When the paper sheets are formed and enter the front drying section, the front 1-4 groups of dryer nets in the front drying section adopt a spiral dryer net (10), the surface of the spiral dryer net (10) is a plane, wherein the spiral dryer net (10) has a plurality of rows of first carriers (101) and second carriers (102) arranged in a staggered manner, and the upper end surfaces of the first carriers (101) and the second carriers (102) are both planes and are on the same horizontal line; the first carriers (101) in each row are arranged in parallel, and the second carriers (102) in each row are arranged in parallel, the first carriers (101) and the second carriers (102) are arranged obliquely to each other, the end of the second carrier (102) is embedded between the ends of two adjacent first carriers (101) in the same row, so that a gap is formed between the two adjacent first carriers (101) in the same row, and the end of the first carrier (101) is embedded between the ends of two adjacent second carriers (102) in the same row, so that a gap is formed between the two adjacent second carriers (102) in the same row; The PAC dosage of the surface layer slurry and the bottom layer slurry is 8.0kg / t; the PAC dosage of the core layer slurry is 6kg / t, and the dry strength agent dosage of the core layer slurry is 0-8kg / t. A certain amount of ASA is added to the core layer according to the water absorption value, that is, 0.5-1kg / t of ASA is added to the core layer according to the water absorption value, and the water absorption value is controlled to be <50 on the front side and <60 on the back side; The bleached softwood pulp used in the core layer is refined by double disc grinding to form a refined pulp with a freeness of 170 csf. The refined pulp fully separates the fibers, and the chemical mechanical pulp adheres to the refined pulp fibers to strengthen the bonding between the fibers and improve the strength and bonding force of the finished paper. The bulk thickness of the chemical mechanical pulp is ≥2.6 cm³ / g, the freeness is ≥420±20 csf, and the tensile index is >18 Nm / g; When applying glue on the sizing machine, increase the amount of glue applied on the front side to 4-7g and increase the solid content of the surface glue to 15-18% to increase the printing surface strength of the finished paper to above 2.3; The total coating amount of the four-coating of the paper sheet is 45-55g; the wet-end dyes do not use red, black and yellow dyes, but royal blue and royal violet dyes, and royal blue and royal violet are added at 10-20ppm according to the hue and coverage.
2. The high bulk coated white cardboard production process according to claim 1, characterized in that: When the three layers of slurry are sizing through the headbox, the concentrations of each layer of slurry are: the sizing concentration of the surface layer is 0.1-0.5%, and the pH value of the surface layer slurry is 7.5±0.5; the sizing concentration of the core layer is 1.0-1.8%, and the pH value of the core layer slurry is 7.0±0.5; the concentration of the bottom layer slurry is 0.1-0.5%, and the pH value of the bottom layer slurry is 7.5±0.
5.
3. The high bulk coated white cardboard production process according to claim 1, characterized in that: When the pressing section is working, the first shoe press in the pressing section provides the maximum dehydration. The pressure of the first shoe press is 550~600kN / m, and the dehydration rate is 60-70%. The second shoe press is to modify the paper surface while taking into account partial dehydration. The second shoe press pressure is 750~790kN / m; the soft calendering pressure is <25kN / m.
4. The high bulk coated white cardboard production process according to claim 1, characterized in that: In the front and rear drying sections, the steam low pressure is 5 bar, the low pressure temperature is 175~200℃; the steam high pressure is 15 bar, the high pressure temperature is 185~210℃.