A high-reliability high-temperature composite heat storage material and preparation method thereof

Through the separation structure of dense ceramic shell and porous carbon layer, the problems of molten salt leakage and volatility at high temperatures are solved, the heat storage density and thermal conductivity of high-temperature heat storage materials are improved, the material life is extended and the cost is reduced.

CN116535217BActive Publication Date: 2024-12-06JILIN UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310576892.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-06
Estimated Expiration
2043-05-22

AI Technical Summary

Technical Problem

Existing high-temperature heat storage materials are prone to leakage and volatility of molten salts at high temperatures, resulting in a decrease in heat storage density and insufficient thermal conductivity, which affects the reliability and life of the system.

Method used

Using a combined structure of dense ceramic shell and internal heat storage composite core material, molten salt is adsorbed in the gap between ceramic powder and thermal reinforcement, and is prepared by molding and high-temperature sintering. The ceramic shell separates molten salt and thermal conductive material from the porous carbon layer. Avoid leakage and volatility of molten salts and improve thermal conductivity.

Benefits of technology

It achieves the improvement of high heat storage density and thermal conductivity, prevents molten salt leakage and volatility, extends the service life of the material, avoids molten salt pollution and oxidation of thermally conductive materials, and has a simple process and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116535217B_ABST
    Figure CN116535217B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-reliability high-temperature composite heat storage material and a preparation method thereof, a high-reliability high-temperature composite heat storage material and a preparation method thereof, the main purpose of which is to solve the problems of molten salt leakage and volatilization, and to develop a ss-PCM with high heat storage density, high thermal conductivity and excellent reliability performance. The present invention adopts a high-temperature sintering method to prepare a dense ceramic shell on the outer layer of the heat storage composite core material, which can prevent the leakage of molten salt, so that more molten salt can be loaded and the heat storage density can be improved; the carbon material, the molten salt and the external heat exchange medium are completely isolated, so as to avoid the high-temperature oxidation of the carbon material, prolong the life of the PCM, avoid the molten salt from contaminating the heat exchange medium, and greatly reduce the moisture absorption rate of the heat storage material. After adding a layer of porous carbon between the shell and the molten salt area, the expansion and deformation of the molten salt when heated can be absorbed to avoid the rupture of the dense shell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-temperature heat storage materials. Background Art

[0002] Phase change heat storage has attracted much attention due to its high energy density, quasi-isothermal heat storage and release process, and reasonable cost. Molten salt is widely used due to its high stability and low cost, but it needs to be packaged to stabilize its shape before it can be used in heat storage systems. The mixing-cold pressing-sintering process is a packaging method suitable for industrial mass production. This process mixes molten salt powder with porous material particles, compresses them into a mixture, and heats them in a high-temperature furnace to near the molten salt phase change temperature (200℃-900℃). After sintering for a certain period of time, a shape-stable composite phase change material (ss-PCM) is obtained.

[0003] The document "L. Sang, F. Li, Y. Xu, Form-stable ternary carbonates / MgO composite material for high temperature thermal energy storage, Sol. Energy. 180 (2019) 1–7" discloses a ss-PCM formed by sintering a mixture of ternary carbonate and MgO. The article points out that ss-PCM relies on the melted molten salt to sinter the molten salt and ceramic particles together, and the capillary action of the gaps between the ceramic particles adsorbs the molten salt to prevent leakage. Therefore, when the mass ratio of molten salt / MgO is higher than 4:6, the molten salt will leak. When the ratio is 7:3, the shape of the material cannot even remain stable. Only when the ratio is 3:7 will the molten salt not leak. This results in too little molten salt content in the ss-PCM and a low heat storage density.

[0004] The literature "Q.Yu, C.Zhang, Y.Lu, Q.Kong, H.Wei, Y.Yang, Q.Gao, Y.Wu, A.Sciacovelli, Comprehensive performance of composite phase change materials based oneutectic chloride with SiO2 nanoparticles and expanded graphite for thermal energy storage system, Renew.Energy.172(2021)1120–1132" improves the thermal conductivity of ss-PCM by adding carbon materials such as expanded graphite (EG), but EG will oxidize at high temperatures, which limits the operating temperature and service life of ss-PCM containing EG.

[0005] In addition, ss-PCM relies on porous pores to absorb molten salt. Although it can prevent molten salt leakage, it cannot prevent the volatilization of molten salt in ss-PCM at high temperatures. The volatilization of molten salt will cause the ss-PCM heat storage density to decrease and corrode the heat storage system. Therefore, it is necessary to develop a ss-PCM with high heat storage density, high thermal conductivity, and high reliability that can prevent leakage and volatilization at the same time. Summary of the invention

[0006] In order to solve the above problems, a ss-PCM with high heat storage density, high thermal conductivity and excellent reliability performance is developed. The present invention proposes a high-reliability high-temperature composite heat storage material and a preparation method thereof. The technical scheme adopted is as follows:

[0007] The invention discloses a high-reliability high-temperature composite heat storage material, which is composed of a dense ceramic shell and an internal heat storage composite core material, the main component of which is ceramic powder B; the heat storage composite core material is composed of molten salt, ceramic powder A and thermal conductivity enhancer, and the molten salt is adsorbed in the gap between the ceramic powder and the thermal conductivity enhancer;

[0008] The mass ratio of molten salt, ceramic powder A and thermal conductivity enhancer is (40-80):(5-60):(0-40); the molten salt is a single-component salt or a multi-component eutectic salt that will not decompose at the sintering temperature of ceramic powder A or ceramic powder B; the ceramic powder A is selected from MgO, SiC, diatomaceous earth and SiO2, and has a particle size of 1 to 100 μm; the ceramic powder B is selected from SiC, AlN, Al2O3 and Si3N4, and has a particle size of 1000 mesh to 3000 mesh.

[0009] The thermal conductivity enhancer is preferably one of graphite powder, carbon fiber powder, graphite oxide, graphene, biochar powder, expanded graphite, SiC and AlN.

[0010] The thickness of the ceramic shell in the present invention is preferably 2 to 6 mm.

[0011] The method for preparing a high-reliability high-temperature composite heat storage material comprises the following specific steps:

[0012] 1) Preparing a cold pressed block: mixing a molten salt, a ceramic powder A, and a thermal conductivity enhancer in a mass ratio of (40-80):(5-60):(0-40), and pressing the mixture in a tablet press at a molding pressure of 10-100 MPa to obtain a cold pressed block; the molding pressure is the ratio of the tablet press cylinder pressure to the sample cross-sectional area; the ceramic powder A is selected from MgO, SiC, diatomaceous earth, and SiO2, and has a particle size of 1 to 100 μm;

[0013] 2) preparing ceramic powder: weighing ceramic powder raw materials according to 55-80wt% ceramic powder B, 15-45wt% flux, 0.5-2wt% binder and 1-3wt% deionized water, and mixing the above raw materials in a ball mill for 0.5 hour; ceramic powder B is selected from SiC, AlN, Al2O3 and Si3N4, and the particle size is 1000 mesh to 3000 mesh;

[0014] 3) Compression molding: a layer of ceramic powder is pre-laid on the bottom of the mold, and then the cold pressed block is placed in the center of the mold, and the gap between the mold and the cold pressed block is filled with ceramic powder and does not exceed the cold pressed block. The composite heat storage material embryo with a ceramic shell is obtained by compression molding. The molding pressure is 50-100MPa and is higher than the molding pressure of the cold pressed block; the width of the gap is adjusted according to the thickness of the ceramic shell;

[0015] 4) High temperature sintering: The green embryo is placed in a high temperature furnace for high temperature sintering, and then naturally cooled to room temperature to obtain a high reliability high temperature composite heat storage material.

[0016] The preferred method of medium-high temperature sintering in step 4) is: placing the green embryo in a high-temperature furnace, heating it to 50-200°C above the melting point of the molten salt at a rate of 2-3°C / min, and the lower heating rate is to avoid rapid expansion of the solid phase molten salt; then continue to heat it to 700-1200°C at a rate of 5°C / min and keep it warm for 1-3 hours to sinter the shell densely, and then naturally cool it to room temperature to obtain a high-temperature composite heat storage material.

[0017] In step 3), the flux is preferably one or more of potassium feldspar, sodium feldspar, glass frit, and kaolin, and the adhesive is sodium carboxymethyl cellulose, sodium polyacrylate, or polyvinyl alcohol.

[0018] Preferably, in order to avoid the ceramic shell from being cracked due to the thermal expansion of the molten salt during use, a 0.5-2 mm porous carbon layer is further provided between the ceramic shell and the internal heat storage composite core material to absorb the thermal expansion of the molten salt. The porous carbon is obtained by carbonizing a resin with a high carbon residue rate. The preparation method thereof is as follows:

[0019] 1) Preparing a cold pressed block: mixing a molten salt, a ceramic powder A, and a thermal conductivity enhancer in a mass ratio of (40-80):(5-60):(0-40), and pressing the mixture in a tablet press at a molding pressure of 10-100 MPa to obtain a cold pressed block; the molding pressure is the ratio of the tablet press cylinder pressure to the sample cross-sectional area; the ceramic powder A is selected from MgO, SiC, diatomaceous earth, and SiO2, and has a particle size of 1 to 100 μm.

[0020] 2) Immerse the cold pressed block in high carbon residue resin, evenly coat the surface of the cold pressed block with a layer of high carbon residue resin of 0.5-2 mm thick, and solidify the cold pressed block;

[0021] 3) preparing ceramic powder: weighing ceramic powder raw materials according to 55-80wt% ceramic powder B, 15-45wt% flux, 0.5-2wt% binder and 1-3wt% deionized water, and mixing the above raw materials in a ball mill for 0.5 hour; ceramic powder B is selected from SiC, AlN, Al2O3 and Si3N4, and the particle size is 1000 mesh to 3000 mesh;

[0022] 4) Compression molding: a layer of ceramic powder is pre-laid on the bottom of the mold, and then the cold pressed block is placed in the center of the mold, and the gap between the mold and the cold pressed block is filled with ceramic powder and does not exceed the cold pressed block. The composite heat storage material embryo with a ceramic shell is obtained by compression molding. The molding pressure is 50-100MPa and is higher than the molding pressure of the cold pressed block.

[0023] 5) High temperature sintering: The green embryo is placed in a high temperature furnace for high temperature sintering, and then naturally cooled to room temperature to obtain a high reliability high temperature composite heat storage material.

[0024] Step 5) The preferred method of medium-high temperature sintering is: place the green body in a high-temperature furnace, heat it to 500°C at 2-3°C / min and keep it at this temperature for 2-4 hours to completely carbonize the resin. Then heat it to 700-850°C at 5°C / min and keep it at this temperature for 1-3 hours to sinter the shell to make it dense, and then naturally cool it to room temperature to obtain a high-reliability high-temperature composite heat storage material.

[0025] The high carbon residue resin used in step 2) is preferably phenolic resin or epoxy resin.

[0026] Beneficial effects of the present invention:

[0027] 1. With a dense ceramic shell, even if the mass fraction of the ceramic phase in the composite PCM is low, the molten salt will not leak, and it can load more molten salt to increase the heat storage density; the molten salt will not volatilize at high temperatures.

[0028] 2. Completely isolate the carbon material, molten salt and external heat exchange medium, avoiding high-temperature oxidation of the carbon material, extending the life of the CPCM, preventing molten salt from contaminating the heat exchange medium, and greatly reducing the moisture absorption rate of the heat storage material.

[0029] 3. There is a layer of porous carbon between the outer shell and the molten salt area, which can absorb the expansion and deformation of the molten salt when heated and avoid the rupture of the outer shell.

[0030] 4. Composite materials are molded by compression molding, and batch production has high consistency. Only one sintering is required, and the process is simple and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram of the structure of the high-reliability, high-temperature composite heat storage material obtained in Example 2 of the present invention.

[0032] Figure 2 This is a scanning electron microscope photograph of the interface between different regions of the high-reliability high-temperature composite heat storage material obtained in Example 2 of the present invention. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is further explained and illustrated in the form of specific embodiments below. The following embodiments are only preferred embodiments of the present invention.

[0034] Example 1

[0035] 1) NaCl and MgO (particle size 10 μm) were mixed in a mass ratio of 6:4 and compressed in a tablet press at a molding pressure of 60 MPa.

[0036] 2) Preparation of ceramic powder: 70 wt% SiC (particle size 2000 mesh), 22 wt% potassium feldspar, 1 wt% sodium carboxymethyl cellulose and 2 wt% deionized water were mixed in a ball mill for 2 hours.

[0037] 3) Pre-lay a layer of ceramic powder in the mold, then place the cold pressed block in the center of the mold, with a gap of 3mm between it and the inner surface of the mold; pour a certain mass of ceramic powder into the mold again, and press it again with a molding pressure of 80MPa. After the pressure is released, take it out to obtain a composite heat storage material embryo with a ceramic shell. .

[0038] 4) The green embryo is placed in a high-temperature furnace, and the temperature is raised to 900°C at 3°C / min, and then raised to 1200°C at 5°C / min and kept at this temperature for 2 hours to sinter the outer shell to make it dense. After naturally cooling to room temperature, a high-reliability high-temperature composite heat storage material is obtained.

[0039] After testing, the performance of the high-temperature composite heat storage material obtained in Example 1 is as follows: working temperature 700-900°C, heat storage density 401.2KJ / kg, thermal conductivity 6.7W / m·K, fine cracks after 800 hot and cold cycles, mass loss rate 1.7%, and thermal conductivity decay 3.8%.

[0040] Example 2

[0041] 1) Mix magnesium chloride, potassium chloride and sodium chloride in a mass ratio of 5:2:3, ball mill them in a ball mill for 40 minutes, heat them in a muffle furnace until they are completely melted, and keep them warm for 60 minutes to obtain eutectic salt. After cooling to room temperature, grind the mixture thoroughly to obtain eutectic salt powder, the melting temperature of which is 385°C.

[0042] 2) The eutectic salt powder, MgO (particle size 10 μm), and expanded graphite were mixed in a mass ratio of 7:2:1, and compressed in a tablet press at a molding pressure of 40 MPa.

[0043] 3) Preparation of ceramic powder: 65 wt% SiC (particle size 2000 mesh), 25 wt% glass frit, 7% kaolin, 1 wt% sodium carboxymethyl cellulose and 2 wt% deionized water were mixed in a ball mill for 0.5 hour.

[0044] 4) The cold pressed block was immersed in phenolic resin, so that a layer of resin with a thickness of 2 mm was evenly coated on its surface, and the resin was cured by heating at 80° C. for 6 hours.

[0045] 5) Pre-spread a layer of ceramic powder in the mold, then place the cold pressed block coated with a resin shell in the center of the mold, with a gap of 5 mm from the inner surface of the mold; pour the ceramic powder into the mold again and cover the cold pressed block, and press mold again at a molding pressure of 80 MPa. After depressurization, take out and obtain a composite heat storage material embryo with a ceramic shell.

[0046] 6) Place the green embryo in a high-temperature furnace, raise the temperature to 500°C at 3°C / min and keep it at this temperature for 3 hours to completely carbonize the resin, then raise the temperature to 700°C at 5°C / min and keep it at this temperature for 2 hours to sinter the shell densely, and naturally cool to room temperature to obtain a high-reliability high-temperature composite heat storage material.

[0047] The lower heating rate during the sintering process is to avoid the rapid expansion of the molten salt during the sintering stage; the long-term heat preservation at 500℃ is to completely carbonize the resin. At this time, the ceramic shell has not yet been sintered densely, and the gas discharged by carbonization can be discharged smoothly. After further heating, no gas will be discharged to avoid affecting the sintering density of the shell. At the set sintering temperature, it can be ensured that the thermal conductivity enhancer will not oxidize.

[0048] The structure of the high-reliability high-temperature composite heat storage material prepared in this embodiment is as follows Figure 1As shown, the outside is a dense ceramic shell 1 with a thickness of 5 mm, the inside is a molten salt area 3 sintered into a composition of molten salt / MgO / EG, and there is a layer of porous carbon 2 in between.

[0049] Figure 2 The scanning electron microscope photograph of the interface between different regions of the high-performance composite phase change material shows that the ceramic shell 1 has a dense structure, and the porous carbon layer 2 is in close contact with the ceramic shell 1 and the molten salt region 3 without any gap.

[0050] After testing, the performance of the high-temperature composite heat storage material obtained in this Example 1 is as follows: working temperature 300-500°C, heat storage density 356.5KJ / kg, thermal conductivity 8.1W / m·K, no deformation and cracking after 1000 hot and cold cycles, mass loss rate 1.12%, and thermal conductivity attenuation 4.7%.

[0051] Comparative Example:

[0052] 1) Mix magnesium chloride, potassium chloride and sodium chloride in a mass ratio of 5:2:3, ball mill them in a ball mill for 40 minutes, heat them in a muffle furnace until they are completely melted, and keep them warm for 60 minutes to obtain eutectic salt. After cooling to room temperature, grind the mixture thoroughly to obtain eutectic salt powder.

[0053] 2) Eutectic salt powder, MgO (particle size 10 μm), and expanded graphite are mixed in a mass ratio of 5:3:2, and compressed in a tablet press at a molding pressure of 60 MPa to obtain a green embryo.

[0054] 3) placing the green embryo in a high temperature furnace, heating it to 500°C at a rate of 2°C / min and keeping it warm, and then naturally cooling it to room temperature to obtain a composite heat storage material.

[0055] After testing, the performance of the high-temperature composite heat storage material obtained in the comparative example is as follows: working temperature 300-500°C, heat storage density 289.2KJ / kg, thermal conductivity 8.85W / m·K, cracking after 500 cycles, mass loss rate 10.2%, and thermal conductivity decay 18.2%.

[0056] The present invention prepares a high-temperature composite heat storage material with a ceramic shell through a one-time molding and sintering method. Compared with the comparative example, the ceramic shell significantly increases the reliability of the heat storage material, and the porous carbon layer further improves the reliability of the heat storage material by absorbing the thermal expansion of the molten salt.

Claims

1. A high-reliability, high-temperature composite heat storage material, characterized in that: The material consists of a dense ceramic shell and an internal heat storage composite core material; the heat storage composite core material is composed of molten salt, ceramic powder A and a thermal conductivity enhancer, and the molten salt is adsorbed in the gap between the ceramic powder A and the thermal conductivity enhancer; the ceramic shell is made of 55-80wt% of ceramic powder B, 15-45wt% of flux, 0.5-2wt% of adhesive and 1-3wt% of deionized water as ceramic powder raw materials; The mass ratio of molten salt, ceramic powder A and thermal conductivity enhancer is (40-80): (5-60): (0-40); the molten salt is a single-component salt or a multi-component eutectic salt that will not decompose at the sintering temperature of ceramic powder A or ceramic powder B; the ceramic powder A is selected from MgO, SiC, diatomaceous earth or SiO2, and has a particle size of 1-100 μm; the ceramic powder B is selected from SiC, AlN, Al2O3 or Si3N4, and has a particle size of 1000 mesh to 3000 mesh; A 0.5-2 mm porous carbon layer is also arranged between the ceramic shell and the internal heat storage composite core material to absorb the thermal expansion of the molten salt. The porous carbon is obtained by carbonizing a resin with a high carbon residue rate.

2. The high-reliability, high-temperature composite heat storage material according to claim 1, characterized in that: The thickness of the ceramic shell is 2~6mm.

3. The high-reliability, high-temperature composite heat storage material according to claim 1, characterized in that: The thermal conductivity enhancer is one of graphite powder, carbon fiber powder, graphite oxide, graphene, biochar powder, expanded graphite, SiC and AlN.

4. A method for preparing the high-reliability high-temperature composite heat storage material as claimed in claim 1, characterized in that: The specific steps of this method are as follows: 1) Preparing a cold pressed block: mixing molten salt, ceramic powder A, and thermal conductivity enhancer in a mass ratio of (40-80): (5-60): (0-40), and pressing in a tablet press at a molding pressure of 10-100 MPa to obtain a cold pressed block; the molding pressure is the ratio of the tablet press cylinder pressure to the sample cross-sectional area; the ceramic powder A is selected from MgO, SiC, diatomaceous earth or SiO2; 2) Immerse the cold pressed block in high carbon residue resin, evenly coat its surface with a layer of high carbon residue resin with a thickness of 0.5-2 mm, and solidify it; 3) preparing ceramic powder: weighing ceramic powder raw materials according to 55-80wt% ceramic powder B, 15-45wt% flux, 0.5-2wt% binder and 1-3wt% deionized water, and mixing the above raw materials in a ball mill for 0.5 hour; ceramic powder B is selected from SiC, AlN, Al2O3 or Si3N4, and the particle size is 1000 mesh to 3000 mesh; 4) Compression molding: a layer of ceramic powder is pre-laid on the bottom of the mold, and then the cold pressed block is placed in the center of the mold, and the gap between the mold and the cold pressed block is filled with ceramic powder and does not exceed the cold pressed block. The composite heat storage material green body with a ceramic shell is obtained by compression molding. The molding pressure is 50-100MPa and is higher than the molding pressure of the cold pressed block. 5) The green body is placed in a high-temperature furnace for high-temperature sintering, and then naturally cooled to room temperature to obtain a high-reliability high-temperature composite heat storage material.

5. The method for preparing a high-reliability, high-temperature composite heat storage material according to claim 4, characterized in that: Step 5) The method of medium-high temperature sintering is: heating at 2-3°C / min to 50-200°C above the melting point of the molten salt, and then continuing to heat at 5°C / min to 700-1200°C and keeping the temperature for 1-3 hours to sinter the ceramic shell to make it dense.

6. The method for preparing a high-reliability, high-temperature composite heat storage material according to claim 4, characterized in that: In step 3), the flux is one or more of potassium feldspar, sodium feldspar, glass frit, and kaolin; and the adhesive is sodium carboxymethyl cellulose, sodium polyacrylate, or polyvinyl alcohol.

7. The method for preparing a high-reliability high-temperature composite heat storage material according to claim 4, characterized in that: The high carbon residue resin used in step 2) is phenolic resin or epoxy resin.