A resin coating liquid suitable for oil lubrication and its preparation method and application

By using bulk molybdenum disulfide and graphite of specific proportions and particle sizes in resin coating liquids, as well as a small layer of molybdenum disulfide, the high friction coefficient and low impact resistance of existing coatings under oil lubricating conditions is solved. , achieving low friction, wear and oil resistant coating effects.

CN116535933BActive Publication Date: 2024-11-15SHANGHAI UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310567256.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-15
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

The existing polymer resin coating has high friction coefficient and poor impact resistance under oil lubricating conditions, resulting in low coating life and insufficient oil resistance and wear resistance.

Method used

Using bulk molybdenum disulfide and graphite of specific proportions and particle sizes as bulk solid lubricants, combined with a small layer of molybdenum disulfide and an appropriate amount of organic solvent and curing agent, a uniform resin coating liquid is formed through ultrasonic dispersion and shearing treatment. , sprayed on a metal substrate to improve the impact resistance and oil resistance of the coating.

Benefits of technology

The friction coefficient of the coating is significantly reduced, the impact resistance and oil resistance are improved, the service life of the coating is extended, and the excellent performance is maintained after long soaking in the lubricating oil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116535933B_ABST
    Figure CN116535933B_ABST
Patent Text Reader

Abstract

The present invention relates to a resin coating liquid suitable for oil lubrication, and a preparation method and application thereof; the resin coating liquid comprises epoxy resin, 15-25wt% of a bulk solid lubricant, an organic solvent and a curing agent; the bulk solid lubricant is composed of bulk molybdenum disulfide and graphite in a mass ratio of 7:4-6; the average particle size of the bulk molybdenum disulfide is 0.1-20μm, and the average particle size of the graphite is 0.1-10μm; the preparation method is: uniformly mixing the components according to a certain proportion and a certain order of adding materials to obtain the resin coating liquid; the application is: spraying the resin coating liquid on the surface of a metal substrate, curing, and obtaining a coating. The method of the present invention is simple, and the obtained coating has a small friction coefficient, excellent impact resistance and oil resistance, and a strong ability to bond with the metal substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings and relates to a resin coating liquid suitable for oil lubrication and a preparation method and application thereof. Background Art

[0002] Solid lubricating coatings are widely used on high-speed, heavy-loaded friction pairs such as gears, and can play an emergency dry lubrication effect in the process of lubricant loss, preventing the friction pair from failing due to high heat generated by friction. The polymer-based solid lubricating coating relies on the resin matrix to bond the substrate and provide protection for the mechanical properties of the coating. However, the dispersion of the bulk wear-resistant filler in the coating causes defects in the coating and reduces the impact resistance. The wear of the coating is often too severe, resulting in a short life. Past patents involving polymer resin matrices (200810203993.7) performed poorly in oil resistance and impact resistance (impact strength of only 50cm). In patents that attempt to use graphene as a wear-resistant additive (such as 201910375103.9), the lowest dry friction coefficient can only reach 0.2. It is of great significance to reduce the negative impact of bulk fillers on the strength of the resin matrix and to enhance the performance of the coating. Summary of the invention

[0003] The purpose of the present invention is to solve the problems existing in the prior art and to provide a resin coating liquid suitable for oil lubrication and a preparation method and application thereof.

[0004] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0005] A resin coating liquid suitable for oil lubrication, comprising epoxy resin, bulk solid lubricant, organic solvent and curing agent;

[0006] The content of bulk solid lubricant is 15-25wt%; when the content of bulk solid lubricant is too small (the proportion of resin matrix is ​​large), the friction reduction and wear resistance of the formed coating is poor; when the content of bulk solid lubricant is too large, the ability of the formed coating to bond with the metal matrix is ​​insufficient, and cohesive failure is likely to occur, which leads to the destruction of the coating;

[0007] The bulk solid lubricant is composed of bulk molybdenum disulfide and graphite in a mass ratio of 7:4-6; the average particle size of the bulk molybdenum disulfide is 0.1-20 μm, and the average particle size of the graphite is 0.1-10 μm.

[0008] One of the purposes of the present invention is to reduce the friction coefficient of the coating, which is specifically solved by designing a bulk solid lubricant composed of a specific ratio and a specific size of blocks of molybdenum disulfide and graphite. The principle is as follows:

[0009] The macroscopic mechanism of solid filler lubrication is explained as the interlayer van der Waals force between graphite and bulk MoS2 is small, which makes them susceptible to shear force to produce slip and form a continuous transfer film, but the interlayer slip barriers of the two are different. According to research, in the process of mixed solid lubricating fillers forming a lubricating film, the number of layers of bulk MoS2 and graphite decreases with slip, and when the bulk MoS2-graphite layers transfer to each other, due to the non-commensurate contact of heterogeneous (different substances) (the term comes from structural superlubrication, this concept was proposed in 1991 and experimentally confirmed between nanographite sheets in 2004; the carbon atoms in graphite are periodically arranged in a hexagonal manner, forming an atomic-scale "peak-valley" landscape that looks like an egg tray in life; when the two graphite surfaces are in commensurate contact (every 60 degrees of rotation), the friction between the two graphite surfaces is the largest, and when the two graphite surfaces rotate relative to each other to non-commensurate contact, the friction will be extremely The earth is lowered; it is like two egg trays in contact with each other. When the rotation prevents them from "biting" each other, relative sliding is more likely to occur;) the friction force is reduced, and the interlayer slip barrier is much smaller than that of bulk MoS2-bulk MoS2 or graphite-graphite (assuming that the bulk MoS2 flakes are all A flakes and the graphite flakes are all B flakes. During the movement caused by shear, the number of flakes decreases. Bulk MoS2 and graphite are like two dozen different playing cards. During the shear process, the playing cards are inserted into each other and mixed, and the transfer of AB / BA flakes in this process is obviously easier than the movement of AA flakes or BB flakes, that is, the interlayer slip barrier is small), which is manifested as a reduction in the friction coefficient.

[0010] So far, structural superlubricity is still formed under harsh conditions, and macroscopic friction cannot perfectly demonstrate the currently defined superlubricity. However, the reduction of particle size and reasonable proportion will theoretically help to increase the possibility of heterogeneous non-commensurate contact in macroscopic friction and reduce the friction coefficient.

[0011] The present invention controls the average particle size of the bulk molybdenum disulfide to be 0.1-20 μm, and the average particle size of the graphite to be 0.1-10 μm; if the average particle size of the bulk molybdenum disulfide and the graphite is too large, the filler will settle significantly during the resin curing process, eventually resulting in uneven coating, which is not conducive to reducing the friction coefficient of the coating; if the average particle size of the bulk molybdenum disulfide and the graphite is too small, they will easily agglomerate, which is not conducive to the quality of the coating;

[0012] Under microscopic conditions, if graphite and bulk molybdenum disulfide slip against each other, the slip barrier between the layers will indeed decrease, but under macroscopic conditions, the different proportions of the two substances added directly affect the probability of the occurrence of this phenomenon under microscopic conditions. Therefore, the specific parameter values ​​must be tested to find the optimal value or reasonable value; the present invention controls the mass ratio of bulk molybdenum disulfide and graphite to 7:4-6; if the proportion of bulk molybdenum disulfide is too large, the brittleness of the coating will increase, and the probability of fatigue wear during the friction process will increase; if it is too small, the texture will become soft, the probability of adhesive wear will increase, and the wear resistance of the coating will drop sharply; both are not conducive to reducing the friction coefficient of the coating and ensuring the long life of the coating.

[0013] In addition, bulk molybdenum disulfide and graphite themselves have a synergistic effect. Pure bulk molybdenum disulfide performs well in a high vacuum environment but is easily oxidized by water and oxygen to molybdenum trioxide (high friction coefficient). Graphite has a lower friction coefficient under atmospheric conditions. During the shear slip process, the filler is sheared and dispersed on the surface. If the sheared graphite is transferred to the top of the bulk molybdenum disulfide, it can protect the bulk molybdenum disulfide from contact with water and oxygen on the surface, and ultimately avoid oxidation.

[0014] As the preferred technical solution:

[0015] As described above, in a resin coating liquid suitable for oil lubrication, the average particle size of bulk molybdenum disulfide is 0.1 to 5 μm, and the average particle size of graphite is 0.1 to 5 μm. This can make the distribution of bulk molybdenum disulfide and graphite in the resin more uniform, reducing the probability of surface defects and internal defects in the coating.

[0016] The resin coating liquid suitable for oil lubrication as described above further comprises 3 to 8 wt % of a few-layer molybdenum disulfide, and the average particle size of the few-layer molybdenum disulfide is 50 nm to 0.5 μm.

[0017] The second purpose of the present invention is to enhance the impact resistance and oil resistance of the coating (the present invention reflects the oil resistance of the coating by testing the pencil hardness and adhesion of the coating after 30 days of oil immersion), which is specifically solved by adding a few layers of molybdenum disulfide. The principle is as follows:

[0018] Few-layer molybdenum disulfide is an inorganic functional filler, which is insoluble in resin, so the coating formed is a two-phase structure (resin and filler). Compared with bulk molybdenum disulfide of the same mass and large particle size, it has a higher specific surface area dispersed in the resin and can better combine with the resin. In previous studies, the reinforcement of the resin by low-content fillers is directly related to the volume fraction. When the filler content increases, which is the case in the present invention, the reinforcement of the resin is related to the filler particle size. The smaller the particle size, the better the reinforcement effect (improvement of impact resistance), which can play a role in transferring loads and stresses between resins. When the filler content is high, the large-particle filler (bulk molybdenum disulfide) will act as a defect or stress concentration point. Few-layer molybdenum disulfide has a very high in-plane strength, and its Young's modulus is comparable to that of graphene. It is easier to disperse evenly with the resin matrix than large-particle bulk fillers, and can be used as a reinforcement for the resin matrix. Compared with few-layer MoS2, bulk MoS2 has a larger particle size and relies on interlayer slippage to act as a lubricant in coatings, but it is prone to local defects as a filler. Liquid-phase exfoliated few-layer MoS2 is neither hydrophilic nor oleophilic. When added to coatings as a filler, it is more oleophobic (improved oil resistance) than the resin matrix.

[0019] In addition, few-layer molybdenum disulfide has fewer defect sites in the surface than graphene, and its thermal properties and lubrication performance in oil environment are more stable than graphene. Most importantly, in addition to acting as an extremely fine filler to disperse stress in the resin for reinforcement, few-layer molybdenum disulfide, as a transition metal compound, has a metallic bond with the metal substrate covered by the coating, providing a stronger ability to bond with the metal substrate, and significantly improving the coating's adhesion.

[0020] In addition, by adding a suitable amount of a small layer of molybdenum disulfide to the coating, the aforementioned reduction in friction coefficient due to non-commensurate contact will be more likely to occur during the stage of transfer film generation.

[0021] The present invention controls the content of the few-layer molybdenum disulfide to be 3-8wt% because the few-layer molybdenum disulfide is also added as a solid phase material, and too much addition will also lead to an increase in the total content of the coating filler, resulting in a decrease in strength; too little addition will not significantly improve its mechanical enhancement performance and friction reduction and wear resistance; the present invention controls the average particle size of the few-layer molybdenum disulfide to be 50-500nm because the few-layer molybdenum disulfide with too large a particle size will produce autonomous shrinkage and curling due to its own large surface energy, which is not conducive to the occurrence of slip, and too small a particle size will result in a high preparation cost, and it tends to aggregate autonomously and is not easy to preserve for a long time.

[0022] As described above, a resin coating liquid suitable for oil lubrication, the preparation process of a few-layer molybdenum disulfide is as follows: after the block molybdenum disulfide is dried (temperature is 80°C, time is 2 to 4 hours), it is added to N-methylpyrrolidone (N-methylpyrrolidone can be replaced by 80% isopropanol solution, but N-methylpyrrolidone is the solvent with the surface energy closest to molybdenum disulfide and the highest stripping effect) to obtain a dispersion with a concentration of 50 to 80 mg / ml, and ultrasonically treated at 250 to 600 W for 4 to 12 hours at 25 to 35°C to obtain a suspension containing a few-layer molybdenum disulfide, and post-treated (centrifuged at a speed of 10,000 rpm for 30 minutes to obtain an upper clear liquid, added 25% ethanol solution for repeated centrifugation and washing until the N-methylpyrrolidone is completely replaced, and the centrifugal precipitate is dispersed in a 25% ethanol solution and then freeze-dried) to obtain a few-layer molybdenum disulfide.

[0023] The resin coating liquid suitable for oil lubrication as described above further comprises 0.1 to 1 wt % of additives.

[0024] The resin coating liquid suitable for oil lubrication as described above, the additive is dispersant Tech-6325 and / or leveling agent MHC60-6100.

[0025] The resin coating liquid suitable for oil lubrication as described above has an epoxy resin content of 20 to 40 wt %, an organic solvent content of 20 to 65 wt %, and a curing agent content of 1 to 5 wt %.

[0026] As described above, the resin coating liquid suitable for oil lubrication, the epoxy resin is bisphenol A epoxy resin YD-128 and / or bisphenol A resin KSR-177; the curing agent is dicyandiamide; the organic solvent is composed of acetone, 2-butanone, cyclohexanone and N,N-dimethylformamide, the volume ratio of acetone, 2-butanone and cyclohexanone is 2:1:1, and the mass ratio of N,N-dimethylformamide to the curing agent is 2-4:1. The present invention uses the boiling point reduction of the solvent miscible to regulate the volatilization rate of the organic solvent in the glue during the spraying process, and forms a uniform and flat resin glue layer in the spraying stage, wherein N,N-dimethylformamide is a good solvent for dicyandiamide with a boiling point of 153°C, which can help to evenly disperse the curing agent in the resin and avoid local excessive cross-linking.

[0027] The present invention also provides a method for preparing a resin coating liquid suitable for oil lubrication as described in any one of the above items, comprising the following steps:

[0028] (1) adding a curing agent to N,N-dimethylformamide and shaking to obtain a clear solution;

[0029] (2) mixing the epoxy resin and the clarified solution uniformly to obtain a resin glue solution;

[0030] (3) After drying the bulk molybdenum disulfide and graphite (temperature is 80° C., time is 2 to 4 hours), the bulk molybdenum disulfide and graphite are mixed with resin glue, acetone, 2-butanone, cyclohexanone and additives, and ultrasonically dispersed for 30 to 60 minutes to obtain a mixed glue;

[0031] (4) filtering the mixed glue solution through a 300-800 mesh gauze (the purpose of this filtering step is to obtain finer filler particles with narrower particle size dispersion. The filler can also be directly sieved after drying to remove large particles of filler, and then the dispersion liquid and glue solution are added) to obtain a filtrate;

[0032] (5) Add a few layers of molybdenum disulfide to the filtrate, and then ultrasonicate for 30 to 60 minutes after shearing to obtain a resin coating liquid suitable for oil lubrication.

[0033] The present invention also provides an application of a resin coating liquid suitable for oil lubrication as described in any of the above items, wherein the resin coating liquid is stirred and ultrasonically pre-dispersed for 20 minutes, sprayed on the surface of the metal substrate with an air spray gun, and cured at 165-175°C for 50-70 minutes to obtain a coating.

[0034] As the preferred technical solution:

[0035] For the application described above, the coating thickness is 20-30 μm, the impact resistance height is 40-45 cm, the friction coefficient of the coating is 0.03-0.045, and the wear rate of the coating is 0.260×10 -6 ~0.430×10 -6 mm 3 / (N·m), the adhesion of the coating is level 0, and the pencil hardness is 5H. After 30 days of oil immersion, the adhesion of the coating is level 0-1, and the pencil hardness is 3-4H.

[0036] Beneficial effects:

[0037] (1) The resin coating prepared by the present invention has high impact resistance, adhesion and pencil hardness on the metal substrate, and also has excellent low friction coefficient (the dry friction coefficient of the prior art can only reach 0.2 at the lowest, and the friction coefficient of the coating of the present invention is further reduced by more than one order of magnitude compared with the prior art) and low wear rate. The above properties remain unchanged after being immersed in lubricating oil for thirty days;

[0038] (2) The preparation of few-layer molybdenum disulfide by the present invention is simple and efficient, and the key solvent can be recycled, which is green and environmentally friendly;

[0039] (3) The preparation steps of the resin coating liquid in the present invention are simple, and the curing is fast and efficient. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1This is a scanning image of the wear scar of the coating prepared in Example 5 under a 350X scanning electron microscope;

[0041] Figure 2 The scanning image and EDS spectrum of the wear scar of the coating prepared in Example 5 under a 4500X scanning electron microscope; in the figure, (a) is a scanning image of the wear scar under a 4500X scanning electron microscope, and (b), (c) and (d) are all EDS spectra at the white frame in (a); it can be seen from the figure that the EDS spectrum shows that there is enrichment of Mo, S and Si elements in the lower right corner of the white frame. Combined with the image, it can be seen that regular molybdenum disulfide sheets are formed on the exposed surface in the lower right corner of the white frame, replacing the friction pair formed between the resin and the metal steel ring, thereby reducing the friction coefficient; smaller-sized few-layer molybdenum disulfide can be seen below the white frame, which is coated with resin, disperses stress and strengthens the coating, thereby reducing the wear rate; part of the few-layer molybdenum disulfide is exposed on the surface during the friction process, further reducing the friction coefficient;

[0042] Figure 3 This is the XRD image of bulk MoS2 before and after ultrasonic stripping; by comparing the peak position with the standard PDF card, it can be seen that the crystal structure of bulk MoS2 is 2H-type MoS2, which is the most stable MoS2 crystal structure with the smallest slip barrier. After ultrasonic stripping, the intensity of each peak decreases significantly, indicating that the orientation degree of MoS2 in the direction of the crystal plane is reduced, that is, it is stripped from top to bottom. The peak has not completely disappeared, indicating that it has not been completely stripped to a single layer, proving the successful preparation of few-layer MoS2. DETAILED DESCRIPTION

[0043] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0044] Sources of related substances in the examples:

[0045] Bisphenol A epoxy resin YD-128: The manufacturer is Kunshan Guodu Chemical Co., Ltd.

[0046] Bisphenol A resin KSR-177: Manufacturer: Kunshan Guodu Chemical Co., Ltd.

[0047] Bulk molybdenum disulfide: The manufacturer is Shanghai Colloid Chemical Co., Ltd., the brand is MF-0;

[0048] Graphite: brand is SIAL, product number is NISTRM8541;

[0049] Dispersant Tech-6325: Manufacturer: Shanghai Tiger Polymer Technology Co., Ltd.;

[0050] Leveling agent MHC60-6100: The manufacturer is Shanghai Tiger Polymer Technology Co., Ltd.

[0051] Detection methods of relevant properties in the embodiments:

[0052] The coating is immersed in oil for 30 days, which means that the prepared coating is completely immersed in lubricating oil (manufacturer is Beijing Xingpu Fine Chemical, brand is RIPP550) at 25°C for 30 days;

[0053] Coating adhesion: Test coating adhesion according to standard GB 1720-79;

[0054] Coating pencil hardness: Test the coating pencil hardness according to standard GB / T 6739-2022;

[0055] Impact resistance height of coating: Test the impact resistance height of coating with reference to standard GB / T 1732-93;

[0056] Friction coefficient of coating: The resin coating liquid prepared in the embodiment is solidified on a Q235 carbon steel plate with a length, width and height of 25×7×4 mm to form a test block, and the test is carried out at 25°C using an M-2000J friction and wear tester in accordance with the standard GB / T 12444-2006. During the test, a peristaltic pump and an oil box are used for cyclic oil spray lubrication. The friction coefficient data are sampled every 0.1 second and recorded. The data with an error greater than 6 standard deviations are removed and the arithmetic mean of the remaining data is taken as the friction coefficient of the sample. The test ring is a GCr15 steel ring with a standard diameter of 36 mm equipped with the test machine. The test loads are 50N, 100N, 150N and 200N, respectively. Each load is tested for 30 minutes, and the linear speed of the steel ring is 0.42m / s.

[0057] Wear rate of coating: The resin coating liquid prepared in the embodiment was solidified on a Q235 carbon steel plate with a length, width and height of 25×7×4 mm to form a test block, and the test was carried out at 25°C using an M-2000J friction and wear tester in accordance with the standard GB / T 12444-2006 to obtain the wear volume and wear distance of the test block; wherein the test ring was a GCr15 steel ring with a standard diameter of 36 mm provided with the test machine, the test time was 30 min, and the linear speed of the steel ring was 0.42 m / s; then the wear rate of the coating was calculated according to the following formula:

[0058] W s =V s / L·F;

[0059] Where W s - Wear rate (mm 3 / (N·m)), V s - Wear volume (mm3 ), L-grinding distance (m), F-load (N);

[0060] Three parallel tests were performed and the arithmetic mean was taken.

[0061] Example 1

[0062] A method for preparing a resin coating liquid suitable for oil lubrication, the specific steps are as follows:

[0063] (1) Prepare materials:

[0064] acetone;

[0065] 2-Butanone;

[0066] Cyclohexanone;

[0067] N,N-dimethylformamide;

[0068] Epoxy resin: a mixture of bisphenol A epoxy resin YD-128 and bisphenol A resin KSR-177 in a mass ratio of 1:3;

[0069] Bulk solid lubricant: composed of bulk molybdenum disulfide and graphite in a mass ratio of 7:4; wherein the average particle size of the bulk molybdenum disulfide is 20 μm, and the average particle size of the graphite is 2 μm;

[0070] Curing agent: dicyandiamide;

[0071] Additives: a mixture of dispersant Tech-6325 and leveling agent MHC60-6100 in a mass ratio of 2:1;

[0072] Few-layer molybdenum disulfide: The preparation process is as follows: After drying the bulk molybdenum disulfide at 80°C for 2 hours, adding it to N-methylpyrrolidone to obtain a dispersion with a concentration of 50 mg / ml, ultrasonicating it at 30°C at a power of 250W for 12 hours to obtain a suspension containing few-layer molybdenum disulfide, and then centrifuging it at a speed of 10,000 rpm for 30 minutes to obtain a supernatant, adding 25% ethanol solution, repeatedly centrifuging and washing until N-methylpyrrolidone is completely replaced, and dispersing the centrifugal precipitate in 25% ethanol solution and then freeze-drying it to obtain few-layer molybdenum disulfide with an average particle size of 500 nm;

[0073] (2) Preparation of resin coating liquid:

[0074] (2.1) Add the curing agent to N,N-dimethylformamide and shake evenly to obtain a clear solution;

[0075] (2.2) mixing the epoxy resin and the clarified solution uniformly to obtain a resin glue solution;

[0076] (2.3) drying the bulk solid lubricant at 80° C. for 2 h, mixing it with the resin glue, acetone, 2-butanone, cyclohexanone and additives, and performing ultrasonic dispersion for 30 min to obtain a mixed glue;

[0077] (2.4) Filter the mixed glue solution through a 300-mesh gauze to obtain a filtrate;

[0078] (2.5) A few layers of molybdenum disulfide were added to the filtrate, and the filtrate was sheared at a shear rate of 1000 rpm for 10 min, followed by ultrasonication for 30 min to obtain a resin coating liquid suitable for oil lubrication.

[0079] In the finally obtained resin coating liquid suitable for oil lubrication, the volume ratio of acetone, 2-butanone and cyclohexanone is 2:1:1, the mass ratio of N,N-dimethylformamide to curing agent is 3:1, the content of the organic solvent composed of acetone, 2-butanone, cyclohexanone and N,N-dimethylformamide is 42.9wt%, the content of the bulk solid lubricant is 15wt%, the content of the few-layer molybdenum disulfide is 8wt%, the content of the additive is 0.1wt%, the content of the epoxy resin is 32wt%, and the content of the curing agent is 2wt%.

[0080] An application of a resin coating liquid suitable for oil lubrication, wherein the resin coating liquid prepared by the above method is ultrasonicated for 20 minutes, sprayed on the surface of a carbon steel sheet with an air spray gun at a pressure of 0.24 bar, and cured at 165° C. for 70 minutes to obtain a coating;

[0081] The thickness of the prepared coating is 24.39 μm, the impact resistance height is 41 cm, the friction coefficient is 0.043, and the wear rate is 0.427×10 -6 mm 3 / (N·m), the adhesion is level 0, the pencil hardness is 5H, and after 30 days of oil immersion, the adhesion is level 1, and the pencil hardness is 3H.

[0082] Comparative Example 1

[0083] A method for preparing a resin coating liquid is basically the same as that of Example 1, except that in step (1), the mass ratio of molybdenum disulfide to graphite in the bulk solid lubricant is 7:2.

[0084] An application of a resin coating liquid is basically the same as in Example 1, except that the resin coating liquid used is the resin coating liquid prepared in this comparative example;

[0085] The impact resistance height of the prepared coating is 34 cm, the friction coefficient is NA (the coating is worn through, and there is no average statistical value within 30 min), and the wear rate is 2.612×10 -6 mm 3 / (N·m), adhesion is level 0, and pencil hardness is 2H.

[0086] Compared with Example 1, Comparative Example 1 has decreased pencil hardness and impact resistance of the coating. This is because the molybdenum disulfide content in the bulk solid lubricant is too large, which makes the coating brittle. At the same time, due to the insufficient content of soft graphite, the coating cannot have sufficient wear resistance. The coating failed to pass the test time of 30 minutes in the test and was worn through to the substrate, with a high wear rate.

[0087] Example 2

[0088] A method for preparing a resin coating liquid suitable for oil lubrication, the specific steps are as follows:

[0089] (1) Prepare materials:

[0090] acetone;

[0091] 2-Butanone;

[0092] Cyclohexanone;

[0093] N,N-dimethylformamide;

[0094] Epoxy resin: a mixture of bisphenol A epoxy resin YD-128 and bisphenol A resin KSR-177 in a mass ratio of 1:2;

[0095] Bulk solid lubricant: composed of bulk molybdenum disulfide and graphite in a mass ratio of 7:6; the average particle size of the bulk molybdenum disulfide is 8μm, and the average particle size of the graphite is 5μm;

[0096] Curing agent: dicyandiamide;

[0097] Additives: a mixture of dispersant Tech-6325 and leveling agent MHC60-6100 in a mass ratio of 1:2;

[0098] Few-layer molybdenum disulfide: The preparation process is as follows: After drying the bulk molybdenum disulfide at 80°C for 2 hours, adding it to N-methylpyrrolidone to obtain a dispersion with a concentration of 60 mg / ml, ultrasonicating it at 30°C at a power of 350W for 10 hours to obtain a suspension containing few-layer molybdenum disulfide, and then centrifuging it at a speed of 10,000 rpm for 30 minutes to obtain a supernatant, adding 25% ethanol solution, repeatedly centrifuging and washing until N-methylpyrrolidone is completely replaced, and dispersing the centrifugal precipitate in 25% ethanol solution and then freeze-drying it to obtain few-layer molybdenum disulfide with an average particle size of 500 nm;

[0099] (2) Preparation of resin coating liquid:

[0100] (2.1) Add the curing agent to N,N-dimethylformamide and shake evenly to obtain a clear solution;

[0101] (2.2) mixing the epoxy resin and the clarified solution uniformly to obtain a resin glue solution;

[0102] (2.3) drying the bulk solid lubricant at 80° C. for 4 h, mixing it with the resin glue, acetone, 2-butanone, cyclohexanone and additives, and performing ultrasonic dispersion for 30 min to obtain a mixed glue;

[0103] (2.4) Filter the mixed glue solution through a 300-mesh gauze to obtain a filtrate;

[0104] (2.5) A few layers of molybdenum disulfide were added to the filtrate, and the filtrate was sheared at a shear rate of 1000 rpm for 10 min, followed by ultrasonic treatment for 60 min to obtain a resin coating liquid suitable for oil lubrication.

[0105] In the finally obtained resin coating liquid suitable for oil lubrication, the volume ratio of acetone, 2-butanone and cyclohexanone is 2:1:1, the mass ratio of N,N-dimethylformamide to curing agent is 2.5:1, the content of the organic solvent composed of acetone, 2-butanone, cyclohexanone and N,N-dimethylformamide is 21wt%, the content of the bulk solid lubricant is 25wt%, the content of the few-layer molybdenum disulfide is 8wt%, the content of the additive is 1wt%, the content of the epoxy resin is 40wt%, and the content of the curing agent is 5wt%.

[0106] An application of a resin coating liquid suitable for oil lubrication, wherein the resin coating liquid prepared by the above method is ultrasonicated for 20 minutes, sprayed on the surface of a carbon steel sheet with an air spray gun at a pressure of 0.24 bar, and cured at 170° C. for 60 minutes to obtain a coating;

[0107] The thickness of the prepared coating is 21.98 μm, the impact resistance height is 43 cm, the friction coefficient is 0.041, and the wear rate is 0.381×10 -6 mm 3 / (N·m), the adhesion is level 0, the pencil hardness is 5H, and after 30 days of oil immersion, the adhesion is level 0 and the pencil hardness is 4H.

[0108] Comparative Example 2

[0109] A method for preparing a resin coating liquid is basically the same as that of Example 2, except that in step (1), the mass ratio of molybdenum disulfide to graphite in the bulk solid lubricant is 1:1.

[0110] An application of a resin coating liquid is basically the same as in Example 2, except that the resin coating liquid used is the resin coating liquid prepared in this comparative example;

[0111] The impact resistance height of the prepared coating is 36 cm, the friction coefficient is NA (the coating is worn through, and there is no average statistical value within 30 min), and the wear rate is 13.368×10 -6 mm 3 / (N·m), adhesion is level 2, and pencil hardness is 2H.

[0112] Compared with Example 2, all performance indicators of Comparative Example 2 have been greatly reduced. This is because the graphite content is relatively high and the molybdenum disulfide content is too small, which causes the texture to become soft, the probability of adhesive wear increases, and the wear resistance of the coating decreases sharply; at the same time, the friction reduction and wear resistance of graphite in an oil environment are poor, and the coating loses drastically after oil immersion, resulting in coating failure.

[0113] Example 3

[0114] A method for preparing a resin coating liquid suitable for oil lubrication, the specific steps are as follows:

[0115] (1) Prepare materials:

[0116] acetone;

[0117] 2-Butanone;

[0118] Cyclohexanone;

[0119] N,N-dimethylformamide;

[0120] Epoxy resin: bisphenol A epoxy resin YD-128;

[0121] Bulk solid lubricant: composed of bulk molybdenum disulfide and graphite in a mass ratio of 7:5; the average particle size of the bulk molybdenum disulfide is 1 μm, and the average particle size of the graphite is 6 μm;

[0122] Curing agent: dicyandiamide;

[0123] Additives: a mixture of dispersant Tech-6325 and leveling agent MHC60-6100 in a mass ratio of 3:1;

[0124] Few-layer molybdenum disulfide: The preparation process is as follows: After drying the bulk molybdenum disulfide at 80°C for 2.5 hours, adding it to N-methylpyrrolidone to obtain a dispersion with a concentration of 55 mg / ml, ultrasonicating it at 35°C at a power of 550W for 6 hours to obtain a suspension containing few-layer molybdenum disulfide, and then centrifuging it at a speed of 10,000 rpm for 30 minutes to obtain a supernatant, adding 25% ethanol solution, repeatedly centrifuging and washing until N-methylpyrrolidone is completely replaced, and dispersing the centrifugal precipitate in 25% ethanol solution and then freeze-drying it to obtain few-layer molybdenum disulfide with an average particle size of 350 nm;

[0125] (2) Preparation of resin coating liquid:

[0126] (2.1) Add the curing agent to N,N-dimethylformamide and shake evenly to obtain a clear solution;

[0127] (2.2) mixing the epoxy resin and the clarified solution uniformly to obtain a resin glue solution;

[0128] (2.3) drying the bulk solid lubricant at 80° C. for 2.5 h, mixing it with the resin glue, acetone, 2-butanone, cyclohexanone and additives, and performing ultrasonic dispersion for 45 min to obtain a mixed glue;

[0129] (2.4) Filter the mixed glue solution through a 800-mesh gauze to obtain a filtrate;

[0130] (2.5) A few layers of molybdenum disulfide were added to the filtrate, and the filtrate was sheared at a shear rate of 1000 rpm for 10 min, followed by ultrasonic treatment for 60 min to obtain a resin coating liquid suitable for oil lubrication.

[0131] In the finally obtained resin coating liquid suitable for oil lubrication, the volume ratio of acetone, 2-butanone and cyclohexanone is 2:1:1, the mass ratio of N,N-dimethylformamide to curing agent is 2:1, the content of the organic solvent composed of acetone, 2-butanone, cyclohexanone and N,N-dimethylformamide is 64.9wt%, the content of the bulk solid lubricant is 15wt%, the content of the few-layer molybdenum disulfide is 3wt%, the content of the additive is 0.1wt%, the content of the epoxy resin is 16wt%, and the content of the curing agent is 1wt%.

[0132] An application of a resin coating liquid suitable for oil lubrication, wherein the resin coating liquid prepared by the above method is ultrasonicated for 20 minutes, sprayed on the surface of a carbon steel sheet with an air spray gun at a pressure of 0.24 bar, and cured at 175° C. for 50 minutes to obtain a coating;

[0133] The thickness of the prepared coating is 29.88 μm, the impact resistance height is 40 cm, the friction coefficient is 0.038, and the wear rate is 0.366×10 -6 mm 3 / (N·m), the adhesion is level 0, the pencil hardness is 5H, and after 30 days of oil immersion, the adhesion is level 0 and the pencil hardness is 4H.

[0134] Example 4

[0135] A method for preparing a resin coating liquid suitable for oil lubrication, the specific steps are as follows:

[0136] (1) Prepare materials:

[0137] acetone;

[0138] 2-Butanone;

[0139] Cyclohexanone;

[0140] N,N-dimethylformamide;

[0141] Epoxy resin: bisphenol A type resin KSR-177;

[0142] Bulk solid lubricant: composed of bulk molybdenum disulfide and graphite in a mass ratio of 14:9; the average particle size of the bulk molybdenum disulfide is 5μm, and the average particle size of the graphite is 10μm;

[0143] Curing agent: dicyandiamide;

[0144] Additives: dispersant Tech-6325;

[0145] Few-layer molybdenum disulfide: The preparation process is as follows: After drying the bulk molybdenum disulfide at 80°C for 3 hours, adding it to N-methylpyrrolidone to obtain a dispersion with a concentration of 65 mg / ml, ultrasonicating it at 25°C at a power of 250 W for 12 hours to obtain a suspension containing few-layer molybdenum disulfide, and then centrifuging it at a speed of 10,000 rpm for 30 minutes to obtain a supernatant, adding 25% ethanol solution, repeatedly centrifuging and washing until N-methylpyrrolidone is completely replaced, and dispersing the centrifugal precipitate in 25% ethanol solution and then freeze-drying it to obtain few-layer molybdenum disulfide with an average particle size of 500 nm;

[0146] (2) Preparation of resin coating liquid:

[0147] (2.1) Add the curing agent to N,N-dimethylformamide and shake evenly to obtain a clear solution;

[0148] (2.2) mixing the epoxy resin and the clarified solution uniformly to obtain a resin glue solution;

[0149] (2.3) drying the bulk solid lubricant at 80° C. for 3 h, mixing it with the resin glue, acetone, 2-butanone, cyclohexanone and additives, and performing ultrasonic dispersion for 60 min to obtain a mixed glue;

[0150] (2.4) Filter the mixed glue solution through a 500-mesh gauze to obtain a filtrate;

[0151] (2.5) A few layers of molybdenum disulfide were added to the filtrate, and the filtrate was sheared at a shear rate of 1000 rpm for 10 min, followed by ultrasonic treatment for 60 min to obtain a resin coating liquid suitable for oil lubrication.

[0152] In the finally obtained resin coating liquid suitable for oil lubrication, the volume ratio of acetone, 2-butanone and cyclohexanone is 2:1:1, the mass ratio of N,N-dimethylformamide to curing agent is 4:1, the content of the organic solvent composed of acetone, 2-butanone, cyclohexanone and N,N-dimethylformamide is 55wt%, the content of the bulk solid lubricant is 15wt%, the content of the few-layer molybdenum disulfide is 3wt%, the content of the additive is 0.5wt%, the content of the epoxy resin is 25wt%, and the content of the curing agent is 1.5wt%.

[0153] An application of a resin coating liquid suitable for oil lubrication, wherein the resin coating liquid prepared by the above method is ultrasonicated for 20 minutes, sprayed on the surface of a carbon steel sheet with an air spray gun at a pressure of 0.24 bar, and cured at 165° C. for 70 minutes to obtain a coating;

[0154] The thickness of the prepared coating is 20.15 μm, the impact resistance height is 43 cm, the friction coefficient is 0.039, and the wear rate is 0.324×10 -6 mm 3 / (N·m), the adhesion is level 0, the pencil hardness is 5H, and after 30 days of oil immersion, the adhesion is level 0 and the pencil hardness is 4H.

[0155] Example 5

[0156] A method for preparing a resin coating liquid suitable for oil lubrication, the specific steps are as follows:

[0157] (1) Prepare materials:

[0158] acetone;

[0159] 2-Butanone;

[0160] Cyclohexanone;

[0161] N,N-dimethylformamide;

[0162] Epoxy resin: a mixture of bisphenol A epoxy resin YD-128 and bisphenol A resin KSR-177 in a mass ratio of 1:1;

[0163] Bulk solid lubricant: composed of bulk molybdenum disulfide and graphite in a mass ratio of 14:11; the average particle size of the bulk molybdenum disulfide is 4μm, and the average particle size of the graphite is 8μm;

[0164] Curing agent: dicyandiamide;

[0165] Additives: leveling agent MHC60-6100;

[0166] Few-layer molybdenum disulfide: The preparation process is as follows: After drying the bulk molybdenum disulfide at 80°C for 3.5 hours, adding it to N-methylpyrrolidone to obtain a dispersion with a concentration of 70 mg / ml, ultrasonicating it at 600W power for 12 hours at 25°C to obtain a suspension containing few-layer molybdenum disulfide, centrifuging it at 10,000 rpm for 30 minutes to obtain a supernatant, adding 25% ethanol solution, repeatedly centrifuging and washing until N-methylpyrrolidone is completely replaced, dispersing the centrifugal precipitate in 25% ethanol solution, and then freeze-drying it to obtain few-layer molybdenum disulfide with an average particle size of 50 nm;

[0167] (2) Preparation of resin coating liquid:

[0168] (2.1) Add the curing agent to N,N-dimethylformamide and shake evenly to obtain a clear solution;

[0169] (2.2) mixing the epoxy resin and the clarified solution uniformly to obtain a resin glue solution;

[0170] (2.3) drying the bulk solid lubricant at 80° C. for 3.5 h, mixing it with the resin glue, acetone, 2-butanone, cyclohexanone and additives, and performing ultrasonic dispersion for 60 min to obtain a mixed glue;

[0171] (2.4) Filter the mixed glue solution through a 500-mesh gauze to obtain a filtrate;

[0172] (2.5) A few layers of molybdenum disulfide were added to the filtrate, and the filtrate was sheared at a shear rate of 1000 rpm for 10 min, followed by ultrasonication for 30 min to obtain a resin coating liquid suitable for oil lubrication.

[0173] In the finally obtained resin coating liquid suitable for oil lubrication, the volume ratio of acetone, 2-butanone and cyclohexanone is 2:1:1, the mass ratio of N,N-dimethylformamide to curing agent is 4:1, the content of the organic solvent composed of acetone, 2-butanone, cyclohexanone and N,N-dimethylformamide is 45wt%, the content of the bulk solid lubricant is 15wt%, the content of the few-layer molybdenum disulfide is 4wt%, the content of the additive is 1wt%, the content of the epoxy resin is 32wt%, and the content of the curing agent is 3wt%.

[0174] An application of a resin coating liquid suitable for oil lubrication, wherein the resin coating liquid prepared by the above method is ultrasonicated for 20 minutes, sprayed on the surface of a carbon steel sheet with an air spray gun at a pressure of 0.24 bar, and cured at 170° C. for 60 minutes to obtain a coating;

[0175] The thickness of the prepared coating is 26.32 μm, the impact resistance height is 45 cm, the friction coefficient is 0.035, and the wear rate is 0.268×10 -6 mm3 / (N·m), the adhesion is level 0, the pencil hardness is 5H, and after 30 days of oil immersion, the adhesion is level 0 and the pencil hardness is 4H.

[0176] Example 6

[0177] A method for preparing a resin coating liquid suitable for oil lubrication, the specific steps are as follows:

[0178] (1) Prepare materials:

[0179] acetone;

[0180] 2-Butanone;

[0181] Cyclohexanone;

[0182] N,N-dimethylformamide;

[0183] Epoxy resin: a mixture of bisphenol A epoxy resin YD-128 and bisphenol A resin KSR-177 in a mass ratio of 2:1;

[0184] Bulk solid lubricant: composed of bulk molybdenum disulfide and graphite in a mass ratio of 14:11; the average particle size of the bulk molybdenum disulfide is 6μm, and the average particle size of the graphite is 4μm;

[0185] Curing agent: dicyandiamide;

[0186] Additives: a mixture of dispersant Tech-6325 and leveling agent MHC60-6100 in a mass ratio of 1:1;

[0187] Few-layer molybdenum disulfide: The preparation process is as follows: After drying the bulk molybdenum disulfide at 80°C for 4 hours, adding it to N-methylpyrrolidone to obtain a dispersion with a concentration of 80 mg / ml, ultrasonicating it at 400W power for 8 hours at 25°C to obtain a suspension containing few-layer molybdenum disulfide, and then centrifuging it at a speed of 10000rpm for 30 minutes to obtain a supernatant, adding 25% ethanol solution, repeatedly centrifuging and washing until N-methylpyrrolidone is completely replaced, and dispersing the centrifugal precipitate in 25% ethanol solution and freeze-drying it to obtain few-layer molybdenum disulfide with an average particle size of 150nm;

[0188] (2) Preparation of resin coating liquid:

[0189] (2.1) Add the curing agent to N,N-dimethylformamide and shake evenly to obtain a clear solution;

[0190] (2.2) mixing the epoxy resin and the clarified solution uniformly to obtain a resin glue solution;

[0191] (2.3) drying the bulk solid lubricant at 80° C. for 4 h, mixing it with the resin glue, acetone, 2-butanone, cyclohexanone and additives, and performing ultrasonic dispersion for 45 min to obtain a mixed glue;

[0192] (2.4) Filter the mixed glue solution through a 500-mesh gauze to obtain a filtrate;

[0193] (2.5) A few layers of molybdenum disulfide were added to the filtrate, and the filtrate was sheared at a shear rate of 1000 rpm for 10 min, followed by ultrasonication for 30 min to obtain a resin coating liquid suitable for oil lubrication.

[0194] In the finally obtained resin coating liquid suitable for oil lubrication, the volume ratio of acetone, 2-butanone and cyclohexanone is 2:1:1, the mass ratio of N,N-dimethylformamide to curing agent is 3:1, the content of the organic solvent composed of acetone, 2-butanone, cyclohexanone and N,N-dimethylformamide is 40wt%, the content of the bulk solid lubricant is 20wt%, the content of the few-layer molybdenum disulfide is 5wt%, the content of the additive is 1wt%, the content of the epoxy resin is 32wt%, and the content of the curing agent is 2wt%.

[0195] An application of a resin coating liquid suitable for oil lubrication, wherein the resin coating liquid prepared by the above method is ultrasonicated for 20 minutes, sprayed on the surface of a carbon steel sheet with an air spray gun at a pressure of 0.24 bar, and cured at 175° C. for 50 minutes to obtain a coating;

[0196] The thickness of the prepared coating is 24.53 μm, the impact resistance height is 41 cm, the friction coefficient is 0.041, and the wear rate is 0.339×10 -6 mm 3 / (N·m), the adhesion is level 0, the pencil hardness is 5H, and after 30 days of oil immersion, the adhesion is level 0 and the pencil hardness is 4H.

Claims

1. A resin coating liquid suitable for oil lubrication, characterized in that: It contains 20-40wt% epoxy resin, 15-25wt% bulk solid lubricant, 20-65wt% organic solvent, 1-5wt% curing agent, 3-8wt% few-layer molybdenum disulfide, and 0.1-1wt% additives; The bulk solid lubricant is composed of bulk molybdenum disulfide and graphite in a mass ratio of 7:4-6; the average particle size of the bulk molybdenum disulfide is 0.1-20 μm, and the average particle size of the graphite is 0.1-10 μm; The organic solvent consists of acetone, 2-butanone, cyclohexanone and N,N-dimethylformamide; The average particle size of few-layer MoS2 is 50nm~0.5μm; The preparation process of few-layer molybdenum disulfide is as follows: after drying the bulk molybdenum disulfide, add it into N-methylpyrrolidone to obtain a dispersion with a concentration of 50-80 mg / mL, ultrasonicate it at a power of 250-600 W for 4-12 hours at 25-35°C to obtain a suspension containing few-layer molybdenum disulfide, and obtain the few-layer molybdenum disulfide after post-treatment.

2. A resin coating liquid suitable for oil lubrication according to claim 1, characterized in that: The average particle size of bulk molybdenum disulfide is 0.1~5μm, and the average particle size of graphite is 0.1~5μm.

3. The resin coating liquid suitable for oil lubrication according to claim 1, characterized in that: The additive is dispersant Tech-6325.

4. The resin coating liquid suitable for oil lubrication according to claim 1, characterized in that: The epoxy resin is bisphenol A epoxy resin YD-128 and / or bisphenol A resin KSR-177; the curing agent is dicyandiamide; the volume ratio of acetone, 2-butanone and cyclohexanone is 2:1:1, and the mass ratio of N,N-dimethylformamide to the curing agent is 2-4:

1.

5. A method for preparing a resin coating liquid suitable for oil lubrication as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Add the curing agent to N,N-dimethylformamide and shake evenly to obtain a clear solution; (2) Evenly mixing the epoxy resin and the clarified solution to obtain a resin glue solution; (3) After drying the bulk molybdenum disulfide and graphite, the bulk molybdenum disulfide and graphite are mixed with resin glue, acetone, 2-butanone, cyclohexanone and additives, and ultrasonically dispersed for 30 to 60 minutes to obtain a mixed glue; (4) filtering the mixed glue solution to obtain a filtrate; (5) Add a few layers of molybdenum disulfide to the filtrate and ultrasonicate for 30 to 60 minutes after shearing to obtain a resin coating liquid suitable for oil lubrication.

6. The use of a resin coating liquid suitable for oil lubrication according to any one of claims 1 to 4, characterized in that: The resin coating liquid is sprayed on the surface of the metal substrate and cured to obtain a coating.

7. The use according to claim 6, characterized in that: The thickness of the coating is 20~30μm, the impact resistance height is 40~45cm, the friction coefficient of the coating is 0.03~0.045, and the wear rate of the coating is 0.260×10 -6 ~0.430×10 -6 mm 3 / (N•m), the adhesion of the coating is level 0, and the pencil hardness is 5H. After 30 days of oil immersion, the adhesion of the coating is level 0~1, and the pencil hardness is 3~4H.

Citation Information

Patent Citations

  • Molybdenum disulphide high dispersion modified epoxy resin wear-resistant coating material and preparation method thereof

    CN101423726A

  • Composition for preparing self-lubricating wear-resistant material, self-lubricating wear-resistant paint, self-lubricating wear-resistant coating, and self-lubricating wear-resistant material

    CN110016277A

  • Liquid coating and preparation method thereof

    CN102002302A

  • Preparation method of stratified molybdenum disulfide nano material

    CN104495936A

  • Expanded grahpite / molybdenum disulfide composite solid lubricating material and its preparing process