Coating composition for flexible display, preparation method and application

By applying a coating composition containing silicone modified polyester resin, nanofiller, curing agent and leveling agent on ultra-thin glass, the UTG product has been solved in terms of hardness, impact resistance and bending resistance. Inadequately, the preparation of high-performance coating films has been achieved.

CN116554774BActive Publication Date: 2024-11-29CHENGDU TOMI SHUANG DU OPTOELECTRONICS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210102725.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-27
Publication Date
2024-11-29
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

Existing ultra-thin glass (UTG) products have shortcomings in hardness, impact resistance, bending resistance and touch feel, and the coating process is complex and impact resistance is limited.

Method used

Using a coating composition comprising 25 to 60 weight percent silicone modified polyester resin, 5 to 25 weight percent nanofiller, 10 to 30 weight percent curing agent and 3 to 6 weight percent Leveling agent and dispersing and mixing by a multi-step preparation method to improve the performance of the coating.

Benefits of technology

The hardness, impact resistance, bending resistance and scratch resistance of the coating composition are significantly improved, and there is basically no warping after curing. The obtained coating film has excellent surface adhesion and self-cleaning ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116554774B_ABST
    Figure CN116554774B_ABST
Patent Text Reader

Abstract

The present application provides a method for preparing a coating composition, a coating composition and a product comprising the coating composition. The coating composition provided in the present application has significantly improved hardness, impact resistance, bending resistance and scratch resistance, and is suitable for flexible display panels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of flexible display materials, and in particular to a coating composition, a method for preparing the coating composition, and a product comprising the coating composition. Background Art

[0002] Early flexible displays usually attached a transparent polyimide (CPI) film to a flexible organic electroluminescent (OLED) display. However, the CPI film has low optical transmittance, poor bending performance, and poor touch feel. The subsequent development of ultra-thin glass (UTG) replaced the CPI film based on relatively high transparency, bending resistance, and touch feel. The bending resistance of UTG increases as the thickness of the glass decreases, but the thinner the thickness, the worse the impact resistance of the glass.

[0003] In order to improve the impact resistance, a film or coating is usually applied to the surface of UTG to form an organic film that is resistant to bending. However, the UTG products with film still have disadvantages such as poor hand feel, low hardness, and creases after bending. The existing coated UTG products need to be coated with multiple layers to basically meet the requirements for hardness, impact resistance, bending resistance, and touch feel. The process is complicated and the impact resistance is limited.

[0004] There is an urgent need for coating compositions that improve the hardness, impact resistance, bending resistance, and touch feel of UTG products. Summary of the invention

[0005] In one aspect, embodiments of the present application provide a coating composition.

[0006] The coating composition comprises:

[0007] 25 to 60 weight percent of silicone-modified polyester resin,

[0008] 5 to 25 weight percent of nanofillers,

[0009] 10 to 30 weight percent of a curing agent, and

[0010] 3 to 6 weight percent of leveling agent,

[0011] All weight percentage values ​​are based on the total weight of the coating composition.

[0012] According to an embodiment of the present application, the coating composition further comprises 20 to 50 weight percent of a solvent based on the total weight of the coating composition.

[0013] The organosilicon-modified polyester resin is a polyester resin modified by one or more of a phenyl organosilicon intermediate containing terminal hydroxyl groups, a methyl organosilicon intermediate containing terminal hydroxyl groups, an amino organosilicon intermediate containing terminal hydroxyl groups, a methoxy organosilicon intermediate, an ethoxy organosilicon intermediate, and a methylphenyl organosilicon intermediate containing terminal hydroxyl groups.

[0014] The ratio of the hydroxyl group of the polyester resin to the methoxy group, ethoxy group or terminal hydroxyl group or a combination thereof of the organic silicon intermediate is 1-4:1.

[0015] The nano filler is one or more of nano silicon dioxide, nano aluminum oxide, nano zirconium oxide, nano calcium carbonate, rutile nano titanium dioxide and anatase nano titanium dioxide.

[0016] The curing agent is isocyanate or amino resin, wherein the ratio of the hydroxyl group of the organosilicon-modified polyester resin to the isocyanate group of the curing agent is 1:0.3-1.5.

[0017] The leveling agent is one or both of a silicon leveling agent and a non-silicon leveling agent. In one example, the non-silicon leveling agent is cellulose acetate.

[0018] The solvent is one or more of oxalic acid ethyl ether acetate, xylene, and methyl isobutyl ketone.

[0019] In an exemplary embodiment, the coating composition has the following properties:

[0020] According to the hardness of H to 3H measured by the pencil hardness tester of GB / T6739-1996 standard on ultra-thin glass of 30 to 100μm,

[0021] Adhesion of 5B was measured by the 100-grid test method according to ISO2409-1992.

[0022] The impact resistance of a 12.8g ballpoint pen with a 0.5mm diameter refill is measured by letting the pen tip fall freely and continuously raising the height of the pen until cracks appear on the glass.

[0023] According to the dynamic U-bending (radius R1.5mm, bending from 180° to 0°, then bending from 0° to 180°, in this cycle, 40 times per minute) measured by dynamic bending 200,000 times without film peeling, and

[0024] According to the steel wool friction resistance of the paint film, there is no visible scratch when rubbed 2500 times with a 20*20mm die and 0000# steel wool under a load of 1000g. On the other hand, the embodiment of the present application provides a method for preparing a coating composition, comprising:

[0025] (a) reacting a polyester resin with an organosilicon intermediate in the presence of a solvent to obtain an organosilicon-modified polyester resin;

[0026] (b) subjecting the organosilicon-modified polyester resin and the nanofiller to a dispersion treatment;

[0027] (c) adding a curing agent to the mixture obtained in step (b) and mixing; and

[0028] (d) adding a leveling agent to the mixture obtained in step (c) and mixing, thereby obtaining the coating composition.

[0029] According to the method of an embodiment of the present application, the polyester resin in the step (a) is obtained by reacting a polyol with a polyacid.

[0030] In an exemplary embodiment, the polyol and the polyacid react at 180° C. to 250° C. for 3 to 6 hours, preferably in a nitrogen atmosphere. The polyol and the polyacid have a molar ratio of 1-5:1, more preferably 1.2-1.7:1.

[0031] In an exemplary embodiment, the polyol is one or more of trimethylolpropane, pentaerythritol, and glycerol. The polyacid is one or more of isophthalic acid, pyromellitic acid, terephthalic acid, and adipic acid.

[0032] According to the method of an embodiment of the present application, in the step (a), the polyester resin and the solvent are heated to 80°C to 120°C, preferably 100°C, under stirring, and then the organosilicon intermediate is added and the mixture is reacted at 120°C to 150°C for 1.5 to 3.5 hours.

[0033] In exemplary embodiments, the solvent is one or more of ethyl ether acetate, xylene, and methyl isobutyl ketone.

[0034] In an exemplary embodiment, the organosilicon intermediate is one or more of a phenyl organosilicon intermediate containing terminal hydroxyl groups, a methyl organosilicon intermediate containing terminal hydroxyl groups, an amino organosilicon intermediate containing terminal hydroxyl groups, a methoxy organosilicon intermediate, an ethoxy organosilicon intermediate, and a methylphenyl organosilicon intermediate containing terminal hydroxyl groups.

[0035] In an exemplary embodiment, the polyester resin is added in an amount of 15 to 30% by weight based on the total weight added. The silicone intermediate is added in an amount of 15 to 30% by weight based on the total weight added.

[0036] In an exemplary embodiment, the solvent is added in an amount of 30 to 60% by weight based on the total weight added. Thus, it can be ensured that the prepared coating composition can contain 20 to 50 weight percent of the solvent based on the total weight of the coating composition.

[0037] In an exemplary embodiment, the ratio of the hydroxyl group of the polyester resin to the methoxyl group, ethoxyl group, or terminal hydroxyl group, or a combination thereof, of the organosilicon intermediate is 1-4: 1. In an exemplary embodiment, the ratio of the hydroxyl group of the polyester resin to the methoxyl group, ethoxyl group, or terminal hydroxyl group, or a combination thereof, of the organosilicon intermediate is 1-2.5: 1.

[0038] According to the method of an embodiment of the present application, in the step (b), the organosilicon-modified polyester resin and the nanofiller are ultrasonically dispersed at 35° C. to 70° C. for 20 to 50 minutes.

[0039] In an exemplary embodiment, the nanofiller is one or more of nano-silicon dioxide, nano-alumina, nano-zirconium oxide, nano-calcium carbonate, rutile nano-titanium dioxide and anatase nano-titanium dioxide.

[0040] In exemplary embodiments, the nanofiller is added in an amount of 5 to 25% by weight based on the total weight added.

[0041] According to the method of an embodiment of the present application, in the step (c), the curing agent is isocyanate or amino resin.

[0042] In an exemplary embodiment, the curing agent is added in an amount of 10 to 30% by weight based on the total weight added.

[0043] In an exemplary embodiment, a ratio of a hydroxyl group of the silicone-modified polyester resin to an isocyanate group of the curing agent is 1:0.3-1.5.

[0044] According to the method of the embodiment of the present application, in the step (d), the leveling agent is one or both of a silicon leveling agent and a non-silicon leveling agent. In one example, the non-silicon leveling agent is cellulose acetate.

[0045] In an exemplary embodiment, the silicon leveling agent is added in an amount of 0.1 to 1% by weight based on the total weight added. The cellulose acetate is added in an amount of 3 to 5% by weight based on the total weight added.

[0046] According to the method of an embodiment of the present application, before step (d), the mixture obtained in step (c) is kept at room temperature for 0 to 12 hours, preferably 6 hours, and more preferably 4 hours.

[0047] On the other hand, an embodiment of the present application further provides an article, which includes the coating composition described in the above aspects.

[0048] In some embodiments, the coating composition is prepared by the method for preparing a coating composition described in the above aspects.

[0049] In an exemplary embodiment, the article is a coating film of ultra-thin glass. In an exemplary embodiment, the coating film has a thickness of 4 to 30 μm.

[0050] The method proposed in the embodiment of the present application is carried out in multiple steps, the reaction process is easy to control, there are few side reactions, and it can react immediately after adding the curing agent, without the need for end-capping and unblocking. In addition, it can also remain stable for a long time at room temperature after adding the curing agent. By adopting the method proposed in the embodiment of the present application, the prepared coating composition has significantly improved hardness, impact resistance, bending resistance and scratch resistance, and basically no warping occurs after curing, and the obtained coating film has an excellent surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 is a flow chart of a method for preparing a coating composition according to an embodiment of the present application. DETAILED DESCRIPTION

[0052] This application is based on the inventor's discovery and understanding of the following facts and problems:

[0053] By adding silicone resin to polyester resin oligomer to copolymerize to generate silicone modified polyester resin, the polyester resin obtains a large number of Si-O bonds, and forms a network structure through cross-linking polymerization, with a high degree of cross-linking, which can significantly improve the hardness of the composition. The silicone modified polyester resin also makes the composition have good viscoelasticity, and the composition is directly coated on ultra-thin glass with good adhesion. A specifically selected curing agent is added to the system so that the composition can withstand high temperature curing, such as using isocyanate or polyurethane as a curing agent, allowing the gap between molecules to be filled during curing, and the reaction is carried out in a slower manner than ultraviolet light curing, which can reduce the internal stress of the coating composition, making the coating film less prone to warping and crack-free. By adding inorganic nanofillers to the system, the high hardness and wear resistance of the inorganic nanofillers further significantly improve the hardness and wear resistance of the composition. At the same time, the inorganic nanofiller can absorb ultraviolet light, absorb light with large energy of the bandgap when irradiated by ultraviolet light, thereby reducing the aging of the coating film by external ultraviolet light, so that the coating film has the performance of yellowing resistance. In addition, the presence of the leveling agent enables the coating composition to exhibit good coating properties. The specifically selected solvent can also dilute the components to the required concentration, ensuring that no bubbles and orange peel lines are generated during the baking and curing process, thereby obtaining an excellent surface.

[0054] Efforts have been made in the art to develop coating materials for flexible displays.

[0055] For example, patent application CN108864938A describes a hard coating material composition and a window construction with a hard coating. In the above patent, the hard coating material composition uses silsesquioxane and siloxane compounds as the main components. The hardness of the composition is very high, but the toughness of the composition is not good, and it is easy to crack when subjected to external force, and the bending resistance is average. The composition adopts a light curing curing method, which has a fast reaction and is prone to obvious warping.

[0056] Patent application CN112876989A provides a highly impact-resistant ultra-thin glass cover plate and a preparation method thereof. The three layers of the ultra-thin glass cover plate are: ultra-thin glass / adhesion enhancement layer / self-healing polymer layer / hard coating. The hard coating is compounded from one or two of acrylate, methyl methacrylate, epoxy resin and polysiloxane. The hardness of acrylate and methyl methacrylate used in the hard coating is not high enough, the strength of epoxy resin is weak and easy to scratch, and the adhesion of polysiloxane to the substrate is poor.

[0057] Patent application CN108623797A discloses a water-soluble silicone-modified polyester resin. The above patent sequentially reacts the reaction system from the first reaction temperature to the fifth reaction temperature, which is complex to control and prone to side reactions. It is also necessary to add a capping agent and unblock the resin material before use, which is a complex process. The obtained silicone-modified polyester resin is a water-based resin material suitable for applications with low requirements on appearance, such as automotive spray painting.

[0058] In one aspect, an embodiment of the present application provides a coating composition. The coating composition comprises:

[0059] 25 to 60 weight percent of silicone-modified polyester resin,

[0060] 5 to 25 weight percent of nanofillers,

[0061] 10 to 30 weight percent of a curing agent, and

[0062] 3 to 6 weight percent of leveling agent,

[0063] All weight percentage values ​​are based on the total weight of the coating composition.

[0064] According to an embodiment of the present application, the coating composition further comprises 20 to 50 weight percent of a solvent based on the total weight of the coating composition.

[0065] The organosilicon-modified polyester resin is a polyester resin modified by one or more of a phenyl organosilicon intermediate containing terminal hydroxyl groups, a methyl organosilicon intermediate containing terminal hydroxyl groups, an amino organosilicon intermediate containing terminal hydroxyl groups, a methoxy organosilicon intermediate, an ethoxy organosilicon intermediate, and a methylphenyl organosilicon intermediate containing terminal hydroxyl groups. The ratio of the hydroxyl group of the polyester resin to the methoxy group, ethoxy group, or terminal hydroxyl group or a combination thereof of the organosilicon intermediate is 1-4:1.

[0066] The nano filler is one or more of nano silicon dioxide, nano aluminum oxide, nano zirconium oxide, nano calcium carbonate, rutile nano titanium dioxide and anatase nano titanium dioxide.

[0067] The curing agent is isocyanate or amino resin, wherein the ratio of the hydroxyl group of the organosilicon-modified polyester resin to the isocyanate group of the curing agent is 1:0.3-1.5.

[0068] The leveling agent is one or both of a silicon leveling agent and a non-silicon leveling agent. In one example, the non-silicon leveling agent is cellulose acetate.

[0069] The solvent is one or more of oxalic acid ethyl ether acetate, xylene, and methyl isobutyl ketone.

[0070] According to an embodiment of the present application, the coating composition comprises 25 to 60 weight percent of an organosilicon-modified polyester resin based on the total weight of the coating composition. In some embodiments, the coating composition comprises 30 to 60 weight percent of an organosilicon-modified polyester resin. In some exemplary embodiments, the coating composition comprises 35 to 55 weight percent of an organosilicon-modified polyester resin. In some exemplary embodiments, the coating composition comprises 40 to 55 weight percent of an organosilicon-modified polyester resin. In some embodiments, the coating composition comprises 25 to 40 weight percent of an organosilicon-modified polyester resin. In some embodiments, the coating composition comprises 25 to 35 weight percent of an organosilicon-modified polyester resin.

[0071] According to an embodiment of the present application, the coating composition comprises 5 to 25 weight percent of nanofiller based on the total weight of the coating composition. In some embodiments, the coating composition comprises 5 to 20 weight percent of nanofiller. In an exemplary embodiment, the coating composition comprises 7 to 15 weight percent of nanofiller.

[0072] According to an embodiment of the present application, the coating composition further comprises 20 to 50 weight percent of a solvent based on the total weight of the coating composition. In some embodiments, the coating composition comprises 20 to 45 weight percent of a solvent. In some exemplary embodiments, the coating composition comprises 25 to 45 weight percent of a solvent. In some exemplary embodiments, the coating composition comprises 30 to 40 weight percent of a solvent.

[0073] In exemplary embodiments, the coating composition of the present application has the following properties:

[0074] According to the hardness of H to 3H measured by the pencil hardness tester of GB / T6739-1996 standard on ultra-thin glass of 30 to 100μm,

[0075] Adhesion of 5B was measured by the 100-grid test method according to ISO2409-1992.

[0076] The impact resistance of a 12.8g ballpoint pen with a 0.5mm diameter refill is measured by dropping the pen tip downward and continuously raising the height of the pen until cracks appear on the glass.

[0077] According to the dynamic U-bending (radius R1.5mm, bending from 180° to 0°, then bending from 0° to 180°, in this cycle, 40 times per minute) measured by dynamic bending 200,000 times without film peeling, and

[0078] According to the paint film's resistance to steel wool friction, there is no visible scratch when rubbed 2500 times with a 20*20mm die and 0000# steel wool under a load of 1000g. In another aspect, the embodiment of the present application provides a method for preparing a coating composition. The method provided in the embodiment of the present application is carried out in multiple steps, the reaction process is easy to control, there are few side reactions, and it can react immediately after adding a curing agent without the need for end-capping and unblocking. In addition, it can also maintain long-term stability at room temperature after adding a curing agent.

[0079] Figure 1 is a flow chart of a method for preparing a coating composition according to an embodiment of the present application. Figure 1 , the method comprises the following steps.

[0080] S101: (a) reacting a polyester resin with an organosilicon intermediate in the presence of a solvent to obtain an organosilicon-modified polyester resin.

[0081] According to the method of the embodiment of the present application, the polyester resin in the step (a) is obtained by reacting a polyol with a polyacid. In an exemplary embodiment, the polyol and the polyacid are reacted at 180° C. to 250° C., preferably in a nitrogen atmosphere, for 3 to 6 hours. The polyol and the polyacid have a molar ratio of 1-5:1, more preferably a molar ratio of 1.2-1.7:1.

[0082] Polyester resin material itself has good viscoelasticity and can be directly coated on ultra-thin glass or primer with good adhesion, and the standard 100-grid test can reach 5B. At the same time, because of its elasticity, it also has good impact resistance.

[0083] In an exemplary embodiment, the polyol is one or more of trimethylolpropane, pentaerythritol, and glycerol. The polyacid is one or more of isophthalic acid, pyromellitic acid, terephthalic acid, and adipic acid.

[0084] According to the method of an embodiment of the present application, in the step (a), the polyester resin and the solvent are heated to 80°C to 120°C under stirring. In some embodiments, the polyester resin and the solvent are heated to 100°C under stirring. The organosilicon intermediate is then added and the mixture is reacted at 120°C to 150°C for 1.5 to 3.5 hours. In some embodiments, the organosilicon intermediate and the polyester resin are heated to 130°C and reacted at this temperature for 2 hours.

[0085] The obtained organosilicon-modified polyester resin contains a large number of Si-O bonds and forms a network structure through cross-linking reaction, which significantly improves the hardness of the coating composition. In addition, the presence of Si-O bonds makes the coating composition have a larger contact angle, making it difficult for dirt to adhere to the surface.

[0086] In an exemplary embodiment, the organosilicon intermediate is one or more of a phenyl organosilicon intermediate containing terminal hydroxyl groups, a methyl organosilicon intermediate containing terminal hydroxyl groups, an amino organosilicon intermediate containing terminal hydroxyl groups, a methoxy organosilicon intermediate, an ethoxy organosilicon intermediate, and a methylphenyl organosilicon intermediate containing terminal hydroxyl groups.

[0087] The polyester resin is added in an amount of 15 to 30% by weight based on the total weight added. The silicone intermediate is added in an amount of 15 to 30% by weight based on the total weight added.

[0088] In an exemplary embodiment, the ratio of the hydroxyl group of the polyester resin to the methoxyl group, ethoxyl group, or terminal hydroxyl group, or a combination thereof, of the organosilicon intermediate is 1-4: 1. In an exemplary embodiment, the ratio of the hydroxyl group of the polyester resin to the methoxyl group, ethoxyl group, or terminal hydroxyl group, or a combination thereof, of the organosilicon intermediate is 1-2.5: 1.

[0089] Within this concentration range, the obtained organosilicon-modified polyester resin serves as the main component of the coating composition rather than as the only component, thereby imparting high hardness, good bending resistance and impact resistance, and good adhesion to the coating composition.

[0090] In an exemplary embodiment, the solvent is one or more of ethyl ether acetate, xylene, and methyl isobutyl ketone. In an exemplary embodiment, the solvent is added in an amount of 30 to 60% by weight based on the total weight added.

[0091] The oily composition of the present application will not produce poor surfaces such as shrinkage cavities and orange peel during coating and baking, and can be used in optoelectronic devices with high requirements on appearance, such as display panels, touch panels, cover plates, camera lenses, etc.

[0092] S102: (b) subjecting the organosilicon-modified polyester resin and the nanofiller to a dispersion treatment.

[0093] According to the method of the embodiment of the present application, in the step (b), the organosilicon-modified polyester resin and the nanofiller are ultrasonically dispersed at 35°C to 70°C for 20 to 50 minutes. In some embodiments, the organosilicon-modified polyester resin and the nanofiller are ultrasonically dispersed at 45°C to 60°C for 30 to 40 minutes. In some embodiments, the organosilicon-modified polyester resin and the nanofiller are ultrasonically dispersed at 50°C for 30 minutes. In this way, the nanofiller can be uniformly dispersed in the organosilicon-modified polyester resin.

[0094] In an exemplary embodiment, the nanofiller is one or more of nano-silicon dioxide, nano-alumina, nano-zirconium oxide, nano-calcium carbonate, rutile nano-titanium dioxide and anatase nano-titanium dioxide.

[0095] By adding nanofillers, the hardness and wear resistance of the coating composition can be significantly improved. The pencil hardness measured on ultra-thin glass of 30 to 100 μm is H to 3H. For glass substrates of 300 to 700 μm, the measured pencil hardness can reach 5H. According to the paint film's resistance to steel wool friction, it will not show visible scratches when rubbed 2500 times with a 20*20mm die and 000# steel wool under a load of 1000g. At the same time, the nanofiller can absorb ultraviolet light and absorb light with large energy of the bandgap when irradiated by ultraviolet light, thereby reducing the aging of the coating film by external ultraviolet light, making the coating film resistant to yellowing.

[0096] In an exemplary embodiment, the nanofiller is added in an amount of 5 to 25% by weight based on the total weight added. Within this concentration range, the hardness and wear resistance of the composition can be significantly improved.

[0097] S103: (c) adding a curing agent to the mixture obtained in step (b) and mixing.

[0098] According to the method of an embodiment of the present application, in the step (c), the curing agent is isocyanate or amino resin. Based on the total weight added, the curing agent is added in an amount of 10 to 30% by weight.

[0099] In an exemplary embodiment, a ratio of a hydroxyl group of the silicone-modified polyester resin to an isocyanate group of the curing agent is 1:0.3-1.5.

[0100] When using heat curing, the curing reaction is slower than that of UV curing, and the resulting paint film has less internal stress, which will not cause serious warping of the paint film.

[0101] The mixing in this step is performed by conventional means in the art so that the components are evenly distributed, for example, by stirring.

[0102] S104: (d) adding a leveling agent to the mixture obtained in step (c) and mixing, thereby obtaining the coating composition.

[0103] According to the method of the embodiment of the present application, in the step (d), the leveling agent is one or both of a silicon leveling agent and a non-silicon leveling agent. In one example, the non-silicon leveling agent is cellulose acetate.

[0104] In an exemplary embodiment, the silicon leveling agent is added in an amount of 0.1 to 1% by weight based on the total weight added. The cellulose acetate is added in an amount of 3 to 5% by weight based on the total weight added. The presence of the leveling agent enables the coating composition to exhibit good coating performance.

[0105] The mixing in this step is performed by conventional means in the art so that the components are evenly distributed, for example, by stirring.

[0106] The molecular weight of the silicone-modified polyester resin in the prepared coating composition is relatively high, the surface tension is lower than 80mN / m, and the surface wettability is poor. In addition, because the silicone-modified polyester resin has few polar groups and hydrophilic groups, the material polarity is extremely small, and the surface free energy is low, a certain amount of surfactant can be added to the system to further reduce the water contact angle, making it difficult for dirt to adhere to the surface, and making the ultra-thin glass surface have good self-cleaning ability.

[0107] According to the method of the embodiment of the present application, before step (d), the mixture obtained in step (c) is kept at room temperature for 0 to 12 hours, preferably 6 hours, and more preferably 4 hours. According to the method of the present application, after adding the curing agent to the system, it can remain stable for a long time at room temperature.

[0108] By adopting the method proposed in the embodiments of the present application, the prepared coating composition has significantly improved hardness, impact resistance, bending resistance and scratch resistance, and basically no warping occurs after curing, and the obtained coating film has an excellent surface.

[0109] On the other hand, the embodiment of the present application proposes a product, the product includes the coating composition described above. In an exemplary embodiment, the product is a coating film of ultra-thin glass. In some embodiments, the coating film has a thickness of 1 to 100 μm. In some embodiments, the coating film has a thickness of 4 to 30 μm, thereby ensuring the hardness, bending resistance and impact resistance of ultra-thin glass.

[0110] The coating composition of the present application has excellent toughness, wear resistance, impact resistance, bending resistance, high hardness and good adhesion to the substrate. Therefore, using the coating provided by the present application, the self-healing polymer layer in the related art can no longer be used. Furthermore, since the coating of the present application has good adhesion to ultra-thin glass, the bonding enhancement layer can be omitted. Therefore, a layer of coating provided by the present application can replace the three-layer film in the related art, such as bonding enhancement layer / self-healing polymer layer / hard coating.

[0111] Example

[0112] Example 1

[0113] Preparation of transparent hard coating material and coating on UTG. The preparation method comprises the following steps:

[0114] A. Preparation of polyester resin prepolymer:

[0115] Add 100g trihydroxymethylpropane and 96g adipic acid into a three-necked flask, pass cold water into the condenser tube so that the cold water in the condenser tube can just flow out continuously, gradually heat up to 130℃, start stirring and pass nitrogen, seal the flask after nitrogen fills it, gradually heat up to 220℃ and maintain this temperature for 4h, the heating rate is 10-20℃ / 10min. After 4h, stop heating and naturally cool to 130℃ and distill under reduced pressure for 1h. After the distillation is completed and cooled, add xylene of the same mass as the product and stir evenly.

[0116] B. Preparation of silicone-modified polyester resin

[0117] Take 100g of the polyester resin prepolymer prepared in step A and heat it to 100°C under stirring, add 58.5g of methoxy silicone intermediate (100% solid component, methoxy content 15%), gradually heat to 130°C for reaction, and the heating rate is 10-20°C / 10min. Stop heating after 2h, and naturally cool to room temperature for use.

[0118] C. Add filler

[0119] Take the organosilicon-modified polyester resin prepared in step B, add 51.2 g of porous fumed silica (particle size 100 nm) modified by KH550, and disperse it by ultrasonic at 50° C. for 30 min.

[0120] D. Compounding of hard coating materials

[0121] Take 242.5g of the material prepared in step C, add 52.5g of isocyanate MDI (100% content, -NCO content 32%) and stir evenly. Then add 0.34g of silicone leveling agent BYK313 and 15g of cellulose acetate butyrate. Add 50g of ethyl acetate, 50g of butyl acetate, and 30g of ethylene glycol ethyl ether acetate. Stir at 2000 rpm for 10 minutes. Thus, about 340g of hard coating material is obtained.

[0122] E. Hard coating material coating

[0123] Take 100g of the material prepared in step D, add 200g of ethyl acetate and 200g of ethylene glycol ethyl ether acetate, stir at 1800 rpm for 3min, put it into a vacuum defoaming box at 5kPa for 5min, then take it out and put it into the sprayer medicine tank. The 30μm thick UTG coated with 30μm thick polyester resin primer or acrylic resin primer is treated with plasma with a power of 700-900W and a travel speed of 2cm / s; then the configured hard coating material is coated with a coating flow of 10ml / min and a coating rate of 100cm / min. After coating, it enters an infrared tunnel furnace for thermal curing, the thermal curing temperature is 100℃, and the curing time is 10min; then the ultra-thin glass coated with the paint film is placed in a final baking oven for aging, the aging temperature is 140℃, and the aging time is 60min.

[0124] Example 2

[0125] A transparent hard coating material was prepared and coated on UTG according to the method described in Example 1. Compared with the preparation method of Example 1, the differences are as follows:

[0126] In step A, 108 g of trihydroxymethylpropane and 74.95 g of isophthalic acid are added to a three-necked flask for the preparation of a polyester resin prepolymer; after distillation is completed and cooled, ethyl ether acetate in an amount equal to the mass of the product is added and stirred evenly.

[0127] In step B, 90.8 g of ethoxy silicone intermediate (100% solid component, ethoxy content 15%) was added for preparing silicone-modified polyester resin.

[0128] In step C, 26.8 g of titanate-modified rutile titanium dioxide (particle size 100 nm) was added as a filler.

[0129] In step D, 123 g of the material prepared in step C was added with 56.5 g of polyurethane (70% solid content) and stirred evenly. 0.46 g of silicone leveling agent BYK313 and 20.5 g of cellulose acetate butyrate were added. 50 g of ethyl acetate, 50 g of butyl acetate and 60 g of xylene were added. Thus, about 360 g of hard coating material was obtained.

[0130] In step E, 100 g of the material prepared in step D was taken, 200 g of ethyl acetate and 200 g of xylene were used as solvents, stirred at 1800 rpm for 3 min, placed in a vacuum defoaming box at 5 kPa for 5 min, and then taken out and placed in a sprayer tank. Subsequently, the hard coating material was coated in a similar manner as in Example 1.

[0131] Example 3

[0132] A transparent hard coating material was prepared and coated on UTG according to the method described in Example 1. Compared with the preparation method of Example 1, the differences are as follows:

[0133] In step A, 108 g of trihydroxymethylpropane and 74.95 g of isophthalic acid are added to a three-necked flask for the preparation of a polyester resin prepolymer; after distillation is completed and cooled, ethyl ether acetate in an amount equal to the mass of the product is added and stirred evenly.

[0134] In step B, 100 g of the polyester resin prepolymer prepared in step A is heated to 110° C. under stirring, and 108.9 g of ethoxylated silicone intermediate (100% solid component, ethoxy content 15%) is added to prepare silicone-modified polyester resin.

[0135] In step C, 26.8 g of titanate-modified rutile titanium dioxide (particle size 100 nm) was added as a filler.

[0136] In step D, 123 g of the material prepared in step C was added with 56.5 g of polyurethane (70% solid content) and stirred evenly. 0.46 g of silicone leveling agent BYK313 and 20.5 g of cellulose acetate butyrate were added. 50 g of ethyl acetate, 50 g of butyl acetate and 60 g of xylene were added. The mixture was stirred at 2000 rpm for 10 min. Thus, about 360 g of hard coating material was obtained.

[0137] In step E, 100 g of the material prepared in step D was added with 200 g of ethyl acetate and 200 g of xylene, stirred at 1800 rpm for 3 min, placed in a vacuum defoaming box at 5 kPa for 5 min, and then taken out and placed in a sprayer tank. Subsequently, the hard coating material was coated in a similar manner as in Example 1.

[0138] Example 4

[0139] A transparent hard coating material was prepared and coated on UTG according to the method described in Example 1. Compared with the preparation method of Example 1, the differences are as follows:

[0140] In step A, 110 g of pentaerythritol and 74.95 g of terephthalic acid are added into a three-necked flask for preparing a polyester resin prepolymer; after distillation is completed and cooled, ethyl ether acetate in an amount equal to the mass of the product is added and stirred evenly.

[0141] In step B, 181.6 g of a methoxy silicone intermediate (100% solid component, methoxy content 15%) was added to prepare a silicone-modified polyester resin.

[0142] In step C, 26.8 g of titanate-modified rutile titanium dioxide (particle size 200 nm) was added as a filler.

[0143] In step D, 123 g of the material prepared in step C was added with 56.5 g of polyurethane (70% solid content) and stirred evenly. 0.46 g of silicone leveling agent BYK313 and 20.5 g of cellulose acetate butyrate were added. 50 g of ethyl acetate, 50 g of butyl acetate and 60 g of xylene were added. The mixture was stirred at 2000 rpm for 10 min. Thus, about 360 g of hard coating material was obtained.

[0144] In step E, 100 g of the material prepared in step D was taken, 200 g of ethyl acetate and 200 g of xylene were added as solvents, stirred at 1800 rpm for 3 min, placed in a vacuum defoaming box at 5 kPa for 5 min, and then taken out and placed in a sprayer tank. Subsequently, the hard coating material was coated in a similar manner as in Example 1.

[0145] Comparative Example

[0146] The cage-type silsesquioxane material is used as a coating material to coat the ultra-thin glass. The specific method is as follows.

[0147] Take 200g of cage-type silsesquioxane (60% solid content) material, add 100g of N,N-dimethylacetamide, stir at 1800 rpm for 5min, put it into a vacuum defoaming box for defoaming for 5min, and then put it into the sprayer tank.

[0148] The 30μm thick UTG coated with 30μm thick acrylic or polyester resin primer was plasma treated with a power of 800W and a travel speed of 2cm / s; the above-configured materials were used for coating, with a coating flow of 5ml / min and a coating speed of 700cm / min. After coating, it was pre-baked in an infrared tunnel furnace with a baking temperature of 140℃ and a baking time of 20min. It was placed in a UV curing machine for curing with a UV power of 6kW and a curing energy of 1700mJ / cm 2 After curing is completed, it is placed in the final oven and baked at 140°C for 30 minutes.

[0149] The ultra-thin glasses coated with the coating materials prepared in Examples 1 to 4 and Comparative Example were tested for performance according to the above-described test method. The test results are shown in Table 1 below.

[0150] Table 1 Performance test results of ultra-thin glass coated with coating materials

[0151]

[0152]

[0153] Conclusion: When the coating film prepared by the coating composition with different components and component contents in the present application is coated on the ultra-thin glass, the adhesion of the coating film on the ultra-thin glass reaches 5B; the ultra-thin glass coated with the coating film is impacted by a 12.8g ballpoint pen with a 0.5mm diameter refill, and no glass breakage is observed within a range of 10cm to 20cm; the hardness of the coating film is tested with a pencil hardness tester, and the hardness is H to 3H for ultra-thin glass of 30 to 100μm; the light transmittance in the visible light region is about 91%, b* (chromaticity value) is below 0.5, YI (yellowness) is below 0.5, and the haze is below 0.5.

[0154] In the present application, the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0155] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in the field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A coating composition for ultra-thin glass, characterized in that: Include: 25 to 60 weight percent of silicone-modified polyester resin, 5 to 25 weight percent of a nanofiller, wherein the nanofiller is one or more of nano-silicon dioxide, nano-alumina, nano-zirconium oxide, nano-calcium carbonate, rutile nano-titanium dioxide and anatase nano-titanium dioxide; 10 to 30 weight percent of a curing agent, and 3 to 6 weight percent of a leveling agent, wherein the leveling agent is one or both of a silicon leveling agent and a non-silicon leveling agent; The coating composition further comprises 20 to 50 weight percent of a solvent, Wherein all weight percentage values ​​are based on the total weight of the coating composition for ultra-thin glass; The organosilicon-modified polyester resin is a polyester resin modified by one or more of a methoxy organosilicon intermediate and an ethoxy organosilicon intermediate; The polyester resin is obtained by reacting a polyol with a polyacid, wherein the polyol is one or more of trimethylolpropane, pentaerythritol, and glycerol; The curing agent is isocyanate or polyurethane; The coating composition for ultra-thin glass has: According to the hardness of H to 3H measured by the pencil hardness tester of GB / T6739-1996 standard on ultra-thin glass of 30 to 100µm, Adhesion of 5B was measured by the 100-grid test method according to ISO2409-1992. The impact resistance of a 12.8g ballpoint pen with a 0.5mm diameter refill is measured by letting the pen tip fall freely and continuously raising the height of the pen until cracks appear on the glass. According to the dynamic U-bending, the radius is R1.5mm, bending from 180° to 0°, and then bending from 0° to 180°, in this cycle, 40 times per minute, the dynamic bending is measured 200,000 times without film peeling, and According to the steel wool friction resistance of the paint film, there is no visible scratch after rubbing 2500 times with a 20*20mm die and 0000# steel wool under a load of 1000g.

2. A method for preparing the coating composition for ultra-thin glass according to claim 1, characterized in that: include: (a) reacting a polyester resin with an organosilicon intermediate in the presence of a solvent to obtain an organosilicon-modified polyester resin; (b) subjecting the organosilicon-modified polyester resin and the nanofiller to a dispersion treatment; (c) adding a curing agent to the mixture obtained in step (b) and mixing; and (d) adding a leveling agent to the mixture obtained in step (c) and mixing, thereby obtaining the coating composition for ultra-thin glass.

3. The method for preparing a coating composition for ultra-thin glass according to claim 2, characterized in that: The polyester resin in step (a) is obtained by reacting a polyol with a polyacid, reacting the polyol with the polyacid at 180° C. to 250° C. for 3 to 6 hours, and / or, the polyol and the polyacid have a molar ratio of 1-5:1, And / or, the polyacid is one or more of isophthalic acid, pyromellitic acid, terephthalic acid, and adipic acid.

4. The method for preparing a coating composition for ultra-thin glass according to claim 3, characterized in that: The polyol and the polyacid have a molar ratio of 1.2-1.7:

1.

5. The method for preparing a coating composition for ultra-thin glass according to claim 2 or 3, characterized in that: In the step (a), the polyester resin and the solvent are heated to 80° C. to 120° C. under stirring, and then the organosilicon intermediate is added and the mixture is reacted at 120° C. to 150° C. for 1.5 to 3.5 hours, And / or, the solvent is one or more of ethyl ether acetate, xylene, and methyl isobutyl ketone.

6. The method for preparing a coating composition for ultra-thin glass according to claim 5, characterized in that: The ratio of the hydroxyl group of the polyester resin to the methoxy group, ethoxy group or terminal hydroxyl group or a combination thereof of the organic silicon intermediate is 1-4:

1.

7. The method for preparing a coating composition for ultra-thin glass according to any one of claims 2 to 4, characterized in that: In the step (b), the organosilicon-modified polyester resin and the nanofiller are ultrasonically dispersed at 35° C. to 70° C. for 20 to 50 minutes.

8. The method for preparing a coating composition for ultra-thin glass according to any one of claims 2 to 4, characterized in that: In the step (c), the ratio of the hydroxyl group of the organosilicon-modified polyester resin to the isocyanate group of the curing agent is 1:0.3-1.

5.

9. The method for preparing a coating composition for ultra-thin glass according to any one of claims 2 to 4, characterized in that: In the step (d), the non-silicon leveling agent is cellulose acetate.

10. The method for preparing a coating composition for ultra-thin glass according to claim 9, characterized in that: The silicon leveling agent is added in an amount of 0.1 to 1% by weight, and the cellulose acetate is added in an amount of 3 to 5% by weight.

11. The method for preparing a coating composition for ultra-thin glass according to any one of claims 2 to 4, characterized in that: Prior to step (d), the mixture obtained in step (c) is kept at room temperature for 0 to 12 hours.

12. The method for preparing a coating composition for ultra-thin glass according to claim 11, characterized in that: Prior to step (d), the mixture obtained in step (c) was kept at room temperature for 6 hours.

13. The method for preparing a coating composition for ultra-thin glass according to claim 11, characterized in that: Prior to step (d), the mixture obtained in step (c) was kept at room temperature for 4 hours.

14. An article comprising the coating composition for ultra-thin glass according to claim 1.

15. The article according to claim 14, which is a coating film of ultra-thin glass, and the coating film has a thickness of 4 to 30 μm.

Citation Information

Patent Citations

  • Water-soluble organic silicon modified polyester resin and water-soluble coating

    CN108623797A

  • Hard coating composition and window member having hard coating layer

    CN108864938A

  • High-impact-resistance ultrathin glass cover plate and preparation method thereof

    CN112876989A

  • Printing ink applied to coated glass and application method of printing ink

    CN105238133A

  • Polyester resin used for glass substrate coating and preparation method thereof and paint

    CN110117354A