Preparation method of magnetic graphene cellulose composite material and flexible light-emitting device

Magnetic graphene cellulose composite materials were prepared by covalent cross-linking method and combined with magnetic field regulation and ITO/PET substrate spin coating process, which solved the problems of short life of OLED luminescent materials and easy to fall off, achieving high mechanical performance and stability Flexible light emitting devices suitable for smart wearable devices.

CN116575259BActive Publication Date: 2024-11-08JIAXING UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310134054.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-20
Publication Date
2024-11-08
Estimated Expiration
2043-02-20

AI Technical Summary

Technical Problem

OLED luminescent materials in existing smart wearable devices have short service life, are sensitive to air humidity, are complex in preparation process and are cost-effective, and flexible light emitting devices are prone to fall off when bent, making it difficult to meet the needs of smart wearable devices.

Method used

Magnetic graphene cellulose composite material was prepared by covalent cross-linking method, and the magnetic properties were encapsulated in graphene oxide by Fe3O4 nanoparticles, and magnetic field was regulated on cellulose filter paper. Flexibility was prepared in combination with ITO/PET substrate layer-by-layer spin coating process. Light emitting device.

Benefits of technology

After 500 bends, the illuminance of the flexible light emitting device is reduced to only the initial 98%, maintaining the luminous brightness of more than 98%, and simplifying the preparation process, reducing costs, and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116575259B_ABST
    Figure CN116575259B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a magnetic graphene-cellulose composite material and its application in a flexible light-emitting device, wherein the preparation method includes the preparation of Fe3O4 nanoparticles, amination of Fe3O4 nanoparticles, and preparation of a co-crosslinking magnetic graphene-cellulose composite material: adding covalently crosslinked magnetic graphene oxide into water to prepare a covalently crosslinked magnetic graphene oxide dispersion, wherein the Fe3O4 in the magnetic graphene oxide prepared by the covalently crosslinking method is all wrapped by graphene oxide; placing cellulose filter paper in the covalently crosslinked magnetic graphene oxide solution, impregnating it under magnetic field regulation, and drying and reducing it. The magnetic field regulation makes the magnetic graphene-cellulose composite material have good electrical conductivity. The composite material is used as an electrode, and the electrode, dielectric layer, light-emitting layer and ITO / PET substrate are combined together by layer-by-layer assembly through a spin coating process. The preparation method is simple and fast, easy to apply and suitable for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphene composite materials, in particular to a preparation method of a magnetic graphene-cellulose composite material and a flexible light-emitting device. Background Art

[0002] Polymer nanocomposite is a composite material with polymer as matrix continuous phase and nanometer-scale filler as dispersed phase. The polymer as matrix is ​​organic, and the nanometer particles, nanometer tubes, etc. as fillers are generally inorganic. Therefore, polymer nanocomposite is generally organic phase-inorganic phase composite. There is a wider interface area between the filler and the matrix of polymer nanocomposite. Therefore, even at low concentration (usually less than 5vol%), nanometer-scale filler can significantly improve the performance of composite material, thereby will not have adverse effect on the processing performance of polymer.

[0003] Nano-scale fillers for polymers are mainly inorganic minerals. Dispersing them in polymers as fillers will greatly improve the performance of polymers. They can improve the original properties of polymers such as tensile strength, elongation at break, wear resistance, thermal stability, rheology, etc., or bring new properties such as flame retardancy, water repellency, electrical conductivity, thermal conductivity, etc. Among them, graphene, carbon nanotubes, nano-carbon fibers and other carbon nanofillers are currently the research hotspots in the scientific community. The orientation of nanoparticles in polymers is often random.

[0004] With the rapid development of smart wearables in recent years, smart displays have become an indispensable part of smart wearable devices

[100] . Currently, the organic light-emitting diode (OLED) solution is widely used. However, in smart wearables, various devices are generally prepared with textiles as the substrate. The surface of the fabric is rough, the yarns are interwoven with gaps, and the flexibility of the fabric is provided by its deformation. OLED requires the substrate to be flat at the nanoscale, and the fabric will affect the uniformity of the OLED layer during preparation. There are currently some solutions that pre-deposit a smooth functional film on the surface of the fabric and then adhere the fabric. However, there are still some problems. The OLED preparation process is complicated and costly; the OLED luminescent material has a shorter service life than other luminescent materials; in addition, both OLED and textile substrates are flexible, and both will fall off after a certain number of bends; OLED materials are sensitive to air humidity and affect display, etc. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a magnetic graphene-cellulose composite material, wherein Fe3O4 in the magnetic graphene oxide prepared by a covalent crosslinking method is encapsulated by GO. The relative content of iron in the magnetic graphene oxide is greatly increased, and the magnetism of the sample is sharply increased. The relative content of carbon is reduced, and the oxygen-containing functional groups are reduced during the preparation, but the aromaticity thereof becomes greater.

[0006] Another object of the present invention is to prepare a flexible light-emitting device with excellent mechanical properties and stability. It is stable during 500 bends, and after bending, the illuminance is reduced from the initial 60.03 lux to 58.92 lux, and the flexible electroluminescent device still maintains more than 98% of the luminous brightness.

[0007] To solve the above technical problems, the purpose of the present invention is achieved as follows:

[0008] The method for preparing the magnetic graphene-cellulose composite material involved in the present invention comprises the following steps:

[0009] Step 1, preparation of Fe3O4 nanoparticles: adding sodium hydroxide into deionized water, and heating to 80°C with stirring to obtain a sodium hydroxide solution;

[0010] FeCl3·6H2O, FeCl2·4H2O and hydrochloric acid are added to the sodium hydroxide solution and mixed evenly; the mixture is reacted for a set time under the protection of ammonia gas, vacuum filtered, washed until the pH value is 7, and dried to obtain Fe3O4 nanoparticles;

[0011] Step 2, amination of Fe3O4 nanoparticles: the Fe3O4 nanoparticles prepared in the previous step are dispersed in 3-aminopropyltriethoxysilane, and then added to an organic solvent and mixed evenly; then heated in an oil bath, and condensed and refluxed to complete the reaction; then the product is washed, vacuum filtered, and vacuum dried to obtain amination of Fe3O4 nanoparticles.

[0012] Step 3, preparation of magnetic graphene oxide by covalent cross-linking method: taking a certain amount of graphene oxide to prepare a graphene oxide dispersion; adding N-hydroxysuccinimide and 1-ethyl-3-dimethylaminopropylcarbodiimide hydrochloride to the graphene oxide dispersion, stirring evenly, then adding amino Fe3O4 nanoparticles, stirring evenly, to obtain co-cross-linked magnetic graphene oxide;

[0013] Step 4. Preparation of co-crosslinked magnetic graphene-cellulose composite material: adding covalently crosslinked magnetic graphene oxide into water to prepare a covalently crosslinked magnetic graphene oxide dispersion; placing cellulose filter paper in the covalently crosslinked magnetic graphene oxide solution and immersing it under magnetic field control, taking it out, drying it, and reducing it to obtain a co-crosslinked magnetic graphene-cellulose composite material.

[0014] On the basis of the above scheme and as a preferred scheme of the above scheme: in step 1, 5 g of sodium hydroxide is added to 250 mL of deionized water, heated to 80°C in a heating magnetic stirrer, 6.75 g of FeCl3·6H2O, 2.48 g of FeCl2·4H2O, 25 mL of deionized water and 0.83 mL of hydrochloric acid are respectively added to the sodium hydroxide solution, after mixing evenly, put into a three-necked flask, react for 1 hour under the protection of ammonia, vacuum filter, wash the product with water and methanol in turn until the pH is 7; and vacuum dry at 50°C to obtain Fe3O4 nanoparticles.

[0015] On the basis of the above scheme and as a preferred scheme of the above scheme: in step 2, 1 g of the prepared Fe3O4 nanoparticles is dispersed in 5.4 ml of 3-aminopropyltriethoxysilane; then added to a mixed solvent of methanol and toluene and mixed evenly, added to a three-necked flask, heated to 110°C in an oil bath, condensed and refluxed for 10 hours to complete the reaction; the product is washed with methanol 2-3 times, repeatedly vacuum filtered, and vacuum dried at 50°C to obtain amino Fe3O4 nanoparticles.

[0016] On the basis of the above scheme and as a preferred scheme of the above scheme: in step 3, a certain amount of graphene oxide is prepared into a 0.6% graphene oxide dispersion by ultrasonic treatment for 10 hours; the amination Fe3O4 nanoparticles prepared in the previous step are taken, wherein the weight ratio of the graphene oxide dry powder to the amination Fe3O4 is 85:15;

[0017] Take 100 mL of 0.6% GO solution, add 0.001-0.1 g of EDC and 0.0001-0.01 g of NHS at room temperature, stir evenly, then add Fe3O4 nanoparticles, stir for 15-30 minutes to obtain covalently cross-linked magnetic graphene oxide.

[0018] On the basis of the above scheme and as a preferred scheme of the above scheme: in step 4, the prepared co-crosslinked magnetic graphene oxide is added with a certain amount of water to form a co-crosslinked magnetic graphene oxide dispersion with a concentration of 0.6%, and a cellulose filter paper is placed in a square container and immersed in the co-crosslinked magnetic graphene oxide dispersion, and a magnet is used for direction control;

[0019] The process is performed by dipping for 5-30 minutes each time under the control of a magnetic field, taking out and drying in an oven at 80-100° C. for 20-60 minutes, and the dipping and drying are repeated for multiple times to complete the preparation; all the obtained products are reduced to obtain a magnetic graphene cellulose composite material.

[0020] On the basis of the above scheme and as a preferred scheme of the above scheme: the reduction is to reduce the co-crosslinked magnetic graphene oxide using HI steam.

[0021] On the basis of the above scheme and as a preferred scheme of the above scheme: the methanol and toluene are mixed in a ratio of 50 mL:50 mL.

[0022] The present invention also relates to a flexible light-emitting device, comprising a magnetic graphene-cellulose composite material prepared by the above-mentioned preparation method, wherein a dielectric layer and a light-emitting layer are sequentially arranged on one side of the magnetic graphene-cellulose composite material; and a side of the light-emitting layer away from the dielectric layer is adhered to an ITO / PET substrate.

[0023] On the basis of the above scheme and as a preferred scheme of the above scheme: the dielectric layer is formed by mixing BaTiO3 and PB glue in a mass ratio of 0.8-1:1-1.5, stirring evenly, and then using a spin coater to spin coat the mixture on the magnetic graphene cellulose composite material at 500 rpm for 60 seconds.

[0024] On the basis of the above scheme and as a preferred scheme of the above scheme: the light-emitting layer is formed by mixing the light-emitting powder ZnS:Cu and PB glue in a mass ratio of 1-1.5:1.2-2, stirring evenly, and then using a spin coater to spin coat the light-emitting powder on top of the dielectric layer at 500rpm for 60s, with a thickness of 20-40μm, and drying the solvent at 80-100℃ to volatilize it.

[0025] The beneficial effects of the present invention are as follows: the preparation method of the magnetic graphene cellulose composite material and the flexible light-emitting device involved in the present invention adopt the magnetic graphene oxide prepared by the covalent cross-linking method, and the Fe3O4 is all wrapped by graphene oxide. The relative content of iron in the magnetic graphene oxide increases greatly, and the magnetism of the sample increases sharply. The relative content of carbon element decreases, and the oxygen-containing functional groups decrease during the preparation, but their aromaticity increases. And the parallel magnetic field regulation makes the magnetic graphene cellulose composite material have good electrical conductivity. Through the layer-by-layer spin coating process on the ITO / PET substrate, the electrode, the dielectric layer, the light-emitting layer and the ITO transparent electrode are combined together by layer-by-layer assembly. The preparation method is simple and fast, easy to apply and suitable for mass production. The flexible light-emitting device has excellent mechanical properties and stability. It is stable during 500 bendings. After bending, the illuminance is reduced from the initial 60.03lux to 58.92lux, and the flexible electroluminescent device still maintains more than 98% of the luminous brightness. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a process flow chart of the preparation method of the magnetic graphene cellulose composite material involved in the present invention;

[0027] Figure 2It is the structural characterization diagram of the prepared GO; wherein ac is the TEM image of GO at different magnifications, d is the SEM image of GO, and e is the EDS element distribution of GO.

[0028] Figure 3 These are the infrared spectrum, Raman spectrum and XRD spectrum of the prepared GO, where a is the infrared spectrum of GO; b is the Raman spectrum of GO; and c is the XRD spectrum of GO.

[0029] Figure 4 The following are the SEM images, TEM images, SEM images and EDS element distribution images of MCG induced by magnetic field. (a) and (b) SEM images of MCG induced by magnetic field at different magnifications; (c) TEM image of MCG; (d) SEM image of MPG; (e) EDS element distribution image.

[0030] Figure 5 These are the infrared spectrum, Raman spectrum and XRD spectrum of MCG, where (a) is the infrared spectrum of MCG; (b) is the Raman spectrum of MCG; and (c) is the XRD spectrum of MCG.

[0031] Figure 6 This is the relationship curve between the square resistance of the MrCG-CEL composite material without magnetic field arrangement and the MrCG-CEL composite material with parallel magnetic field arrangement and the number of times of immersion in MCG dispersion liquid.

[0032] Figure 7 It is the structural analysis diagram of MrCG-CEL. Among them, (a) the full XPS spectra of MCG-CEL, MrCG-CEL and the original sample; (b) the C1s spectrum of MCG-CEL XPS; (c) the C1s spectrum of MrCG-CEL XPS; (d) the thermogravimetric diagram of MrCG-CEL induced by magnetic field, MrCG-CEL without magnetic field induction and the original sample; (e) the Raman spectrum test curves of rGO-CEL, GO-CEL, MrCG-CEL and MCG-CEL; (f) the XRD test curves of MCG and GO; (g) the XRD test curves of GO-CEL, unarranged MCG-CEL, arranged MCG-CEL and arranged MrCG-CEL. Figure 8 is a schematic diagram of the structure of a flexible light-emitting device;

[0033] Fig. 9The figures are morphological diagrams of flexible light-emitting devices; (a) cross-sectional fluorescence image of flexible electroluminescent device; (b) cross-sectional SEM image of flexible electroluminescent device; (c) device photograph of the working color of the flexible electroluminescent device changing from dark to bright with MrCG-CEL electrodes of different resistance as substrates; (d) cross-sectional diagram of MrCG-CEL electrode; (e) cross-sectional diagram of the dielectric layer attached to the MrCG-CEL electrode; (f) cross-sectional diagram of the light-emitting layer attached to the dielectric layer; (g) cross-sectional diagram of ITO / PET transparent electrode.

[0034] Fig.10 It is a performance analysis diagram of MrCG-CEL composite materials arranged in four different directions: uninduced, induced by parallel straight magnetic lines, induced by parallel closed magnetic lines, and induced by vertical closed magnetic lines; among them, (a) schematic diagram of the preparation of MrCG-CEL electrodes without magnetic field induction; (b) schematic diagram of the preparation of MrCG-CEL electrodes induced by parallel straight magnetic lines; (c) schematic diagram of the preparation of MrCG-CEL electrodes induced by parallel closed magnetic lines; (d) schematic diagram of the preparation of MrCG-CEL electrodes induced by vertical closed magnetic lines; (e) illumination diagram of flexible electroluminescent devices prepared by MrCG-CEL electrodes arranged in four different directions; (f) CIE1931 coordinate diagram of flexible electroluminescent devices prepared by MrCG-CEL electrodes arranged in four different directions; (g) normalized spectrum diagram of flexible electroluminescent devices prepared by MrCG-CEL electrodes arranged in four different directions

[0035] Fig.11 This is a comparison chart of the illumination of flexible electroluminescent devices prepared by MrCG-CEL electrodes without magnetic field induction and MrCG-CEL electrodes induced by parallel straight magnetic lines under different driving voltages.

[0036] Fig.12 This is a comparison chart of illumination data of a flexible light-emitting device that is not induced by a magnetic field and a flexible light-emitting device that is induced by parallel straight magnetic lines of force.

[0037] Fig.13 The illumination of a flexible electroluminescent device induced by parallel straight magnetic lines of force changes with the number of bends. DETAILED DESCRIPTION

[0038] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0039] The method for preparing the magnetic graphene-cellulose composite material involved in the present invention comprises the following steps:

[0040] Step 1: Preparation of Fe3O4 nanoparticles: Add sodium hydroxide into deionized water, and heat to 80°C with stirring to obtain a sodium hydroxide solution.

[0041] FeCl3·6H2O, FeCl2·4H2O and hydrochloric acid are added to a sodium hydroxide solution and mixed evenly; the solution is reacted for a set time under the protection of ammonia gas, vacuum filtered, washed until the pH value is 7, and dried to obtain Fe3O4 nanoparticles.

[0042] Step 2, amination of Fe3O4 nanoparticles: the Fe3O4 nanoparticles prepared in the previous step are dispersed in 3-aminopropyltriethoxysilane, and then added to an organic solvent and mixed evenly; then heated in an oil bath, and condensed and refluxed to complete the reaction; then the product is washed, vacuum filtered, and vacuum dried to obtain amination of Fe3O4 nanoparticles.

[0043] Step 3. Preparation of covalently cross-linked magnetic graphene oxide: take a certain amount of graphene oxide to prepare a graphene oxide dispersion; add N-hydroxysuccinimide and 1-ethyl-3-dimethylaminopropylcarbodiimide hydrochloride to the graphene oxide dispersion, stir evenly, then add amino Fe3O4 nanoparticles, stir evenly, and obtain co-cross-linked magnetic graphene oxide.

[0044] Step 4. Preparation of co-crosslinked magnetic graphene-cellulose composite material: adding covalently crosslinked magnetic graphene oxide into water to prepare a covalently crosslinked magnetic graphene oxide dispersion; placing cellulose filter paper in the covalently crosslinked magnetic graphene oxide solution and immersing it under magnetic field control, taking it out, drying it, and reducing it to obtain a co-crosslinked magnetic graphene-cellulose composite material.

[0045] Specifically, in step 1, 5 g of sodium hydroxide is added to 250 mL of deionized water, which is heated to 80° C. in a heating magnetic stirrer, 6.75 g of FeCl3·6H2O, 2.48 g of FeCl2·4H2O, 25 mL of deionized water and 0.83 mL of hydrochloric acid are respectively added to the sodium hydroxide solution, mixed evenly and put into a three-necked flask, reacted for 1 hour under the protection of ammonia, vacuum filtered, and the product is washed with water and methanol in turn until the pH is 7; and vacuum dried at 50° C. to obtain Fe3O4 nanoparticles.

[0046] Specifically, in step 2, 1 g of the prepared Fe3O4 nanoparticles is dispersed in 5.4 ml of 3-aminopropyltriethoxysilane; then added to a mixed solvent of methanol and toluene and mixed evenly, added to a three-necked flask, heated to 110° C. in an oil bath, condensed and refluxed for 10 hours to complete the reaction; the product is washed with methanol 2-3 times, repeatedly vacuum-filtered, and vacuum-dried at 50° C. to obtain amination Fe3O4 nanoparticles. The methanol and toluene are mixed in a ratio of 50 mL:50 mL.

[0047] Specifically, in step three, a certain amount of graphene oxide is prepared into a 0.6% graphene oxide dispersion by ultrasonic treatment for 10 hours; the amination Fe3O4 nanoparticles prepared in the previous step are taken, wherein the mass ratio of the graphene oxide dry powder to the amination Fe3O4 is 85:15.

[0048] Take 100 mL of 0.6% GO solution, add 0.001-0.1 g of EDC and 0.0001-0.01 g of NHS at room temperature, stir evenly, then add Fe3O4 nanoparticles, stir for 15-30 min to prepare covalent cross-linked magnetic graphene oxide. In this embodiment, add 0.001 g of EDC and 0.0001 g of NHS, stir evenly, then add Fe3O4 nanoparticles, stir for 15 min.

[0049] Furthermore, the reduction is to reduce the co-crosslinked magnetic graphene oxide using HI steam.

[0050] In step three, graphene oxide is prepared by the improved Humans method, and magnetic graphene oxide is prepared by the coprecipitation method, and the microscopic morphology and structure of graphene oxide and magnetic graphene oxide are analyzed by instruments such as SEM, TEM, and XRD. The graphene used is produced by Shanghai Aladdin Biochemical Technology Co., Ltd., with a carbon content of 99.95% and a particle size of 8000 mesh. The experimental drugs used are shown in Table 1.

[0051] Table 1 Experimental drugs

[0052]

[0053]

[0054] The experimental instruments and equipment used are shown in Table 2.

[0055] Table 2 Experimental instruments and equipment

[0056]

[0057] The preparation of the graphene oxide comprises the following steps:

[0058] S1. Pre-oxidized graphite: add 5g of potassium persulfate and 5g of graphite into a beaker and stir, add 50mL of concentrated sulfuric acid and stir for 5min, then add 5.5g of phosphorus pentoxide and stir evenly; heat to 80°C and heat for 5h; cool to room temperature and slowly add 200mL of deionized water; let stand and settle to separate, then absorb the upper clear liquid, repeat the operation four to five times, wash the clear liquid until the pH is neutral, filter it, dry it at 50°C for 24h, and obtain the product pre-oxidized graphite.

[0059] S2. Preparation of graphene oxide: Add crushed ice to a heated magnetic stirrer to lower the temperature to 0°C, put it in a beaker, add 46mL of concentrated sulfuric acid and 1g of sodium nitrate, stir, react for 2h, add 2g of pre-oxidized graphite prepared in the first step, and then slowly add 6g of KMnO4; after reacting at 0°C for 2h, remove the crushed ice and raise the temperature to 45°C, and react for 30min; after the reaction is completed, add a total of 92mL of deionized water twice, add quickly the first time, and add slowly the second time; continue to react for 30min. After cooling to room temperature, add 280mL of deionized water and 10mL of 30% H2O2 solution from dark red to bright yellow to react for 15min; after standing, pickle with hydrochloric acid diluted to 5%, then wash and centrifuge for multiple times until the pH is neutral. Use a freeze dryer to freeze-dry for 24h to obtain graphene oxide.

[0060] GO was tested by transmission electron microscopy, scanning electron microscopy and EDS element distribution, such as Figure 2 As shown, through the SEM image, we can see that there are a lot of wrinkles on the GO. In the TEM image, there are also a lot of wrinkles on the edge of the GO. The relatively flat surface also has such wavy wrinkles. This kind of wrinkle is a natural property of two-dimensional materials, which is consistent with the description in related research. The size of the prepared graphene oxide sheet is 10-15μm. Related research believes that the wrinkled structure is a site that is easier to adsorb substances and react. From the EDS energy spectrum, Figure 2 It can be seen from Figure e that the carbon content of the prepared graphene oxide is the highest among all elements, accounting for 59.97% by mass. The oxygen content is 40.03%, indicating that there are a large number of oxygen-containing functional groups in GO.

[0061] GO was tested by infrared spectroscopy, Raman spectroscopy and XRD. The test results are shown in Figure 3 Infrared absorption spectra mainly judge the possible functional groups by the position of the absorption peak. -1 There is an absorption peak with strong intensity and wide width at 1725cm -1 The sharp peak at 1620 cm-1 is attributed to the C=O in the -COOH group. -1 The stretching vibration peaks of C=C on the benzene-like ring structure in graphene oxide correspond to the vibrations of carboxyl (OC=O), epoxy (CO) and alkoxy (CO) at 1401 cm -1 、1202cm -1 and 1045cm -1 At the same time, the oxygen-containing groups in graphene oxide are abundant.

[0062] Raman spectroscopy is often used to characterize the degree of defects and structural information of carbon materials.1 The peak formed at 1600cm is called D peak, which is caused by lattice vibration. Generally speaking, it indicates the disorder of the material, and the apparent manifestation is the wrinkles on the surface of the material. -1 The peak at is called G peak, which is due to SP 2 The vibration of carbon atoms generally indicates the regularity of the material. The ID / IG value is often used to characterize the degree of defects on the surface of carbon-based materials. As shown in the figure, it is obvious that the Raman spectrum of the GO sample has a large area at 1350cm -1 and 1588cm -1 The two characteristic peaks are both strong. The strong D peak indicates that the GO defect is large, which corresponds to the prepared sample being GO. If GO is reduced to rGO, the D peak will become weak. The G peak is the characteristic peak of GO. The strong G peak indicates that hybridized carbon atoms are generated. The ID / IG is 0.93, indicating that the defect density is small.

[0063] XRD is often used to characterize the crystal structure of graphene oxide. Figure 3 As shown. It can be seen that there is a strong diffraction peak at about 10°. According to relevant research, it can be known that it is a strong diffraction peak of GO belonging to the 001 crystal form. At about 26°, the curve is smooth and there is no diffraction peak of graphite, which shows that graphite is completely oxidized during the preparation of graphene oxide.

[0064] SEM and TEM were used to observe the magnetic graphene oxide MCG prepared by covalent cross-linking method to characterize its micromorphology. Figure 4 (a) and (b) are SEM morphology images of the oriented arrangement of synthesized MCG under magnetic field induction and SEM morphology images of synthesized MCG. Figure 4 (d) is the SEM image of MCG without magnetic field induction. It can be seen that under the induction of the magnetic field, MCG is neatly arranged into I-type folds, showing a clear groove structure. The microscopic morphology of MCG is not covered, and a clear and obvious microstructure can be seen. Figure 4 The edge of MCG in the TEM image (c) has relatively flat wrinkles, which has some morphological characteristics of GO. It can be seen from the figure that the Fe3O4 particles are wrapped by graphene oxide and oriented under the action of the magnetic field. The same arrangement effect can be seen from the SEM image. Figure 4 (a) in the figure is confirmed. From the EDS spectrum, Figure 4 In (e), it can be seen that the carbon content of the prepared MCG is 44.66%, the oxygen content is 52.70%, and the iron content is 2.64%. The mass proportion of C decreases, O increases, and Fe increases, indicating that after the iron element is introduced in the MCG preparation process, its mass proportion increases.

[0065] Figure 5(a) is the infrared spectrum of MCG. MCG is at 3575cm -1 There is an absorption peak with strong intensity and wide width at 1712 cm -1 The sharp peak at 1608 cm-1 is attributed to the C=O in the -COOH group. -1 The corresponding peak is the stretching vibration of C=C on the benzene-like ring structure in graphene oxide. The vibration of alkoxy (CO) is at 1027 cm -1 At 588cm -1 The peak at is a strong vibration peak of Fe-O, indicating the lattice absorption of iron oxide. Therefore, Fe3O4 nanoparticles have been successfully loaded on graphene. Figure 2-4 The intensity of the functional groups in graphene oxide in (a) is slightly lower than that of -OH, C=O, and CO, 1608 cm -1 The peak intensity of CC at increased, indicating that the oxygen-containing groups decreased during the synthesis of MCG.

[0066] Figure 5 (b) shows the Raman spectrum of MCG. Obviously, the Raman spectrum of the sample has a peak at 1346 cm -1 and 1598cm -1 There are two characteristic peaks at the bottom, corresponding to the D peak and the G peak. The intensity ratio of the D peak to the G peak (ID / IG) is related to the degree of defects on the graphene surface and the size of the sp2 hybrid domain. I2D / IG is often used to infer the number of graphene layers. As the ratio decreases, the more and thicker the graphene layers are. Figure 5 In (b), it can be seen that the I2D / IG of GO is 0.29. Figure 5 The I2D / IG of MCG in (b) is 0.26. It means that the thickness of prepared MCG increases. After GO is covalently cross-linked with Fe3O4 to become MCG, the ID / IG value increases from 0.93 to 0.97, indicating that the defect structure on the surface of MCG increases during the covalent cross-linking process. 2 The hybrid domains increase, but their sizes decrease, which indicates that the aromatized domains formed during the preparation process are smaller but more numerous, and the MCG surface contains more defect structures.

[0067] XRD spectra are used to reveal the crystal structure of MPG particles. Figure 5In the spectrum of the MPG spectrum shown in (c), the diffraction peaks with 2θ values ​​of 30.2° and 35.6° correspond to the (220) and (311) crystal planes of Fe3O4, respectively, indicating that the Fe3O4 supported on the graphene sheet has a pure cubic spinel crystal structure

[66] . (Since the amount of Fe supported is relatively small, the role of Fe in this experiment is to orient GO, so some of the Fe crystal forms are not obvious in XRD.) It can be seen from the figure that compared with the XRD diffraction pattern of GO, MCG has shifted to the left as a whole, because the sample is doped with Fe, and the impurity atoms will increase or decrease the unit cell parameters. The left shift indicates that the unit cell parameters are increased and the interplanar spacing is increased.

[0068] Specifically, in step 4, the prepared co-crosslinked magnetic graphene oxide is added with a certain amount of water to form a co-crosslinked magnetic graphene oxide dispersion with a concentration of 0.6%, a cellulose filter paper is placed in a square container and immersed in the co-crosslinked magnetic graphene oxide dispersion, and a magnet is used for direction control;

[0069] The impregnation is carried out for 5-30 minutes each time under the control of the magnetic field, and the impregnation is carried out in an oven at 80-100°C for 20-60 minutes, and the impregnation and drying are repeated for multiple times to complete the preparation; all the obtained products are reduced to obtain a magnetic graphene cellulose composite material. In this embodiment, the impregnation is carried out for 5 minutes each time under the control of the magnetic field, and the impregnation is carried out in an oven at 100°C for 30 minutes.

[0070] The cellulose filter paper used was Jiejie brand 202 model cellulose filter paper. The experimental drugs used are shown in Table 3.

[0071] Table 3 Experimental drugs

[0072]

[0073] The experimental instruments and equipment used are shown in Table 4.

[0074] Table 4 Experimental instruments and equipment

[0075]

[0076]

[0077] The conductive properties of magnetic graphene-cellulose composites were analyzed. Figure 6It can be seen that the square resistance of MrCG-CEL composite material decreases with the increase of impregnation times, and the conductive performance gradually improves. The square resistance of MrCG-CEL composite material induced by magnetic field is smaller than that of MrCG-CEL composite material without magnetic field induction under the same number of impregnations. It shows that the oriented arrangement of MrCG on cellulose fibers makes MrCG particles interconnected to form a more compact and coherent network. This proves that oriented MrCG more effectively improves the conductive performance of MrCG-CEL composite material.

[0078] Without alignment, the probability of contact between adjacent MCGs is low, thus limiting the conductivity of the composite. Magnetic field induction overcomes this obstacle due to the interaction between induced dipoles. In the present composite, the magnetic field induces MCG alignment, and then an attractive force is generated between the aligned MCGs, which increases the effective aspect ratio of the MCG polymer composite. This increased effective aspect ratio reduces the percolation threshold. In addition, the conductive paths between MCGs may be located not only in the direction of the magnetic field, but also between materials aligned through lateral contacts. The connection of MCGs to adjacent points to form short chains is the reason for the relatively high conductivity of the composite in the direction perpendicular to the orientation field.

[0079] In addition, it can be seen that the square resistance value remains basically unchanged after repeating the immersion and drying process 6 times. This is because the adsorption amount tends to saturation with the increase in the number of immersion times, forming an effective arrangement and connection of the three-dimensional conductive network MCG.

[0080] MrCG-CEL structural analysis, see Figure 7 The prepared samples were tested using an X-ray photoelectron spectrometer. The full XPS spectra of magnetic field-induced MCG-CEL, MrCG-CEL and original samples are shown in Figure 7 As shown in (a) in the figure. Obvious Fe 2p peaks, C 1s peaks and O1s peaks can be observed from the XPS full spectrum, indicating that the magnetic graphene surface contains Fe, C and O elements, and their relative contents are shown in Table 5. When MCG is reduced to MrCG, the relative content of O element in the composite material decreases from 30.87% to 14.70%, indicating that the oxygen-containing functional groups decrease during the reduction process. The grafting of amination Fe3O4 nanoparticles on the cellulose paper matrix is ​​further confirmed by the presence of Fe2p peaks in the full spectrum ( Figure 7 The C1s spectra of MCG-CEL and MrCG-CEL are shown in Figure 2. Figure 7As shown in (b) and (c) of FIG. 3 , the XPS C 1s results of MrCG-CEL after reduction show that it has four obvious fitting peaks at 284.7 eV, 285.5 eV, 286.6 eV and 287.6 eV, corresponding to C=C, CN, C=O and O=CO. Compared with MCG-CEL before reduction, the content of C=C (284.7 eV) and CN (285.5 eV) functional groups after reduction increases, while the content of C=O (286.6 eV) and O=CO (287.6 eV) functional groups decreases (see Figure 7 (b) and (c) XPS and Tables 5 and 6), they further demonstrated the effective chemical reduction and successful grafting of Fe nanoparticles.

[0081] like Figure 7 As shown in (d) in Figure 2, the composition of MrCG-CEL with and without magnetic field regulation was characterized by TGA under nitrogen environment. For both MrCG-CEL samples with and without magnetic field regulation, a slow weight loss (5.98wt%) at low temperature (<100℃) was observed, which can be attributed to the loss of residual or absorbed solvent. A stage of weight loss occurred at 150℃ for both samples, indicating the decomposition and evaporation of various functional groups at different positions on MrGO and MCG. Then, a large amount of weight loss occurred at 225℃ for MrCG-CEL with magnetic field regulation and at 239℃ for MrCG-CEL without magnetic field regulation. According to the comparison with the thermogravimetric curve of the original sample, it was the weight loss caused by the decomposition of the substrate. The weight loss stages of the two samples at around 293℃ and 313℃, respectively, may be attributed to the decomposition of the –COO groups in MrCG and MCG coordinated with Fe3O4 nanoparticles. Similar results were also observed for the preparation of polymer / Fe3O4 magnetic microspheres. When the temperature reaches 750℃, the weight of the two samples of MrCG-CEL remains at 32.1wt% and 22.3wt%, and there is almost no weight loss after this temperature. At the same time, according to the comparison of the original sample without any treatment, it is found that the thermogravimetric curve of the original sample is a typical thermogravimetric curve of cellulose paper, with a large amount of weight loss at around 300℃ and almost zero weight after the final decomposition.

[0082] Figure 7 (e) shows the Raman spectra of rGO-CEL, GO-CEL, MrCG-CEL and MCG-CEL before and after reduction. Obviously, the Raman spectra of the four samples have a peak at 1360 cm -1 and 1600cm -1Two characteristic peaks are shown at the surface, corresponding to the D peak and the G peak. The intensity ratio of the D peak and the G peak (ID / IG) is related to the degree of defects on the graphene surface and the size of the sp2 hybrid domain. Compared with MCG-CEL (0.90), the ID / IG ratio of MrCG-CEL increases after reduction (1.22); after GO is chemically reduced to rGO, the ID / IG value increases from 0.91 to 1.08, indicating that the defect structure on the MrCG surface increases during the reduction process. Although the sp2 hybrid domain increases, the size decreases. This indicates that the aromatization areas formed during the reduction process are smaller but more numerous, and the MrCG surface contains more defect structures.

[0083] The XRD spectra of MCG, GO and GO-CEL, unaligned MCG-CEL, aligned MCG-CEL and aligned MrCG-CEL are shown in Figure 7 As shown in (f) and (g) in the figure. XRD spectra are used to reveal the crystal structure of MCG particles and MrCG-CEL. In the spectrum of MCG particles, the diffraction peaks with 2θ values ​​of 30.2° and 35.6° correspond to the (220) and (311) crystal planes of Fe3O4, respectively, indicating that the Fe3O4 supported on the graphene sheet has a pure cubic spinel crystal structure

[66] . (Since the amount of Fe loaded is relatively small, the role of Fe in this experiment is to orient GO, so some crystal forms of Fe are not obvious in XRD.) Figure 7 It can be seen from (g) that compared with GO-CEL, the XRD spectra of MCG-CEL, MCG-CEL and MrCG-CEL have shifted to the left as a whole, because these three samples are doped with Fe. The impurity atoms will make the unit cell parameters larger or smaller. If they shift to the left, it means that the unit cell parameters have increased and the interplanar spacing has increased. The main diffraction peaks of cellulose paper are located at 2θ=14.8, 16.6, 22.8 and 34.5, corresponding to the (101), (107), (002) and (040) crystal planes of cellulose I, respectively. The 101-type crystal plane of C is located at 2θ=11.1. Compared with the four samples, the samples doped with Fe have shifted to the left, and the 001-type crystal plane disappears in the reduced sample.

[0084] Table 5 Elemental composition of MCG-CEL and MrCG-CEL induced by magnetic field

[0085]

[0086] Table 6 Bonding of C elements in MCG-CEL and MrCG-CEL induced by magnetic field

[0087]

[0088] The present invention also relates to a flexible light-emitting device, comprising a magnetic graphene-cellulose composite material 1 prepared according to the above-mentioned preparation method, wherein a dielectric layer 2 and a light-emitting layer 3 are sequentially arranged on one side of the magnetic graphene-cellulose composite material 1; and the side of the light-emitting layer 3 away from the dielectric layer 2 is adhered to an ITO / PET substrate 4.

[0089] Furthermore, the dielectric layer 2 is formed by mixing BaTiO3 and PB glue at a mass ratio of 0.8-1:1-1.5, stirring evenly, and then using a spin coater to spin coat the mixture at 500 rpm for 60 seconds on the magnetic graphene cellulose composite material. The thickness of the formed dielectric layer 2 is 40 μm, and then drying at 100° C. for 2 hours to volatilize the solvent. The dielectric layer 2 is used to prevent voltage breakdown of the device. In this embodiment, BaTiO3 and PB glue are mixed at a mass ratio of 1:1.

[0090] Further, the light-emitting layer 3 is formed by mixing the light-emitting powder ZnS:Cu and PB glue in a mass ratio of 1-1.5:1.2-2, stirring evenly, and then using a spin coater to spin-coat the light-emitting powder on the dielectric layer 2 at 500rpm for 60s, with a thickness of 20-40μm, and drying at 80-100℃ for 2 hours to volatilize the solvent. The light-emitting layer 3 is used for electroluminescence. In this embodiment, ZnS:Cu and PB glue in the light-emitting layer 3 are mixed in a mass ratio of 1:1.5, with a thickness of 40μm, and dried at 100℃ for 2 hours.

[0091] The conductive surface of the cleaned ITO / PET substrate is adhered to the light-emitting layer to prepare a flexible electroluminescent device, the structure of which is as follows: Figure 8 shown.

[0092] The flexible light-emitting device formed was analyzed. The structure and photos of the flexible light-emitting device prepared using the MrCG-CEL composite material are shown in Fig. 9 As shown. The device consists of electrodes formed by a flexible ITO / PET substrate and a MrCG-CEL composite material with a light-emitting layer sandwiched in between. The light-emitting layer is prepared by embedding ZnS:Cu phosphors doped with different metals into various flexible polymer matrices with different dielectric constants. As a prototype device, ZnS:Cu phosphors are dispersed in polyisobutylene (PB) to form a blue light-emitting layer. The device is manufactured by a simple spin coating method, and the detailed manufacturing process is described in the experimental section. Fig. 9 As shown in (b), the cross-sectional image of the sample taken with a scanning electron microscope (SEM) verifies the layer-by-layer stacking structure of the obtained device. The image also shows a clear interface and close contact between two adjacent layers ( Fig. 9 (d), (e), (f) and (g) in ). Fig. 9(a) shows a cross-sectional fluorescence image of the flexible electroluminescent device. These results also show the layer-by-layer stacking of the obtained device, with close contact between two adjacent layers. Fig. 9 (d) is a cross-sectional view of the MrCG-CEL composite electrode. It can be seen from the figure that the fiber roots intersect with numerous gaps, which is conducive to the adsorption of MCG and adhesion to the dielectric layer. Fig. 9 (e) is a cross-sectional view of the dielectric layer attached to the MrCG-CEL composite electrode, and the dielectric layer thickness is about 50 μm. It can be seen from the figure that the dielectric powder BaTiO3 is evenly dispersed in polyisobutylene and evenly coated on the MrCG-CEL composite material, and it is tightly combined with the MrCG on the electrode surface. Fig. 9 (f) is a cross-sectional view of the light-emitting layer attached to the dielectric layer. The figure shows that the ZnS:Cu phosphor with an average diameter of about 25μm is evenly distributed in the PB glue, the thickness of the blue emission layer is about 40μm, and the dielectric layer and the light-emitting layer use the same adhesive, so the two layers are more tightly bonded due to the formation of chemical bonds. Fig. 9 (g) is a cross-sectional view of the ITO / PET transparent electrode, which serves as the top electrode and is in close contact with the light-emitting layer and has good interconnection.

[0093] Under an alternating electric field, metal-doped ZnS phosphors emit light due to the radiation relaxation of the luminescent center. When the bottom electrode resistance is different, the intensity and brightness of the light emitted are also different, such as Fig. 9 As shown in (c) in . Fig. 9 (c) in the figure shows the luminescence of the flexible light-emitting device prepared by electrodes prepared by dipping MCG from one to six times. It can be seen that the brightness gradually changes from dark to bright during operation. When the number of dipping times is small, the resistance of the electrode after reduction is large, and the flexible light-emitting device is easily broken down under the same excitation voltage.

[0094] Fig.10 (a) in the figure has not been induced to arrange by any directional magnetic field. From the embedded image on the upper right (the actual luminescence picture of the device prepared), it can be seen that its luminescence is random and non-directional. From the embedded image on the lower right (MrCG-CEL SEM picture), it can be seen that the MCG distribution on it has no directionality. Fig.10 (b) is induced by parallel linear magnetic lines of force. From the inset picture on the upper right, it can be seen that the luminescence is directional, emitting light parallel to the direction of the magnetic field. From the inset SEM picture on the lower right, it can be seen that the MCG distribution on it is directional. The GO on the MCG is attached to the cellulose fiber, and the Fe3O4 is arranged linearly on the GO. The directionality of it as an electrode is further reflected in the flexible light-emitting device. Fig.10(c) in the figure is a parallel closed magnetic line induced arrangement. From the embedded image on the upper right, it can be seen that its luminescence is directional, emitting in an arc shape along the direction of the applied magnetic field. From the embedded SEM image on the lower right, it can be seen that the MCG on it is distributed along the arc direction. Fig.10 (d) is a vertical closed magnetic line induced arrangement. From the embedded figure on the upper right, it can be seen that the direction of its light emission is the triangular aggregation area formed by the magnetic field formed by the bar magnet below on the electrode. This area has a smaller resistance and brighter light. From the SEM electron microscope image on the lower right, it can be seen that Fe3O4 is attracted by the magnetic field and moves downward, that is, inside the matrix. Observation of its surface morphology shows that unlike the other three morphologies, the surface of Fe3O4 is flatter because it is attracted from below.

[0095] The luminescence data of four flexible electroluminescent devices were tested by Yuanfang SPIC-300 spectral color illuminance meter. Fig.10 (e) is a comparison chart of the illuminance of four flexible light-emitting devices when driven by a 3V voltage driver. It can be seen from the figure that the device with parallel magnetic field induced arrangement has the highest illuminance, corresponding to the data at position 2 in the figure, and the illuminance reaches 64.74lux; followed by the device without arrangement, corresponding to the data at position 1 in the figure, and the illuminance reaches 59.15lux; the illuminance of the device with unilateral divergent magnetic field induced arrangement and the device with downward divergent magnetic field induced arrangement are 40lux and 39.7lux respectively, corresponding to No. 3 and No. 4 in the figure. The analysis shows that firstly, the resistance of the magnetic field arrangement area is small, so the obvious difference can be seen from the luminous direction in the actual picture above. Secondly, not all areas of the electrode are arranged under the influence of the magnetic field, and the unarranged areas are still the original disordered distribution, and the resistance is relatively large. All areas of the sample arranged in parallel magnetic field are arranged by the magnetic field, so its resistance is relatively small. The resistance difference leads to a specific luminescence reversal. Fig.10 (f) in the figure is the CIE1931 color coordinate diagram of the flexible electroluminescent device prepared by arranging MrCG-CEL electrodes in four different directions. It can be seen that the arrow direction in the CIE coordinate diagram moves from the light blue area to the dark blue area. The arrow directions are samples No. 4, No. 3, No. 1 and No. 2 respectively. Coordinate movement and Fig.10 The trend of the luminous illumination data in (e) is consistent. Fig.10(g) is the normalized spectrum of the flexible electroluminescent device prepared by arranging MrCG-CEL electrodes in four different directions. First, the wavelength of blue light is 440-475nm, the emission peak of sample No. 2 is at 460nm, and the emission peaks of samples No. 1, No. 3 and No. 4 are 466nm, 470nm and 487nm respectively. It can be seen that No. 2, No. 1, No. 3 and No. 4 are gradually moving towards the red light wavelength. Secondly, from the normalized intensity data in the normalized spectrum, it can be seen that the spectral intensity of sample No. 2 is the highest, followed by No. 1, No. 3 and No. 4. This shows that the flexible electroluminescent device prepared by induced arrangement of parallel linear magnetic lines of force excites the brightest blue light.

[0096] The flexible light-emitting devices without magnetic field induced arrangement and the flexible light-emitting devices induced by parallel straight magnetic lines of force were driven to emit light under different driving voltages, and their illuminance was tested. The data are as follows: Fig.11 As shown in the figure, it can be seen that as the voltage increases from 1V to 12V, the illumination of the two devices increases significantly. Comparing the illumination of the two devices at the same driving voltage, the flexible light-emitting device induced by parallel magnetic field is better than the flexible light-emitting device without magnetic field induced arrangement, which shows that the directional arrangement of electrodes is effective in increasing the illumination.

[0097] Fig.12 (a, c, e) are flexible light-emitting devices without magnetic field induced arrangement and Figure 4-7 (b, d, f) are the illumination data comparison of the flexible light-emitting device induced by parallel straight magnetic field lines. The voltage is changed at a constant 50 Hz driving frequency to compare its luminescence performance.

[0098] Fig.12 (a) and Fig.12 (b) is the illumination diagram of the two flexible electroluminescent devices at different voltages for five cycles. The device was powered on continuously at different voltages for 1 minute, turned off and paused for 5 seconds, and then the previous step was repeated five times. It can be seen that both devices remain stable at different voltages, and the illuminance values ​​do not fluctuate much. Secondly, the two devices were compared at the same voltage, and it was found that the illuminance of the flexible light-emitting device induced by parallel straight magnetic lines of force was higher than that of the flexible light-emitting device without magnetic field induced arrangement. Fig.12(c) in Figure 1 and (d) in Figure 12 are normalized electroluminescence spectra of flexible light-emitting devices that are not induced by magnetic field and flexible light-emitting devices that are induced by parallel straight magnetic field lines at different driving voltages. It can be seen from the figure that the brightness of the two light-emitting devices increases with the increase of voltage. The wavelength of the peak emission of the sample with magnetic field regulation moves from 489nm to 470nm, and the wavelength of the peak emission of the sample without magnetic field regulation moves from 488nm to 468nm, indicating that when the voltage increases, they are moving in the direction of short-wave blue light. Visually, the device emits brighter light as the voltage increases. Comparison Fig.12 It can be seen from (c) and (d) that under the same input voltage, the normalized intensity of the flexible light-emitting device induced by parallel straight magnetic lines is greater than that of the flexible light-emitting device without magnetic field control. Fig.12 (e) in 12 and (f) in 12 are CIE1931 color coordinate diagrams of flexible light-emitting devices that are not induced by magnetic field and flexible light-emitting devices that are induced by parallel straight magnetic lines of force at different driving voltages. From them, we can directly observe how the color of the electroluminescent device changes with the voltage. The luminous color of the electroluminescent device moves to the blue area with the increase of the input voltage. The color coordinate value of the flexible light-emitting device that is directional arranged at the same voltage is smaller and the blue area is deeper. In terms of luminous intensity, the illuminance of the flexible light-emitting device induced by parallel straight magnetic lines of force at different voltages is higher than that of the flexible light-emitting device that is not induced by magnetic field, and the difference between the two is more obvious; in terms of luminous color, the luminous color areas of the two are basically the same, and the luminous trends are basically the same. The flexible light-emitting device that is directional arranged is in a deeper blue area.

[0099] Fig.13 The illuminance of a flexible electroluminescent device induced by parallel linear magnetic field lines changes with the number of bending times. A stepper is used to repeatedly bend the sample at a frequency of 1 Hz, and the illuminance values ​​at different bending times are measured to characterize the stability of the device. Fig.13 The embedded figure (a) and the embedded figure (b) are digital photos of the flexible electroluminescent device before and after bending during work. It can be seen that it still works normally and emits light evenly after bending. It is driven by a 3V AC driver. It can be seen from the figure that the illuminance is stable during 500 bends. After bending, the illuminance decreases from the initial 60.03lux to 58.92lux, and the flexible electroluminescent device still maintains more than 98% of the luminous brightness. This result shows that the prepared flexible electroluminescent device has good mechanical fastness and strong bending stability. The remarkable stability of the flexible light-emitting device can be attributed to the intrinsic flexible component of the polymer matrix, which makes it reliable in practical applications. The surface light emission of the flexible electroluminescent device is uniform and soft, coupled with its flexible structure, so it has good development potential and broad application prospects in the field of flexible wearables.

[0100] The abbreviations used in this article are as follows: GO is graphene oxide; rGO is reduced graphene oxide; MrGO is magnetic reduced graphene; CEL is cellulose filter paper; MCG is covalently cross-linked magnetic graphene oxide; MCG-CEL is covalently cross-linked magnetic graphene oxide cellulose composite material; MrCG-CEL is reduced covalently cross-linked magnetic graphene oxide cellulose composite material; GO-CEL is graphene oxide cellulose composite material; rGO-CEL is reduced graphene oxide cellulose composite material.

[0101] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing a magnetic graphene-cellulose composite material, characterized in that: The steps include: Step 1, preparation of Fe3O4 nanoparticles: adding sodium hydroxide into deionized water, and heating to 80°C with stirring to obtain a sodium hydroxide solution; FeCl3·6H2O, FeCl2·4H2O and hydrochloric acid are added to the sodium hydroxide solution and mixed evenly; the mixture is reacted for a set time under the protection of ammonia gas, vacuum filtered, washed until the pH value is 7, and dried to obtain Fe3O4 nanoparticles; Step 2, amination of Fe3O4 nanoparticles: dispersing the Fe3O4 nanoparticles prepared in the previous step in 3-aminopropyltriethoxysilane, and then adding it to an organic solvent and mixing it evenly; then heating it in an oil bath, and condensing and refluxing to complete the reaction; then washing the product, vacuum filtering, and vacuum drying to obtain amination of Fe3O4 nanoparticles; Step 3, preparation of magnetic graphene oxide by covalent cross-linking method: taking a certain amount of graphene oxide to prepare a graphene oxide dispersion; adding N-hydroxysuccinimide and 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride to the graphene oxide dispersion, stirring evenly, then adding amino Fe3O4 nanoparticles, stirring evenly, to obtain covalent cross-linking method magnetic graphene oxide; Step 4. Preparation of co-crosslinked magnetic graphene-cellulose composite materials: adding covalently crosslinked magnetic graphene oxide into water to prepare a covalently crosslinked magnetic graphene oxide dispersion; placing cellulose filter paper in the covalently crosslinked magnetic graphene oxide solution and immersing it under magnetic field regulation, taking it out, drying it, and reducing it to obtain a co-crosslinked magnetic graphene-cellulose composite material; the magnetic field regulation refers to the covalently crosslinked magnetic graphene oxide being induced to arrange by parallel straight magnetic lines of force.

2. The method for preparing the magnetic graphene-cellulose composite material according to claim 1, characterized in that: In step 1, 5 g of sodium hydroxide is added to 250 mL of deionized water, heated to 80°C in a heating magnetic stirrer, 6.75 g of FeCl3·6H2O, 2.48 g of FeCl2·4H2O, 25 mL of deionized water and 0.83 mL of hydrochloric acid are respectively added to the sodium hydroxide solution and mixed evenly before being put into a three-necked flask, reacted under the protection of ammonia for 1 h, vacuum filtered, and the product is washed with water and methanol in turn until the pH is 7; and vacuum dried at 50°C to obtain Fe3O4 nanoparticles.

3. The method for preparing the magnetic graphene-cellulose composite material according to claim 1, characterized in that: In step 2, 1 g of the prepared Fe3O4 nanoparticles is dispersed in 5.4 ml of 3-aminopropyltriethoxysilane; then added to a mixed solvent of methanol and toluene and mixed evenly, added to a three-necked flask, heated to 110°C in an oil bath, condensed and refluxed for 10 h to complete the reaction; the product is washed with methanol 2-3 times, repeatedly vacuum filtered, and vacuum dried at 50°C to obtain amino Fe3O4 nanoparticles.

4. The method for preparing the magnetic graphene-cellulose composite material according to claim 1, characterized in that: In step 3, a certain amount of graphene oxide is ultrasonically treated for 10 h to prepare a 0.6% graphene oxide dispersion; the amination Fe3O4 nanoparticles prepared in the previous step are taken, wherein the weight ratio of the graphene oxide dry powder to the amination Fe3O4 is 85:15; Take 100 mL of 0.6% GO solution, add 0.1-0.001 g of EDC and 0.01-0.0001 g of NHS at room temperature, stir evenly, then add Fe3O4 nanoparticles, stir for 15-30 min to obtain covalently cross-linked magnetic graphene oxide.

5. The method for preparing the magnetic graphene-cellulose composite material according to claim 1, characterized in that: In step 4, the prepared co-crosslinked magnetic graphene oxide is added with a certain amount of water to form a co-crosslinked magnetic graphene oxide dispersion with a concentration of 0.6%, and a cellulose filter paper is placed in a square container and immersed in the co-crosslinked magnetic graphene oxide dispersion, and a magnet is used to control the direction; The process is performed by dipping for 5-30 minutes each time under the control of a magnetic field, taking out and drying in an oven at 80-100°C for 20-60 minutes, and repeating the dipping and drying process for multiple times to complete the preparation; all the obtained products are reduced to obtain a magnetic graphene cellulose composite material.

6. The method for preparing the magnetic graphene-cellulose composite material according to claim 5, characterized in that: The reduction is to reduce the co-crosslinked magnetic graphene oxide by HI steam.

7. The method for preparing the magnetic graphene-cellulose composite material according to claim 3, characterized in that: The methanol and toluene were mixed in a ratio of 50 mL:50 mL.

8. A flexible light-emitting device, characterized in that: It comprises a magnetic graphene cellulose composite material (1) prepared by the preparation method according to any one of claims 1 to 7, wherein a dielectric layer (2) and a light-emitting layer (3) are sequentially arranged on one side of the magnetic graphene cellulose composite material (1); and a side of the light-emitting layer (3) away from the dielectric layer (2) is adhered to an ITO / PET substrate (4).

9. The flexible light-emitting device according to claim 8, characterized in that: The dielectric layer (2) is formed by mixing BaTiO3 and PB glue at a mass ratio of 0.8-1:1-1.5, stirring evenly, and then using a spin coater to spin coat the mixture on the magnetic graphene cellulose composite material at 500 rpm for 60 seconds.

10. The flexible light-emitting device according to claim 8, characterized in that: The light-emitting layer (3) is formed by mixing light-emitting powder ZnS:Cu and PB glue in a mass ratio of 1-1.5:1.2-2, stirring evenly, and then using a spin coater to spin coat the light-emitting powder on the dielectric layer (2) at 500 rpm for 60 s to a thickness of 20-40 μm, and drying at 80-100° C. to volatilize the solvent.