Preparation method of coconut shell capacitor carbon for supercapacitors and coconut shell capacitor carbon and its application

Through the premixing and asphalt coating treatment of coconut shell carbonized material, low-ash asphalt and activator, coconut shell capacitive carbon with high conductivity and porous structure is formed, which solves the problems of poor conductivity and specific capacitance performance in the existing technology. , achieving high performance and simplified production process of supercapacitors.

CN116588932BActive Publication Date: 2024-10-01CHINA SHENHUA COAL TO LIQUID & CHEM CO LTD +1
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202310569946.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-10-01
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

After increasing the specific surface area of ​​existing coconut shell capacitor carbon, the conductivity and specific capacitance performance are not absolutely proportional, and the high specific surface area leads to surface defects and reduced pore structure efficiency. Conductive agents need to be added to improve conductivity, but this will affect Material uniformity and electricity storage performance.

Method used

Coconut shell carbonized material, low-ash asphalt and activator are premixed for activation pore creation, pickling to remove impurities and asphalt coating. The specific surface area and conductivity are controlled through the calcination process to form micropores-mesopores-macropores. The hierarchical porous structure reduces surface defects and improves electrical conductivity without adding conductive agents.

Benefits of technology

It achieves controllable specific surface area and high conductivity of coconut shell capacitor carbon, simplifies the production process, improves the specific capacitance and long cycle capacity retention rate of supercapacitors, and avoids the negative impact of conductive agents on material uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004238110130000151
    Figure BDA0004238110130000151
  • Figure BDA0004238110130000161
    Figure BDA0004238110130000161
Patent Text Reader

Abstract

The method for preparing coconut shell capacitor carbon for supercapacitors includes: (1) premixing raw materials, crushing and mixing coconut shell carbonized material, low-ash asphalt, and activator to obtain a premix; (2) activation and pore formation, activating the premix to obtain an activated material; (3) pickling and impurity removal, pickling, water washing and drying the activated material in sequence to obtain porous carbon; (4) asphalt coating, mixing asphalt powder with porous carbon to obtain a mixture; and then calcining the mixture to obtain asphalt-coated coconut shell activated carbon, i.e. coconut shell capacitor carbon. Also provided is the prepared coconut shell capacitor carbon and its application in the preparation of supercapacitors, electrode sheets for supercapacitors, and electrode materials for supercapacitors. In the preparation method, the raw materials are widely available, the preparation cost is low, and large-scale production is possible; the coconut shell capacitor carbon has a controllable specific surface area, high conductivity, and a micropore-mesopore-macroporous hierarchical porous structure. When the obtained coconut shell capacitor carbon is applied to supercapacitors, no conductive agent needs to be added.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparing adsorbents from electrochemical energy storage materials, and in particular relates to a preparation method of coconut shell capacitor carbon for supercapacitors and coconut shell capacitor carbon and applications. Background Art

[0002] A supercapacitor is an energy storage device between traditional capacitors and rechargeable batteries. It has the advantages of fast charging and discharging and long service life of capacitors, as well as the high energy density of secondary batteries. Therefore, it is widely used in new energy, military defense, aerospace and other fields.

[0003] Electrode materials are key factors affecting supercapacitor performance and production costs. Commonly used electrode materials include carbon materials, transition metal oxides, hydroxides, conductive polymers and their composites. Among them, carbon materials have become the focus of current supercapacitor electrode material production and research due to their advantages such as wide sources, low prices, large specific surface area, good chemical stability and high and low temperature resistance.

[0004] According to the different raw materials, capacitor carbon can be divided into different types such as biomass-based, coal-based, petroleum-based, polymer-based, etc. Among them, biomass is favored by industrial production due to its low cost and renewable advantages. Coconut shell is an important raw material for preparing biomass-based activated carbon. Its unique natural structure can provide excellent ion transmission channels for activated carbon.

[0005] At present, the commonly used coconut shell capacitor carbon is mostly activated by physical activation of CO2, water vapor or chemical activation of KOH. The literature reports that the capacitor carbon prepared by these methods usually has a capacitance of 2000m 2 Patent CN 108101054 B discloses a method for preparing capacitor carbon from coconut shells, and the surface area of ​​the finished product is as high as 2000-2200m 2 / g; Patent CN 105923634B discloses a method for preparing capacitor carbon from coconut shell fiber, and the maximum specific surface area of ​​the obtained product can reach 2898m 2 / g.

[0006] However, studies have shown that the specific capacitance and specific surface area of ​​capacitor carbon are usually not absolutely proportional. Generally, when the BET specific surface area of ​​capacitor carbon reaches 1500m 2 / g, the specific capacitance reaches its maximum value, and further increasing the specific surface area will reduce its specific capacitance. The reasons may be: (1) Although a higher specific surface area can provide a developed pore structure, it will also cause a large number of defects on its surface, resulting in an increase in its internal resistance and a decrease in conductivity; (2) A high specific surface area will also cause the framework structure of the carbon material itself to be too thin, and there will be mutual influence between adjacent active sites. Therefore, when a certain specific surface area is exceeded, a part of the "invalid" pore structure will appear. Therefore, simply increasing the specific surface area cannot effectively improve the specific capacitance. The pore size distribution, pore structure and microcrystalline structure are also key influencing factors.

[0007] In addition, the activation depth using physical methods is usually not enough, resulting in fewer effective active sites and lower specific capacitance; and chemical activation often requires subsequent acid washing, which will also introduce some heteroatoms and surface functional groups, and will also reduce the electrochemical properties of the carbon material, requiring further treatment. Patent CN 109850892B discloses a method for preparing highly conductive coconut shell activated carbon, which mentions that the method of carbonization after acid washing can well remove the functional groups on the surface of the carbon material, thereby greatly improving its conductivity. Patent CN 109592681 B discloses a method for step-by-step purification of coconut shell-based supercapacitor carbon, which uses a series of methods such as low-temperature eutectic melting of oxides, surface polishing, and reduction after acid washing to achieve the effect of removing impurities and surface functional groups of capacitor carbon, but still faces practical production problems such as cumbersome steps and long process flow.

[0008] On the other hand, due to the surface defect problem caused by the high specific surface area, a certain proportion of conductive agent is often needed to be added in the subsequent preparation of supercapacitor electrode sheets to increase its overall conductivity. However, the conductive agent itself does not provide active sites, and will also reduce the overall uniformity of the material and block some pores, thereby reducing the electrical storage performance of the carbon material.

[0009] Currently, there is no suitable method to solve the above-mentioned technical problems. Summary of the invention

[0010] The first object of the present invention is to provide a method for preparing coconut shell capacitor carbon for supercapacitors, which is simple and easy to operate, and can control the specific surface area of ​​the obtained coconut shell capacitor carbon. The obtained coconut shell capacitor carbon has a high specific surface area and good conductivity.

[0011] The second object of the present invention is to provide a coconut shell capacitor carbon prepared by the above-mentioned preparation method, wherein the coconut shell capacitor carbon has a high specific surface area and good electrical conductivity;

[0012] The third object of the present invention is to provide the use of the coconut shell capacitor carbon in the preparation of supercapacitors, electrode sheets for supercapacitors, and electrode materials for supercapacitors.

[0013] The fourth object of the present invention is to provide an electrode material for a supercapacitor made from the coconut shell capacitor carbon.

[0014] To achieve the first object of the present invention, the following technical solutions are adopted:

[0015] A method for preparing coconut shell capacitor carbon for supercapacitors comprises the following steps:

[0016] (1) Raw material premixing

[0017] The coconut shell carbonized material, low-ash asphalt and activator are crushed and mixed to obtain a premix;

[0018] (2) Activation Pore Formation

[0019] Activating the premix obtained in step (1) to obtain an activated material;

[0020] (3) Pickling and impurity removal

[0021] The activated material obtained in step (2) is sequentially acid-washed, water-washed and dried to obtain porous carbon;

[0022] (4) Asphalt coating

[0023] The asphalt powder is mixed with the porous carbon obtained in step (3) to obtain a mixture; the mixture is then calcined to obtain asphalt-coated coconut shell activated carbon, i.e., coconut shell capacitor carbon.

[0024] The method for preparing coconut shell capacitor carbon for supercapacitors of the present invention has the advantages of wide sources of raw materials, low preparation cost, and large-scale production; and the coconut shell capacitor carbon product has the advantages of controllable specific surface area, high conductivity, and a micropore-mesopore-macroporous hierarchical porous structure. When the obtained coconut shell capacitor carbon is applied to supercapacitors, no conductive agent needs to be added.

[0025] In order to improve the comprehensive performance of the prepared coconut shell capacitor carbon, in one embodiment, in step (1), the mass ratio of coconut shell carbonized material, low ash asphalt, and activator is 1: (0.25-1): (1.25-6), such as 1: (0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9 or 0.95): (1.5, 1.75, 2, 2.25, 2.5, 2.75, 3, 3.25, 3.5, 3.75, 4, 4.25, 4.5, 4.75, 5, 5.25, 5.5 or 5.75).

[0026] In one embodiment, in step (1), the coconut shell carbonized material is a coconut shell carbonized material obtained by high-temperature carbonization of coconut shell, preferably the carbonization temperature is 550-800°C, such as 575°C, 600°C, 625°C, 650°C, 675°C, 700°C, 725°C, 750°C and 775°C, and the carbonization time is 0.5-3h, such as 1h, 1.5h, 2h and 2.5h; preferably, the carbonization atmosphere is an inert gas, preferably nitrogen and / or argon.

[0027] In one embodiment, in step (1), the ash content of the low-ash asphalt is less than 0.5%, such as 0.4%, 0.3%, 0.2% and 0.1%; preferably, the low-ash asphalt includes a combination of any one or more of coal liquefaction asphalt, petroleum asphalt, coal tar, coal coke asphalt, synthetic asphalt and natural asphalt.

[0028] In one embodiment, in step (1), the activator includes any one or more combinations of potassium metal oxides (such as potassium oxide K2O, potassium oxide K2O2, potassium superoxide KO2, etc.), hydroxides (such as potassium hydroxide KOH, etc.) and their derivative salts (such as potassium chloride KCl, potassium sulfate K2SO4, potassium carbonate K2CO3, etc.), preferably KOH and / or K2CO3.

[0029] Those skilled in the art will appreciate that in step (1), the crushing and mixing are carried out in a commonly used crushing equipment, such as a pulverizer, and the crushing can be performed 1-5 times, such as 2, 3, or 4 times; preferably, the rotation speed of the pulverizer is 5000-20000 r / min, such as 6000 r / min, 7000 r / min, 8000 r / min, 9000 r / min, 10000 r / min, 11000 r / min, 12000 r / min, 13000 r / min, 14000 r / min, 15000 r / min, 16000 r / min, 17000 r / min, 18000 r / min, or 19000 r / min.

[0030] In order to improve the comprehensive performance of the prepared coconut shell capacitor carbon, in one embodiment, in step (2), during the activation treatment, the activation temperature is 600-900°C, such as 625°C, 650°C, 675°C, 700°C, 725°C, 750°C, 775°C, 800°C, 825°C, 850°C and 875°C, and the activation time is 1-3h, such as 1.5h, 2h and 2.5h; preferably, the process of heating to the activation temperature is linear heating, and the preferred heating rate is 2-5°C / min, such as 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min and 4.5°C / min; preferably, the activation atmosphere is an inert atmosphere, preferably nitrogen and / or argon.

[0031] Those skilled in the art will appreciate that in step (2), after the activation treatment process is completed, the mixture needs to be naturally cooled to room temperature to obtain an activated material.

[0032] Those skilled in the art will appreciate that step (2) is carried out in a commonly used activation device, such as a tube furnace.

[0033] In one embodiment, in step (3), the acid used for pickling is hydrochloric acid and / or sulfuric acid, and the preferred acid concentration is 0.5-1.5 mol / L, such as 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L and 1.4 mol / L.

[0034] Those skilled in the art will appreciate that the pickling times may be selected as required, such as 1-5 times, such as 2, 3, or 4 times; the water washing may be performed with deionized water until neutral; and the drying may be performed in a drying equipment commonly used in the art, such as drying in an oven at 100-120°C.

[0035] In one embodiment, in step (4), the mass ratio of the asphalt powder to the porous carbon obtained in step (3) is 1:(1-9), such as 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8 and 1:8.5.

[0036] In one embodiment, in step (4), the asphalt powder is obtained by crushing the low-ash asphalt in step (1), and preferably has a particle size of 100-800 mesh, such as 200 mesh, 300 mesh, 400 mesh, 500 mesh, 600 mesh and 700 mesh.

[0037] Those skilled in the art will understand that the asphalt powder is obtained by crushing the low-ash asphalt in step (1) separately taken, which means that the asphalt powder is obtained by crushing the same low-ash asphalt as the low-ash asphalt in step (1), and the asphalt used is not a part of the low-ash asphalt in step (1), but is separately taken. For example, the amount of low-ash asphalt in step (1) is m1, which is all used in step (1); and the amount of low-ash asphalt in step (1) taken separately in step (4) is m2, which is crushed and all used in step (4); which is equivalent to the amount of low-ash asphalt in step (1) used in steps (1)-(4) being m1+m2.

[0038] In order to improve the comprehensive performance of the prepared coconut shell capacitor carbon, in one embodiment, in step (4), the calcination treatment is a staged calcination, comprising:

[0039] In the first stage, the calcination temperature is 120-350°C, such as 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C and 340°C; the calcination time is 20-90min, such as 30min, 40min, 50min, 60min, 70min and 80min, mainly to melt the asphalt powder into a fluid state to facilitate the coating in the second stage; and / or

[0040] In the second stage, the calcination temperature is 600-800°C, such as 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C and 790°C; the calcination time is 1-2h, such as 1.5h, mainly to effectively remove the surface functional groups caused by acid washing, further improve the conductivity, and carbonize the asphalt wrapped outside the porous carbon at high temperature to achieve its coating on the outer surface of the porous carbon.

[0041] In one embodiment, in step (4), the calcination temperature in the first stage is 10-150° C. higher than the softening point of the asphalt powder to ensure that the asphalt powder is melted into a fluid state.

[0042] Those skilled in the art understand that different asphalts have different softening points. The calcination temperature of the first stage, 120-350°C, is 10-150°C higher than the softening point of the specific asphalt to ensure that the asphalt powder melts into a fluid state.

[0043] For example, when the softening point of the asphalt powder is 130°C, the calcination temperature in the first stage can be increased by 10-150°C, that is, 140-280°C.

[0044] In order to improve the comprehensive performance of the prepared coconut shell capacitor carbon, in one embodiment, in step (4), in the first stage, the heating rate to the calcination temperature is 2-10°C / min, such as 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6°C / min, 6.5°C / min, 7°C / min, 7.5°C / min, 8°C / min, 8.5°C / min, 9°C / min and 9.5°C / min.

[0045] In order to improve the comprehensive performance of the prepared coconut shell capacitor carbon, in one embodiment, in step (4), in the second stage, the heating rate of heating to the calcination temperature is 2-10°C / min, such as 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6°C / min, 6.5°C / min, 7°C / min, 7.5°C / min, 8°C / min, 8.5°C / min, 9°C / min and 9.5°C / min.

[0046] In one embodiment, in step (4), the calcination atmosphere is an inert atmosphere, preferably nitrogen and / or argon.

[0047] Those skilled in the art will appreciate that step (4) is carried out in a commonly used calcining device, such as a tubular furnace.

[0048] Those skilled in the art will appreciate that in step (4), after the calcination treatment is completed, the product may be naturally cooled to room temperature, and further, it may be washed with water and dried in sequence as needed.

[0049] To achieve the second purpose of the present invention, the following technical solutions are adopted:

[0050] A coconut shell capacitor carbon prepared by the above-mentioned preparation method.

[0051] In one embodiment, the conductivity of the coconut shell capacitor carbon is 2-5 S / cm, such as 2.5 S / cm, 3 S / cm, 3.5 S / cm, 4 S / cm and 4.5 S / cm.

[0052] In one embodiment, the specific surface area of ​​the coconut shell capacitor carbon is 1000-1600m 2 / g, for example 1050m 2 / g、1100m 2 / g, 1150m 2 / g、1200m 2 / g, 1250m 2 / g、1300m 2 / g, 1350m 2 / g、1400m 2 / g, 1450m 2 / g、1500m 2 / g and 1550m 2 / g.

[0053] In one embodiment, the pore volume of the coconut shell capacitor carbon is 0.9-1.8m 3 / g, for example 1m 3 / g, 1.1m 3 / g, 1.2m3 / g, 1.3m 3 / g, 1.4m 3 / g, 1.5m 3 / g, 1.6m 3 / g and 1.7m 3 / g.

[0054] In one embodiment, the specific capacitance of the coconut shell capacitor carbon is 200-310F / g, such as 210F / g, 220F / g, 230F / g, 240F / g, 250F / g, 260F / g, 270F / g, 280F / g, 290F / g, 300F / g.

[0055] In order to achieve the third object of the present invention, the application of the coconut shell capacitor carbon in the preparation of supercapacitors, electrode sheets for supercapacitors, and electrode materials for supercapacitors is also provided.

[0056] In order to achieve the fourth object of the present invention, an electrode material for a supercapacitor made from the coconut shell capacitor carbon is also provided.

[0057] In one embodiment, the raw material of the supercapacitor electrode material does not include a conductive agent, but includes the coconut shell capacitor carbon and a binder; preferably, the mass ratio of the coconut shell capacitor carbon to the binder is (9-19):1, such as 9.5:1, 10:1, 10.5:1, 11:1, 11.5:1, 12:1, 12.5:1, 13:1, 13.5:1, 14:1, 14.5:1, 15:1, 15.5:1, 16:1, 16.5:1, 17:1, 17.5:1, 18:1 and 18.5:1.

[0058] The beneficial effects of the present invention are:

[0059] (1) The method for preparing coconut shell capacitor carbon for supercapacitors of the present invention has the advantages of wide raw material sources, low preparation cost, and large-scale production; and has the advantages of controllable specific surface area, high conductivity, and micropore-mesopore-macroporous hierarchical porous structure. When the obtained coconut shell capacitor carbon is used in supercapacitors, no conductive agent needs to be added; wherein,

[0060] Using cheap coconut shell carbonized material as raw material can provide sufficient mesoporous and macroporous skeletons for the obtained coconut shell capacitor carbon, which is more convenient for the storage and transmission of electrolyte ions when used in electrode materials for supercapacitors;

[0061] In the first stage of step (4), the porous carbon after the activated impurity removal is coated by utilizing the excellent fluidity of asphalt near the softening point, thereby reducing the surface defects of the obtained coconut shell capacitor carbon, improving its conductive properties, and at the same time increasing the compaction density of the material. The specific surface area can be controlled by the amount of asphalt used, so that it can be applied to different scenarios;

[0062] In the second stage of step (4), high temperature carbonization is used to effectively remove the surface functional groups caused by pickling, further improving the conductivity, and can be completed together with the coating step, simplifying the process flow and making it easier to achieve large-scale production;

[0063] (2) The obtained coconut shell capacitor carbon has the advantages of controllable specific surface area, high conductivity, micropore-mesopore-macroporous hierarchical porous structure, and good conductivity; when it is used to prepare electrode materials for supercapacitors, electrode sheets for supercapacitors and supercapacitors, no additional conductive agent needs to be added. DETAILED DESCRIPTION

[0064] The technical scheme and its effects of the present invention are further described below in conjunction with specific implementation methods / examples. The following implementation methods / examples are only used to illustrate the content of the present invention, and the invention is not limited to the following implementation methods or examples. Simple changes made to the present invention using the concept of the present invention are all within the scope of protection claimed by the present invention.

[0065] The sources of the raw materials and equipment used in the following examples and comparative examples are as follows:

[0066] Coconut shell carbonized material, produced in the Philippines, has a moisture content of 12%, an ash content of 3%, a volatile matter content of 15%, and a carbon content of 70%;

[0067] Low ash asphalt 1, coal liquefaction asphalt with ash content <0.1% and softening point of 170°C, obtained by China Shenhua Coal to Oil Chemical Co., Ltd. through direct liquefaction oil residue extraction and separation process;

[0068] Low ash asphalt 2, petroleum asphalt with ash content <0.1% and softening point of 120℃, customized asphalt by Hebei Zhengri Energy Technology Development Co., Ltd.;

[0069] Low ash asphalt 3, coal liquefaction reformed asphalt with ash content <0.1% and softening point of 290℃, China Shenhua Coal to Liquid Chemical Co., Ltd.;

[0070] KOH, Sinopharm Reagent, AR, ≥85%, CAS No.: 1310-58-3;

[0071] PTFE, Shenzhen Kejing, polytetrafluoroethylene concentrate EQ-Lib-PTFE, concentration 60±2%;

[0072] Ethanol, Sinopharm Reagent, AR, ≥99.7%, CAS No.: 64-17-5;

[0073] Conductive carbon black, Shenzhen Kejing, super conductive carbon black ECP-600JD;

[0074] Crusher, Tianjin Test Instrument Co., Ltd. High-speed Universal Crusher FW100;

[0075] Tube furnace, SG-GL-1100K, Shanghai Institute of Optics and Precision Mechanics, Chinese Academy of Sciences.

[0076] Test method:

[0077] 1. The obtained coconut shell capacitor carbon has the following properties:

[0078] The conductivity was tested using Ningbo Ruike Micro Four-Probe Resistivity Tester FT-345. All sample powders were compacted into blocks at 0.1Mpa and then tested.

[0079] The specific surface area was tested using the ASAP 2020PLUS fully automatic specific surface area and pore analyzer. The specific surface area was calculated based on the BET (Brunauer-Emmet-Teller) and t-plot theories.

[0080] The pore volume was tested using the ASAP 2020PLUS fully automatic specific surface area and pore analyzer, and the pore volume was calculated using the DFT density functional theory;

[0081] 2. The rate performance and long cycle performance of the obtained button battery were tested using the Xinwei battery testing system. The test voltage was 0-1V, the test current density was 1A / g, and the long cycle charge and discharge number was 20,000 times, and its specific capacitance and long cycle capacity retention rate were obtained.

[0082] Preparation of coconut shell capacitor carbon for supercapacitors

[0083] Example 1

[0084] The coconut shell capacitor carbon A1 for supercapacitors was prepared as follows:

[0085] (1) Raw material premixing

[0086] 8g of coconut shell carbonized material, 2g of low-ash asphalt, and 20g of KOH (activator) were placed in a pulverizer for crushing and mixing to obtain a premix; wherein,

[0087] The crushing times were 3 times, the speed of the crusher was 20000r / min, and the crushing time was 10s each time;

[0088] The low-ash asphalt is obtained by China Shenhua Coal-to-Liquid Chemical Co., Ltd. through a direct liquefaction oil residue extraction and separation process, with an ash content of <0.1% and a softening point of 170°C;

[0089] The coconut shell carbonized material is obtained by carbonizing coconut shell at high temperature, wherein the carbonization temperature is 600° C. and the carbonization time is 1 hour; the carbonization atmosphere is nitrogen gas;

[0090] (2) Activation Pore Formation

[0091] The premix obtained in step (1) is placed in a tubular furnace for activation treatment, and then naturally cooled to room temperature to obtain an activated material; wherein,

[0092] The activation temperature is 800°C, the activation time is 1.5h, the temperature rise to the activation temperature is linear, the heating rate is 5°C / min, and the activation atmosphere is nitrogen atmosphere;

[0093] (3) Pickling and impurity removal

[0094] The activated material obtained in step (2) is sequentially acid-washed, water-washed and dried to obtain porous carbon; wherein:

[0095] The acid used for pickling is 1 mol / L HCl solution, and the pickling is performed 3 times; the water washing is performed with deionized water until neutral; and the drying is performed in an oven at 100°C;

[0096] (4) Asphalt coating

[0097] 1 g of asphalt powder was mixed with 4 g of the porous carbon obtained in step (3) to obtain a mixture; the mixture was then placed in a tubular furnace for calcination, and then naturally cooled to room temperature to obtain asphalt-coated coconut shell activated carbon, i.e. coconut shell capacitor carbon A1; wherein,

[0098] The asphalt powder is obtained by crushing and screening "a low-ash asphalt with an ash content of less than 0.1% and a softening point of 170° C. (the same as the low-ash asphalt described in step (1)) obtained by direct liquefaction oil residue extraction and separation process of China Shenhua Coal-to-Liquid Chemical Co., Ltd.", and its particle size is 300 mesh;

[0099] The calcination treatment is a staged calcination, the calcination atmosphere is a nitrogen atmosphere, and the staged calcination includes:

[0100] In the first stage, the calcination temperature was 300°C, the calcination time was 45 min, and the heating rate to 300°C was 2°C / min;

[0101] In the second stage, the calcination temperature is 700°C, the calcination time is 1h, and the heating rate from 300°C to 700°C is 5°C / min.

[0102] Example 2

[0103] The coconut shell capacitor carbon A2 for supercapacitors was prepared according to the following steps; wherein the method was different from Example 1 only in the following ways:

[0104] In step (1), the low-ash asphalt is a petroleum asphalt with an ash content of less than 0.1% and a softening point of 120°C;

[0105] In step (4), the asphalt powder is obtained by crushing and screening "petroleum asphalt with ash content <0.1% and softening point of 120°C (the same as the low-ash asphalt in step (1))", and its particle size is 300 mesh; in the calcination treatment, in the first stage, the calcination temperature is 200°C;

[0106] Get coconut shell capacitor carbon A2.

[0107] Example 3

[0108] The coconut shell capacitor carbon A3 for supercapacitors was prepared according to the following steps; wherein the method was different from Example 1 only in the following ways:

[0109] In step (1), the amounts of coconut shell carbonized material, low-ash asphalt, and KOH are 4 g, 4 g, and 24 g, respectively;

[0110] Get coconut shell capacitor carbon A3.

[0111] Example 4

[0112] Coconut shell capacitor carbon A4 for supercapacitors was prepared according to the following steps; wherein the method differed from Example 1 only in the following ways:

[0113] In step (2), the activation time is 0.5 h;

[0114] Get coconut shell capacitor carbon A4.

[0115] Example 5

[0116] The coconut shell capacitor carbon A5 for supercapacitors was prepared according to the following steps; wherein the method differed from Example 1 only in the following ways:

[0117] In step (1), the activating agent is K2CO3;

[0118] Get coconut shell capacitor carbon A5.

[0119] Example 6

[0120] Coconut shell capacitor carbon A6 for supercapacitors was prepared according to the following steps; wherein the only difference from Example 1 is as follows:

[0121] In step (4), the particle size of the asphalt powder is 100 mesh;

[0122] Get coconut shell capacitor carbon A6.

[0123] Example 7

[0124] The coconut shell capacitor carbon A7 for supercapacitors was prepared according to the following steps; wherein the method differed from Example 1 only in the following ways:

[0125] In step (4), during the calcination treatment, in the first stage, the calcination temperature is 250° C. and the calcination time is 60 min;

[0126] Get coconut shell capacitor carbon A7.

[0127] Example 8

[0128] The coconut shell capacitor carbon A8 for supercapacitors was prepared according to the following steps; wherein the method differed from Example 1 only in the following ways:

[0129] In step (4), during the calcination treatment, in the second stage, the calcination temperature is 700° C.;

[0130] Get coconut shell capacitor carbon A8.

[0131] Example 9

[0132] The coconut shell capacitor carbon A8 for supercapacitors was prepared according to the following steps; wherein the method differed from Example 1 only in the following ways:

[0133] In step (1), the amounts of coconut shell carbonized material, low-ash asphalt, and KOH are 8 g, 8 g, and 12 g, respectively; the low-ash asphalt is a petroleum asphalt with an ash content of less than 0.1% and a softening point of 90°C;

[0134] In step (2), the activation temperature is 600°C, the activation time is 3h, the temperature is increased to the activation temperature in a linear manner, the temperature increase rate is 2°C / min, and the activation atmosphere is an argon atmosphere;

[0135] In step (3), the acid used for pickling is a 0.5 mol / L sulfuric acid solution;

[0136] In step (4), the amounts of asphalt powder and porous carbon obtained in step (3) are 1 g and 1 g, respectively;

[0137] The asphalt powder is obtained by crushing and screening "petroleum asphalt with ash content <0.1% and softening point of 90°C (the same as the low-ash asphalt in step (1))", and its particle size is 800 mesh;

[0138] The calcination atmosphere is argon atmosphere; during the calcination process,

[0139] In the first stage, the calcination temperature is 120°C, the calcination time is 20 min, and the heating rate to 120°C is 5°C / min;

[0140] In the second stage, the calcination temperature is 600°C, the calcination time is 1.5h, and the heating rate from 120°C to 600°C is 2°C / min;

[0141] Get coconut shell capacitor carbon A9.

[0142] Example 10

[0143] The coconut shell capacitor carbon A8 for supercapacitors was prepared according to the following steps; wherein the method differed from Example 1 only in the following ways:

[0144] In step (1), the amounts of coconut shell carbonized material, low-ash asphalt, and KOH are 8 g, 2 g, and 48 g, respectively; the low-ash asphalt is coal liquefaction reformed asphalt with an ash content of less than 0.1% and a softening point of 290°C;

[0145] In step (2), the activation temperature is 900°C, the activation time is 1 h, the temperature is increased to the activation temperature in a linear manner, the heating rate is 4°C / min, and the activation atmosphere is an argon atmosphere;

[0146] In step (3), the acid used for pickling is a 1.5 mol / L hydrochloric acid solution;

[0147] In step (4), the amounts of asphalt powder and porous carbon obtained in step (3) are 1 g and 9 g, respectively;

[0148] The asphalt powder is obtained by crushing and screening "coal liquefaction reformed asphalt with ash content <0.1% and softening point of 290°C (the same as the low-ash asphalt in step (1))", and its particle size is 100 mesh;

[0149] The calcination atmosphere is argon atmosphere; during the calcination process,

[0150] In the first stage, the calcination temperature was 350°C, the calcination time was 90 min, and the heating rate to 350°C was 10°C / min;

[0151] In the second stage, the calcination temperature is 800°C, the calcination time is 2h, and the heating rate from 350°C to 800°C is 10°C / min;

[0152] Get coconut shell capacitor carbon A10.

[0153] Comparative Example 1

[0154] The coconut shell capacitor carbon A1' for supercapacitors was prepared according to the following steps; wherein the method differed from Example 1 only in the following ways:

[0155] In step (1), low-ash asphalt is not mixed, and the amounts of coconut shell carbonized material, low-ash asphalt, and KOH are 4 g, 0 g, and 8 g, respectively;

[0156] Obtain coconut shell capacitor carbon A1'.

[0157] Comparative Example 2

[0158] The coconut shell capacitor carbon A2' for supercapacitors was prepared according to the following steps; wherein the method was different from Example 1 only in the following ways:

[0159] In step (4), 4 g of the porous carbon obtained in step (3) is directly placed in a tubular furnace for calcination without mixing with asphalt powder;

[0160] Obtain coconut shell capacitor carbon A2'.

[0161] Comparative Example 3

[0162] The coconut shell capacitor carbon A3' for supercapacitors was prepared according to the following steps; wherein the method was different from Example 1 only in the following ways:

[0163] In step (4), the amounts of asphalt powder and porous carbon obtained in step (3) are 8 g and 4 g, respectively;

[0164] Obtain coconut shell capacitor carbon A3'.

[0165] Preparation of electrode materials, electrode sheets and button cells for supercapacitors The coconut shell capacitor carbons A1-10 and A1'-3' obtained in Examples 1-10 and Comparative Examples 1-3 were respectively mixed with PTFE (binder) at a mass ratio of 95:5 in ethanol at a solid-liquid ratio of 1:100 to obtain electrode materials B1-10 and B1'-3' for supercapacitors;

[0166] The coconut shell capacitor carbon A1 obtained in Example 1, conductive carbon black and PTFE were mixed in ethanol at a mass ratio of 90:5:5 and a solid-liquid ratio of 1:100 to obtain an electrode material B4' for supercapacitors;

[0167] Then the obtained supercapacitor electrode materials B1-10 and B1'-4' are subjected to conventional coating, rolling and cutting to obtain supercapacitor electrode sheets C1-10 and C1'-4'; wherein the coating amount is 1.5 mg / cm 2 ;

[0168] The supercapacitor electrode sheets C1-10 and C1'-4' were symmetrically assembled into button cells E1-10 and E1'-4', respectively; wherein the electrolyte was 6M KOH solution.

[0169] Performance Testing

[0170] The conductivity, specific surface area and pore volume of the coconut shell capacitor carbons A1-10 and A1'-3' were tested. The test results are shown in Table 1.

[0171] The performance of the button batteries E1-10 and E1'-4' was tested using the Xinwei battery testing system to test their rate performance and long cycle performance. The test voltage was 0-1V, the test current density was 1A / g, and the long cycle charge and discharge times were 20,000 times. The test results are shown in Table 1.

[0172] Table 1 Performance test results of coconut shell capacitor carbon A1-10 and A1'-3' and button battery E1-10 and E1'-4'

[0173]

[0174]

[0175] It can be seen from the performance test results of coconut shell capacitor carbon A1-10 and A1'-3' in Table 1 that the coconut shell capacitor carbon prepared by the method for preparing coconut shell capacitor carbon for supercapacitor of the present invention has an electrical conductivity of 2-5S / cm and a specific surface area of ​​1000-1600m 2 / g, pore volume is 0.9-1.8m 3 / g, the specific capacitance and long cycle capacity retention rate are also high;

[0176] According to the comparison of the performance test results of coconut shell capacitor carbon A1 and A1'-2' in Table 1, it can be seen that compared with comparative example 1-2, when low-volatile asphalt is not added in step (1) or step (4), when low-ash asphalt is added in both step (1) and step (4) in embodiment 1 of the present invention, although the specific surface area of ​​the material is reduced to a certain extent, the electrical conductivity of the material is also improved at the same time; finally, according to the comparison of button cells E1 and E1'-2', it can be seen that when other conditions are the same, the button cell E1 prepared with coconut shell capacitor carbon A1 as the active material exhibits higher specific capacitance characteristics and long cycle capacity retention rate.

[0177] According to the performance test results of coconut shell capacitor carbon A1 and A3', the amount of asphalt powder used in step (4) of comparative example 3 is too large, resulting in a significant decrease in the specific surface area of ​​the material, thereby causing the active sites to disappear, and further causing a significant decrease in the specific capacitance of the material, indicating that under the same other conditions, increasing the amount of asphalt powder used in step (4) is not conducive to improving the specific surface area and conductivity of the material, and is not conducive to improving its conductive properties. Finally, according to the comparison of button cells E1 and E3', under the same other conditions, the button cell E1 prepared with coconut shell capacitor carbon A1 as the active material exhibits higher specific capacitance characteristics and long cycle capacity retention rate.

[0178] According to the comparison of the test results of button batteries E1 and E4', when the coconut shell capacitor carbon A1 obtained in Example 1 of the present application is used as an active material to prepare electrode materials for supercapacitors, electrode sheets thereof, and button batteries, the addition of a conductive agent has little effect on the performance of the button battery. When the coconut shell capacitor carbon A1 obtained in Example 1 of the present invention is used to prepare electrode materials for supercapacitors, electrode sheets thereof, and button batteries, good electrical properties can be achieved without adding a conductive agent. This shows that the coconut shell capacitor carbon obtained according to the method for preparing coconut shell capacitor carbon for supercapacitors of the present invention has excellent conductive properties, and can be used as a capacitor carbon product without the addition of a conductive agent in supercapacitors, further simplifying the application process.

[0179] In summary, the coconut shell capacitor carbon prepared by the method for preparing coconut shell capacitor carbon for supercapacitor of the present invention has high conductivity and controllable specific surface area, and the preparation method has the characteristics of simple process steps, low preparation cost and continuous production, etc. The prepared coconut shell capacitor carbon is applied to supercapacitors, and the supercapacitors can have higher specific capacitance and cycle capacity retention rate without adding conductive agents.

[0180] The detailed preparation method described above is only a preferred embodiment of the present invention and does not limit the counting range of the present invention. Any simple changes and modifications made within the scope of the patent claims of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing coconut shell capacitor carbon for supercapacitors, It is characterized in that The method comprises the following steps: (1) Raw material premixing The coconut shell carbonized material, low-ash asphalt and activator are crushed and mixed to obtain a premix; (2) Activation pore creation Activating the premix obtained in step (1) to obtain an activated material; (3) Pickling and impurity removal The activated material obtained in step (2) is sequentially acid-washed, water-washed and dried to obtain porous carbon; (4) Asphalt coating The asphalt powder is mixed with the porous carbon obtained in step (3) to obtain a mixture; the mixture is then calcined to obtain asphalt-coated coconut shell activated carbon, i.e., coconut shell capacitor carbon; wherein: In step (4), the calcination treatment is a staged calcination, comprising: In the first stage, the calcination temperature is 210-350 °C; In the second stage, the calcination temperature is 610-800 °C; In step (4), the mass ratio of the asphalt powder to the porous carbon obtained in step (3) is 1:(1-9).

2. The method according to claim 1, It is characterized in that In step (1), the mass ratio of coconut shell carbonized material, low-ash asphalt and activator is 1: (0.25-1): (1.25-6).

3. The method according to claim 1 or 2, It is characterized in that In step (1), the coconut shell carbonized material is a coconut shell carbonized material obtained by high-temperature carbonization of coconut shell, the carbonization temperature is 550-800°C, and the carbonization time is 0.5-3 h; the carbonization atmosphere is an inert gas, including nitrogen or argon; and / or In step (1), the ash content of the low-ash asphalt is less than 0.5%; the low-ash asphalt includes any one or more of coal liquefaction asphalt, petroleum asphalt, coal tar, coal coke asphalt, synthetic asphalt and natural asphalt; and / or In step (1), the activator includes any one or a combination of multiple of potassium metal oxides, hydroxides and their derivative salts.

4. The method according to claim 3, It is characterized in that In step (1), the activator is KOH and / or K 2 CO 3 .

5. The method according to any one of claims 1, 2 and 4, It is characterized in that In step (2), during the activation treatment, the activation temperature is 600-900 °C, and the activation time is 1-3 h; the process of heating to the activation temperature is linear heating, and the heating rate is 2-5 °C / min; the activation atmosphere is an inert atmosphere of nitrogen and / or argon.

6. The method according to claim 1, It is characterized in that In step (3), the acid used for pickling is hydrochloric acid and / or sulfuric acid, and the acid concentration is 0.5-1.5 mol / L.

7. The method according to any one of claims 1, 2, 4 and 6, It is characterized in that In step (4), the asphalt powder is obtained by crushing the low-ash asphalt in step (1), and its particle size is 100-800 mesh.

8. The method according to claim 1, It is characterized in that In step (4), In the first stage, the calcination time is 20-90 min; and / or In the second stage, the calcination time is 1-2 h.

9. The method according to claim 8, It is characterized in that In step (4), in the first stage, the heating rate to the calcination temperature is 2-10 °C / min; and / or In step (4), in the second stage, the heating rate to the calcination temperature is 2-10 °C / min.

10. The method according to claim 9, It is characterized in that In step (4), the calcination atmosphere is an inert atmosphere of nitrogen and / or argon.

11. A coconut shell capacitor carbon prepared by the method according to any one of claims 1 to 10.

12. The coconut shell capacitor carbon according to claim 11, It is characterized in that The conductivity of the coconut shell capacitor carbon is 2-5 S / cm; and / or The specific surface area of ​​the coconut shell capacitor carbon is 1000-1600 m 2 / g; and / or The pore volume of the coconut shell capacitor carbon is 0.9-1.8 m 3 / g; and / or The specific capacitance of the coconut shell capacitor carbon is 200-310 F / g.

13. Use of the coconut shell capacitor carbon according to claim 11 or 12 in the preparation of supercapacitors, electrode sheets for supercapacitors, and electrode materials for supercapacitors.

14. An electrode material for supercapacitors made from the coconut shell capacitor carbon according to claim 11 or 12.

15. The supercapacitor electrode material according to claim 14, It is characterized in that The raw materials of the electrode material for the supercapacitor do not include a conductive agent, but include the coconut shell capacitor carbon and a binder.

16. The electrode material for supercapacitor according to claim 15, It is characterized in that The mass ratio of the coconut shell capacitor carbon to the binder is (9-19):1.

Citation Information

Patent Citations

  • Coconut shell fiber-based activated carbon for supercapacitors and its preparation method

    CN105923634B

  • Preparation method of activated carbon for supercapacitors with controllable specific surface area

    CN108101054B

  • A stepwise purification method for the industrial preparation of high-purity activated carbon from coconut shell supercapacitors.

    CN109592681B

  • An industrial-scale preparation method for highly conductive coconut shell activated carbon for supercapacitors using a two-stage activation process.

    CN109850892B

  • Method for preparing active carbon for super-capacitor from potassium humate in one-step carbonization way

    CN103373728A